Document by4VVjxa6xr285EEROxzB6931

it X Houston Office August 25,1960 C. W. Beam - Baton Rouge Cast Iron Pipe Sales Propaganda Thank you very kindly for the attachment to your memo of August 22. I had not seen this particular effort on the part of our competition but it represents nothing particularly new. It does, however, contain some outright misrepresentation and generally twists the facts, as one would expect, in a manner intended to make the reader believe that thin walled cast iron pipe represents progress. I will not attempt in this letter to provide you with all of the details but will discuss the matter on our next personal visit. It is sufficient for the moment to state that, when the original ASA Specification A21.1 was published in 1939, these specifications clearly recognized that pipe could be made with a thinner wall than that recommended as minimum ' by the responsible committee. Without attempting to quote the specifications verbatim, the committee simply stated that the possibilities of breakage in handling and other hazards were such that the thicknesses developed . on the basis of using 18/40 iron were the minimum practicable for normal usage. WHW/plg cc: W. P. Richardson - New Orleans File W. H. Waring aJ<Jy ~ MEMO Office. ^3^_ Locatioi y-Date- ^2a, -g. WHY FILE THIS! Form 3-2B '"-" *- in TO: Water Works Engineers ke: Specifications for underground water pipes There has been some ambiguity and resulting confusion in regard to the various specifications and materials governing underground water distribution pipes* The history of these specifications is enlightening. The American Standards Association Committee A21, formed in 1926 made an extensive study of the requirements that: an underground pressure pipe oust meet to assure that it will do the job for which it was intended. The ASA, under the sponsorship of the American Gas Association, the American Society for Testing Materials, The American Water Works Association ami the Mew England Water Works Association, studied the factors influencing the design of pipes, evalua ting the best available knowledge of ground stresses and experience with pressure pipes. Participating in this work were representatives of sponsors, producers and consulting engineers. The result of this comprehensive, scientific study was the development of a formula which recognized in pipe design such factors as trench loads, water hammer, inter nal pressure and safety factors. The formula is as follows: Wm W V? - p sTF-- (a) W t2R .0795 (d i t) (b) P s 2tS t - Thickness of pipe in inches S - Bursting Tensile in lb. per sq. in. d - Internal diameter of pipe in inches R - Modulus of Rupture in Id. per sq. in. p - Internal Water pressure in lb. per sq. in. w - Load (earth & traffic) in lb. per linear foot of pipe. W - Crushing load in lbs per linear foot of pipe. In 1939, when the formula was published, centrifugal pipe casting foundries were able to consistently attain a metal strength of 18,000 psi bursting tensile and a 40,000 psi Modulus or Rupture. Therefore, the necessary tables for various sizes of pipe, trench conditions and depths of cover were begun to be compiled on this basis. In 1953 these tables -2- were published end the ASA specifications formally adopted* In the aeaatiae however* technical advances in the cast iron pipe Industry enabled pipes to be cast consistently with a 21,000 psi Bursting Tensile Strength end a 45,000 pel Modulus of Rupture. Inis increase in strength was accomplished without changing the chemical composition of the matal which has given cast iron pipe its' long record of service. Cast iron pipe manufactured using 21/45 iron must then be recalculated in accordance with the formula developed by the ASA to ascertain the wall thickness required. Thicknesses for pipes laid in e flat bottom trench and under 5 feet of cover for 150 psi water working pressure are as follows: SJiizes 4" Wall Thickness .32" 6" *.32" 8" .35" 10" .38" 12" .41" Minimum rscotrooended thickness for shipping and handling is .35" These thicknesses are manufactured and marketed under Speci fication ASA 21.1. It should be noted that the pipes with s thicker well will have an even greater safety factor then those set up by the ASA and will give better service where in later years unforeseen stresses occur. Using s minimum Bursting Tensile Strength of 3,400 psi and s Modulus of Rupture of 7,600 psi (Mote 1) for Cement Asbeetoe, the thicknesses calculated for 150 pel ere ae follows: ASA Calculated C.A. Class 200 C, A. Class 150 Pine Size Wall Thickness Wall Thickness Wall Thickness 4" .48" .51" .51" 6" .68" .685" .61" 8" .87" .835" .71" 10" 1.11" 1.095" .91" 12" 1.28" 1.260" 1.04" 3- To Mut the minimum strength requirements of underground water pipes es calculated by the ASA formula, Class 200 Ceasnt- Asbes tos cones fairly close to these requirements. The thicknesses listed under die coluens labeled Class 200 and Class 150 are Manufactured and marketed under A.W.W.A. Specifications C40053T. Because these specifications follow the manufacturer1s standards, the intoduction to AWWA Specifications for CementAsbestos pipe contains the following statements: "AWWA specifi cations for Asbestos-Cement pipe ere based upon the best known experience and are intended for use under normal conditions. They are not designed for unqualified use under sll conditions, and the advisability of their use for any installation euat ba subjected to review by die engineer responsible, The use of the terms "Class 100", "Class 150" and "Class 200" applied to aabeatoa-ceoent pipe produced under these specifications is not intended to imply that the material, when initially installed, is die engineering equivalent of cast iron pipe bearing the same designation." In May 1954 the National Bureau of Standards published die results of thirteen years of testing the "Effect of exposure to soils on the properties of Asbestos-Cement pipe." The results show that, in general, for the first five years of exposure, the exposed pipe absorbed less water than unaxposed pipe; however, after that period of time, the pipe, in general, absorbed more water as the time increased. The graphs show that the strength of the pipe decreases with die percentage of water absorbed. It la noted that saturation with watar reduces the strength of Asbestos-Cement pipe from 10 to 20%. Consequently, all bursting pressures or tensile strengths of test made on unsaturated asbestos-cement pipe must be reduced by 10 to 20% for comparison with actual working conditions. Unfortunately these test were concluded by the National Bureau of Standards after only thirteen years of testing. At the same velocity of flow die volume delivered by two pipe of different sizes is proportional to the squares of their diameters. With the same nead, however, die velocity is less in the smaller pipe and the volume delivered varies about as the square root of the fifth power of the diameter. Inside diameters of both cast Iron and asbestos-cement pipes as as follows: Nominal Pipe Size Cement-Asbestos Class 200 Cast Iron Class 150 w/half-thickness cement linina (1/16"> 4" 3.95" 3.975" 6" 5.70" 6.015" 8" 7.60" 8.105" 10" 9.63" 10.095" 12" 11.56" 12.115" Note: C * 130 to 140 for both pipes. 4- Dev*loped, this give* Cast Iron Pipe with half-thickness ceaent lining nor* capacity a* follow*: 4" Half*thickness ceaent lined cast iron pipe delivers 1.6X nor* water than aabestos-ceaent pipe. 6" ditto 14.4X sore 8" ditto 16.6X nor* 10" ditto 12.3X nor* 12" ditto 11.IX nor* In light of the foregoing facts, it appears that Cast Iron Pipe, Class 150 has only a slight advantage over Cement-Asbestos Class 200 from a structural standpoint, therefore, the engineer oust evaluate the proven long life, additional carrying capacity, tapping chara cteristics and reliability of cast iron pipe with the lower first cost of naterial for cenent-asbestos pipe to detersine thich material he should specify for his client. Yours very truly. CMF/sh NOTE 1: Cecil K. Forbes 926 North 3rd Street Jacksonville Beach, Florida These values were taken from actual test as reported to the Cast Iron Pipe Research Association by the Southern Research Institute. A. Pinal Report to Cast Iron Pip* Research Association on Comparative Testing of Cast Iron Pressure Pipe and Asbestos-Cement Pressure Pipe. Project 444, Report 1. B. American Water Works Association Specifications C400-53T. C. American Standards Association Manual for the Computation of strength and thickness of Cast Iron Pipe. ASA 21.1, 1939. 0. "Effect of Exposure to Soils on the Properties of Asbestos Ceaent Pipe", by Melvin Romanoff and Irving A. Denison - Corrosion Section, Metallurgy Division, National Bureau of Standards Washington, D.C. E. Review of Paper "D" Enclosure". SPECIFICATION FOR CEMENT-ASBESTOS PIPS / Cement-Asbestos Pipe shall be manufactured In accordance^f-J^t^^, with Federal Specification SS-P-351a, Class 200, with ifi- Ringtite or equal joints. Fittings shall be Mechanical ' V Joint Cast Iron, Class 250. In tlay soils, pipe shall be enveloped in a minimum of "s four inches of tamped sand. In such instances trench bottom must be dug at least 4" deeper than grade and then brought back to grade with tamped sand. In / unstable soils, it will be neeessary to dig deeper and j A y refill with selected materials of gravel or crushed stone until pipe grade is reached. When spreading refill soli on the trench bottom, a 2" minimum clearance shall be left beneath the coupling and thoroughly tamped for coupling support. All fittings shall be suitably anchored with a thrust- ' block of 1:2:5 concrete. In soft soils, each coupling shall be similarly anchored for side thrust. All ( e> - AT" Valves shall be similarly anchored with a V steel rod looped over each hub of the valve and securely embedded in the concrete thrust block. Service connections shall be made with a Clow F4339 Double Strap Service Clamp equipped with a rubber ^ outlet gasket. Before placing the clamp, file the . 7 V surface of. the pipe and provide a clean hard surface for the clamp. 2 > <-#f-" ' -f-jt Cement Asbestos Pip* shall have a minimum of A'-O*' cover over the top of the pipe. Stub roots exposed by trenching that are within one foot of pipe in place shall be ceeted with hot bituminous tar or other suitable growth inhibitant. y TESTDC: Dry Cement Asbestos Pipe will absorb some water, so the line shall be filled with water at least 24 hours before the leakage tests begin. Pipe shall be purged of air and then tested to 200 psi for 24 hours. Leakage shall not exceed 75 U.S. Gallons per 24 hours per mile of pipe per inch diameter. 4/