Document bbXN24YGjE1yN1gpjvrM42n6

MONSANTO CHEMICAL COMPANY 10-1-44 SAIXSMIH'S HAMPAL AJIOCLON ' iffiscBimoN ato mopiarns Th# Aroolora in a mmm or eblarlnattd hydrocarbon# baaed on biphenyl and terphenyl, Thty aro. not pur* ocmpound# tout or* aUttur## or closely related chlorlns substitution products Man ufactured essentially to a o*t of apselfleatlana baaed on physical propartloa rathar than chwlaal eoapoalUon. The approximate chlorine content Is indicated toy th* loot two figure# of ttao Arcelor nuMber. Tta* ehealeal ecupoeltlon closely approaches tba ivifiii Tor th# indicated ehlero-asrlvetlves a foilova,but ahould not to# rpr##at#d as slapla chsaleal coupe, altlon# according to th# foruula showni Approximate Equivalent Ghouleel CcMpound 12Wa| 1272 1242 1246 1234. 1260 1262 1266 1271 5460 Monoehloroblphanyl toiehlcrcblphonyl Trlehleroblbhanyl Ttreehlorooiphonyl Fastaehlorobipbsnyl Hexaehlorobiphenyl Haptachloroblpbsnyl Nonaehlorobiph#nyl Doeaehlorobiphenyl Ifcnaobloroterphenyl Itf#r#M# ahould to# aado to technical bull#tin 2-115 for table# and graph# of.physical prop#rtl#s. This Manual #oatalaa only that InYoraatlon which is not d#slgn#d for g#n#ral putolle distribution or has b##n sad# aors rscsntly available than permitted Incorpora tion la th# printed bulletin- Th# following Aroalors not .In oonmnlal production (tout available) hav# toaaa proposed: . Arcelor No. FU#d OhlorlM Color (Lovipond) Pour Point ' Softening Feint 5446 47.9# 6.0 600 630 5454 54.83# 20.0 84 850 1 KONS 9'1*4*3 WATER PCB-SD0000067071 MOfBAXTO CHOUCAL COMMIT* 10-1-** Aroolor 80. Viscosity 98*9C (810F) 5**8 395.0* * flash Point Bum Point . o?o *000 Chlorides Acidity ag. XOH/f. Rosie 0.008 Rone 0.00* Xvaporation 0.006 0.007 Resistivity Ageing Dielectrlo Constant egOS **65 *ri7.2 KJCWIOAL. M0P8MIIS kU LM Aroolor Akrrotlor Arcelor Areilor "1 ^ ia*fl las* ia6o 5** 7 1 Dlele:trlc Constant itfo f-f *.6J *.15-*.35 3.S-J.S *.9* `Reeietivlty 100^ Mgg'jjP* 500*10? Above 1*69x10? 500x10? Dieleetrlo Strength 3^IV Min. Poser Motor (100C, looO'ke) LeSI tlu 0.1J6 . Less thin 0.1Jt IRS Method 8.3955671 Resistivity 100 under 500 Volts DC A51M 0-177*11 .. Rtfrsetiv Indsx san Aroolor 1870 Aroolor 1871 'Tetrsdsesehlorcswtatsrphsnyl Tetrsdsosehlereparuterphenyl 1.691*1.7* 1.691-1.7* 1*718-1.718 1.691-1.7* Rest of Vaporisation . Aroolor I860 (> hi. pros sum) ' . Aroolor 1868 760 sat* pressure) Aroolor 116$ 0.151 ata, 350C) (0.079 ta. 6 JS$C) . *. Midpoint 1.718 1.718 1.712 B.I.P./lb. 10* Ja.t 9.8 70.6 A* -*U * MOHS 0*20** JKfk- WATER PCB-SD0000067072 MOSAXTO COMICAL COKPAW 10-1-33 aoLcaaiTY aolTtnt Aeaton* Alcohol, Poraul* J*A Aayl Acttata Aayl Aloohol Btnstnt Butyl Aeatat* . R> Butyl Aloohol Carbitol Chi orofora Ol Butyl Phthaiat* Stbar Sthyl Acttat# Zthyl Laotat* Stbyloiw Diohlorld# tojf Poraaldohyda Xurfurol High Toot OuoUni Olyotrin Xtroatn# United OU Kothyl Aeatat# Mineral Spirit* Farafrin Phenol 900 Plm Oil Pyrldin# Toluoao Trt Crooyl Fhoaphat# Tunf OU Turpentine ' Xylene Aroalor 1263 Cold Bot ! 8 PS 8 3 I -'Hx -8 8 3 PS 1 3 I PS X PS X PS fJr 1 8 8 PS jfgfi't PS 8 8 8 S //jr* *t s 8 S 8 8 i srs. I laaolubl# PS Partially Soluble S Bolublo 3 olvent Oao* Aroolor 1*70 par 100 ao.Solr*at Furfural . Furfural . Secondary Aayl Aeotat* - Secondary Aayl Aloohol* 2,0 3.0 3.0 3.0 Carbitol . Boary Vhlto Mineral Oil 3.0 3.0 Approx. Trap, at which aoln.coarelet# 105-U0OC 1*0-1250 110-115*0 Mot oenplataly aolubl# at boll Abort 10* IIO-IOT -3- MOHS 031*39 WATER PCB-SD0000067073 HOSAJITO CHBUCAL COKPABt 10-1-44 ( Toward Heat STABILITY ' A rod op 1215 vii heated to 650F la atainlaa* ateul autoclave with the.reeultlng changes indicated la tho following tabulationi Tine oT Tanper- Acidity Original Sample Autoclave #1 Autoclave #2 Autoclave #5 moot reaulta or* intaroreted m Indicating ery.excanant stabil ity for Aroelore under the condition* of toot. .* * Toward Oxidation ' ' When Aroelor 1254 is>boated for 50 op 60 day* ot 15000 la tho proaonoo of oxygen and copper,-there is likely to bo aoo attook on tho coppor. Xxaninetion of Aroelor 1254 after that period of tine vl 11 usually ebev tb* proaonoo of aolublo coppor. Tbia alee occur* vltb mineral oil aud other Ineuletng liquid*. In general. even after severe oxidation condition* no evidence of chlorln* splitting rroai tho paront hydrocarbon bag. b*#n found. Toward Aoldo . ' ' Atm lore 1242 and 1254 vort otlrrod vltb an tqual volant- of eon- c antratod Sulfuric Acid dilute Sulfuric Acid (lojfj, Hi trie Acid (70)0, and dllut* Bltrlo Aold (5)f). at rooa tonpernture <25C) for 1$0*250 boura. Tho Aroelor vu than vaabod until nutral, de hydrated vltb Sodlwt Sulfat*. -tban analyaod in comparison vltb a control aaaplo for tbo various properties ohleb art regularly oon- aldered, without causing tboaa properties to depart fro* aptelflea* tlon Unite. , .. Aroelor 1202 vaa treated for 160 hour* ouapended In tbo mm eolde aa above at 50 to 5500. Tbo concentrated Bltrlo Acid cauaod an lnoroeoo in color, othenrlae no olgnlfleant change In ebaraeterla- tiea. . . The acid layer fro* the treataent of Aroelor 1254 vee concentrated Sulfuric Acid at roes temperature for 150 hour# and vaa tooted for chloride content. Tbe quantity of SCI found vac ao anil that it vaa not poealble by ordinary netbodt to obtain a quantitative fig- urv. Thua It appears that practically no hydrogen chloride le evolved under these uondltlone. . - .oi 4"'6 :-4 r.-.jLrt? WATER PCB-SD0000067074 HOMSAXTO CHBUCAL CCMVAXY w-i-4% f cowoaiox Additional corrosion dsta hot included la bulletin P-H5 (n h.bt-x) it as follows t ..... . t . 1 He tel Tempereturo flM Of Irooturt ftattrition ___ 33/7* . Monti . J420 Dov Htttl 1500 Yellow greet ;0 A1 tilof 175T 12000 A1 alloy 5288 12000 A1 alloy 5T 1200 360 hrs. , .. 80 days . 2,960 hrs.r In stwel tw 21 21 * - * 21 .006 .001 *003,, .00035* . *.00035* 00036 The weight loti occurred la tbt flrtt tttta days of the tttt. Xagiiglble lott was encountered la tat iwt 14 dtyt. , . The vapor ooadtattr tad tbt product rtotlvtr of tbt plant distills- tioo unit for producing Aroolor 1254 it teaatruettd of Monti and no failure la the system nor any noticeable reaction between the Aro olor tad tbt Monti hat beta discovered after three years of opera tion. . 'BCBJOhltiTY Of VAm IX AXOCtO* 1212 The vattr content of a sample of Aroolor 1242 saturated with vttor at approxiaately JOC vat determined,using tht Xerl Pitcher reagent, to be about 0.080, - ............ . - Arcelor 1242, at regularly produced, eontalne by the um test lose than 0.0013 voter, ,, ................... ,v . ' *' ' atmPAd Ttwiox The eurfse# tenaioa of Arotlor 1254 It at foil over ^ ' ' Temperature 10000 ,, . * . "' . Prats per Oentlaeter {?;?........................ * v *r .* 42.0 :.* ..v:: sssaia... .;v.\ . . All chlorinated hydrocarbons have measurable degrees of toxicity'to the animal organism. Aroelore are ao exception,.. The eymptceu of Aroolor poisoning erct , . ` 1.. Tore acne (ohler-tche) nodular eruption ~Sr tbh "" hair follielee or sebaceous glands as a reeult `of*. . v.. insufficient eleaaalng ef tbe eXloT. r'"' '* * : .1 'f. v"/. u . .* '^ V' i;*., . uX___ H0HS octet? V- WATER PCB-SD0000067075 MOMAKTO CSBIXCAL CWAJOf 10-1-4% 0. Mute yellow Atrophy of the llnr la white tlu lirar oella ihov availing, hypergranulAtlon, hyaline lnelueieoa and raeuciatlen u a remit of extensive. txpooure otr loot period* of tine. The** ijsptou My Alio reeult frcn expMure to othor telorlnatad hydrocarbon* of ammrot, auah Mi oarbcn tetrachloride, dichlor- thyIon*i trlahlor ethylene, chlorineted naphthalene (Bslcvax), The boot known {ot pretest) *t*urc of tho degree of toxlelty or tho Arealore le preeented belwt . .. reigioelblo Unite (in M./au.n,) of CoaeentratlOB in Air of Worie room r [journal orinduatrlai aygitno * ?qi5%dlodrgI7 Too tod op ltoto by Inhalation Chior1m fonlaoltolo Content Unit 0 g./ou.n. Aroolor li66 68 Aroolor *t|5 Aroolor 60 Aroolor 5* c Trtohlornopbtholono pluo tree# Tetrechlor* naphthalene . ' Totra ud renteehlomephtbaltnea Tonto tad Bexaeblornsphthaltnaa Of.6 Totro ud Penteohlernepbtbelenee plot Refined Chlorinated Diphenyl : *3.5 900 Ponte and Baxa6hlersaphtbalene / 100 Aroolor M65 - > Chlorinated Dipbonyl Oxide - ' f5t*.'00 Chlorinated Diphenyl Oxide . 57.0 Htxaehlor Diphenyl Oxide / 50 Trlehlor- naphthaln - . 50-55 Baxoohlemepbthalene and Crudo Chlorinated OlplWIITl . Speaial Chlorinated naphthalene * ' ** . . 50-56 10.0 0.5 0.5 0.5 10.0 1.0 0 0,5 * 0.5 * 0.5 0.5 . *? 0.5 0.5 . .. *5 Tooted also by feeding," , # 8 m--ry of Qroei feeding Ixpsrteonto1 ,, b .# . .. . i * Of tho veriw* Mteriele'fed rota te large doses, THehlornaphthoiono plus treeee of TetretelomepbtealeM. Wee gulte lnnoououa. Totro and Pentaebloraephtealent thawed definite liver dawega, Ponte and Xexaehiortephthalanes oaused 0 1tellor ando pT injury. Tho addi tion of ehlorlaated dlphonyl to fonte and Bawahlornaphthal*noa Inaroaaad tea tcxlilty, Chlorinated Dlphonyl alooo produced liver l looleno toot In tho dotage naod wee loot effective than vboh'alxod . ' with highly chlorinated aaphthalonoa. Zn no --o* did the eewpounde " WATER PCB-SD0000067076 ' MDIBAX70 OHKNXOAS. COHTJCK ( . ' .w t t, , ., , used product abut# yellow atrophy tout the lotions observed indi cate this might tot possible if opt found a dosage ehich could set for tbt proper period of time. . V , .; . - , feeding free lit poses tor Stomach Tubst the eempeunds employed vert irupnSe<J"Ih gum Acacia. in ngurlng the dotage tfefe totel amount e son of 50 kg. eould inbelt In en o-hour day, teaming on eir ccn- oentretien of 20 Ufa. per eU.m., vet flret calculated end reduced to mllllgrcaa per kilogram. -The rate end rabbits received tbit doae each Oaf. the compounds used ware tboet employed Id tht fro*a raiding experiments end .the reeulte vtre essentially ainilar though the lesions were lt at.tart. . ` .. i, :*-`''--i-v.r)-i, -. / ' ` , Subcutaneous Injections* '`the teat gun aotoia suspensions .vert in- jaeVtd tubdutaneouilfInto rets end retoblte, the dotage toting oel- eulattd on the toealt of A agm. per eu.a. of air. Again iniUr rtaulte vara obtained. In ell eueh txptrlatnta there auet of nee- . aaitjr be dlffertnete in tht degrte of afftet but invariably the liver via tha eole organ affected and tha latlene Vara thoea already described many tlaae. - : : .- ' BeocmnsnOatlons for Industrial Praotlost bnlaaa there la a vary "~7 ^ loocTriaaon for using tod hoi mecaoA of impregnation, all naf in stallations should use the oold or eelvent method of lapragnetion with chlorinated naphthalanea and diphenyls. Where tha hot aathod ' la cov being uaod It ahould ba ehangad over to oold. If possible, or surrounded vltb every known proteotlve aaaaura. . Otneral hygienic measures should be followed, but la no oaea should that* ba allowed to supersede engineering control of fbe primary teuroe of the exposure, the operations In the plant. , ., Tha following hyglanlo measures may be considered good practise vbtro these ooopounda ar* handledi ' ; - . (a) Two looker* for each worker exposed to`chlorinated waxes (om for . .vo, iki.ng and . one for *s. t,reet . slothes). . (b) All tort clothes above tbo underwear should be pro- . tided and laundered .at leasttwice e week, by the management'. ^ .... ; _ ; ... ,, ' . .. *(o>. The worker* "sh'duld change to clean underwear at'the ' e\ndSiof, ea*c,h>.shift befo.*r*e*(gett'ing into hie street clothes.. td) Supervised aleaningi. (1) At noon tbe 'voikere should : raaovs outsr clothing and scrub hands.and face under supervision! (t). mt The and of . the shift they should' ' . be reaulred te poke. * supervised abover^bafore. changing . - ** *-:- V v; - v .; "J.v vt . . WATER PCB-SD0000067077 MHAAMTO CHEMICAL COtPAHT . lO-l-W {) Trotsotlve skin artess or protective slothing should b* . provided by the aanageaent at the discretion of tho for*, in, nurse, aadleal, r plant superintendent, ' . (f) AU departnenta handling chlorinated ty&thetie mn should be thoroughly cleaned aooordlag to a prearranged eoheduie. This should inoluda the.reaoyal of all de- poalta of van notarial frea tha naehinee. floor* and surrounding objects. Vorkere doing tbs aisanlng ihould ba provided vltb protective clothing and auppllad air or organic vapor aaaksvhere exhaust ventilation is lr*Co quets or net poaslbls. - Tha forenen* of all departnenta vberv this aatarlal la haadlad should ba apprised of tha toxle nature of tha aatarlal and In structed in safe handling procedures. These asn should sake it their duty to cheek up on the vorkere la their dapartaante and laaferuct thaa in safe praettoa, -. - rre-eaployaent and periodic ptoyaleal exaainatlona should ha aada of all exposed vorkere. Thaas should Include the taking of * full ellnloal history, vlth apodal eaphaala on gaatro-intcatinai die. turbaness and dcraatltit. In addition, tha akin should ba care fully exaalned periodically and tha aors reliable liver function teste performed. Oaatro-latestInal oofficiate developing in a vorkar at any tlao ahould ba a signal .for an iMMdiate nodical eh*ok-up, A history of liver dlaoaao, Jaundice, or aatleypbllitie treataent should auponatlehlly exclude a vorkar froa Jobs involv. Ing a possible toxic exposure* INgnant veaan ahould not bo aa- ployad vbere there la a possible exposure to tha amthetie chlor inated vaxaa. ' Znglaeering aootrol of plant operations aAnnot be 'ovar-anphaalesd but specific reocaaondatlo&a are not applicable to all oaata. It vould bo visa for a plant using this alas a of haterlale to ebeek their control aaaeurai vlth the state industrial hygiene agenoy, tha inauraaet carrier and boas eoapeteat consultant before occu pational, disease' occurs,'. ...... .. . .. . ' APFLiCATIOPS OP AhOdOTO ibrnira . Adhaalvaa of good, tlootrioal aharaateristlea eon be prepared con taining Aroolom. Tho foilwing are typical axaaplaai WATER PCB-SD0000067078 MOJBAJrTO CHEMICAL CQMPAHT 10-1-M . fttlcll TUw 11038 Aroolor 2565 (S.T. 77.5*0) (Cod* >140-0114) IS) Hmn 50.8*0 . Mineral Oil (Ixtra Bury libit* - Soon*bom') Barytes - Mepbaa't ft - #131 Aroelor 4165 (Cod* 3140-0144) B-n um (Mai - kw #iaoeooa hi* 658 Paraffin 50.8C Baryta* Xiphia'l #2 #155 Aroolor 4465 (Cod* 3140-0144) Sotor Mb - BOO #1202S0OC HI* Mineral Oil .(tatra Heavy Vblt* lonnebom'*) Serytee . Kipha'i #2 #& Areolor 4465 (Cod* 3140-0144) ,, 508 Mineral Oil (Ixtra Heavy Vblt* - Sonnebom'e) 8*rrtt* . Kipbu*! #2 #" Aroelor 4465 ' ,, Mineral Oil (Bxtra Heavy Vblt* - Sonnaborn**) 46.50# 1.17 2.33 50,00 16.10# 14.55 4.55 65.00 20.TO# 18.45 5.85 55.00 50.0 69.5# 10.5 . #"M" Aroelor 4465, ' . 58.2# Mineral Oil (txtr* Heavy White - Soon*bom'*) 6.8 Silica (Scbulta, Chenplaln 8 bibbo) , 35.0 for tb* preparation of therao-plaetlo adbealree Purdue Onlvaralty found that tb* harder. Aroelor* are bettor than anythin* tie* diecovered to date, prlaarlly because of their high compatibility with other realm and their thomo-atablllty.. . ` PJW81CAL Pleieotrtea and Ileotrleel Ineulatare ,. , . The Aroolora have excellent dieleetrie prop*rtlet, that le, lew dieleotrio oenetant and reactivity and lot power factor. Aro elor 1242 baa the bigheat dialectal* oonetaat of the vhole aeriee vhlch ve are amifecturlng com*reicily, vhile higher chlorine Aroolor* have higher reoletlvlty. ,. *v The Aroolor* have found ueefulneei aa a dleleetrie 1a condensers and aa a dleleetrie and cooling nedluu in transfomerti and a number of alseelleneou* inner were where the eheraeteriatlea above naaed are of InporUneo. A80CUHB aa BATORAIITS Saturation nay be defined as that operation by vhleh 11guide or |-U----f--i---a--r-e eaueed` t`oi penetreke relatively porous Material*. The penetrating nedlun 1* known a* tmh* eaturant andgenerally In MOW doles i ... y-jjTfej :^rtfjbpgz. WATER PCB-SD0000067079 NOSAXTO CHWICAL CWPAW 10-1-4% the liquid statu. Saturation uj be assisted or accelerated by noons of. increased temperature sad pressure or by the us# of a vacuus. ' . Various desses of products or# saturated for the purpose of sir ing then s vide rarlsty of properties. Sene of the properties attained by sstdratlon eret voter and flam* resistance! resistance to chenloelsf abrasion; moisture) light and veather changes; In creased strength; end Increased weight. . ^ i . Among the srtleles that are treated to obtain son# one or ell of the ebove aentioned properties ere Included the various fibres end fabrics t salasl; vegetable end ninerail woods, both herd end soft; ceramics vsro and cement; and csrtsln kinds of elsetrlssl appara tus, uoh as carbon resistors. ' ' '. The saturate*, or, as they sm tometimes called, the lnpregnants, are usuelly made up of waxes, oils, resins, or water solutioris of oortain inorganic salts. . Applications . At present the saturating applications that are of ohiaf interest ere insuleted wire, low voltage cable commonly called network cable, and carbon resistor fields, These proposed uses ere des cribed more fully under the asperate heedlngs vbloh follow. network Osble . *' " Attempts are being mads to develop a use for Aroolor as a saturant for aeoendary network op lpw voltage cable. . Cable of this kind is used in electrical network distribution eyeteas, Ocnerauy, it - consists of the oopper conductor or conductor*, the paper insula tion, and the leed sheeth. The paper ie saturated with an oil., usually s good grad* of oil such as. the Central fieetrle Company's Trenail Oil, nils form of construction Is objectionable because under the condition*' Imposed by e short circuit, oasbuetlbls geses ere genereted which flow through the conduit* to the manholes, at which point they may form explosive mixtures with the sir And, In turn, eeue* explosions la the manholes. Both the psper and the -oil are source* of combustible gases. , Xt is therefore desirable to replace thorn -- the paper with as inert form of Insulation, If possible, and the oil with a nom-inflamuable saturant sueh as Aro- clor. Thus far, Aroclor 1354 appears 'to meet the requirements of this uso. , -W * . .; > , " + - * `a*. . ' ' . H' 1 * The more important sable manufacturere In the country are already et work cm the development of a flam* resistant oabls and also on* In vhloh the explosion hasard will be., lessened or eliminated. ` * , i. ~ ........ * 1 . y; none 092052 *a. .*** . m m *4 Sm" * . r Iff. .. n1*iiifVt.-r.f.mM ..*'V WATER_PCB MORSAAfO CHEMICAL COMPAJflf 10-I-44 Carbon Kselltore * Carbon resistors or* nail molded rod* of a mixture of carbon black and tend tltb a rtelneua binder. They era paroue and their elec trical rgelttaeee la seriously affected by the entrance of Bolature,' To prevent moisture getting Into the mite they are uaoally impreg nated with 'tone, notorial to flU up the volda and to coat the eur- raee of the realator. A ax la generally need for thlt purpose and aervee very veil a* far ae oole turf-proofing la eeneemed. Hoe- ever, after completion, the reeiator must be lacquered Tor Identi fication. Lacquer doae not adhere veil to the vexed eurfacee. Arcelor 4465 hoiature-proofing Conpoundt give nolature proofneae (ttnidity teat) equal to that of vox and, In addition, give a aur icoe to vhlch lacquer vlll adhere. . ' The Aroclor Compound la nom-crystalllne-end therefore does not have a definite melting point and doee not becone extremely fluid at tht melting point of moot vaxoe that are ueed in thle application, but it gradually eoftene under Increaaed temperature. In extensive teete to find the moat effective medium for Impregna ting radio reelatora to stabilise the electrical realetivlty under exaggerated and extreme humidity teata, Aroclor 3460 govt by for the beet results vhen compared vlth Santevex and various petroleum vaxee and oompeunda. , - This excellent Aroclor success vae aoceopllabed by grinding off or sanding the eurface of the carbon realator prior to impregnating, thue expoeing the Inner poree of the realator, permitting excellent penetration. Penetration hat alvaye been a problem in the impreg nation of realitore vlth resinous materials uoh ae Aroclor. Coble insolation - . 1 . '. . Electrical conductors and cablet insulated vlth asbestos are fre quently lacking la veterproafneee. Impregnation vlth vax composi tions gives am Insulating medium resistant to atmospheric nolstuf* and anmottmee even to immersion la voter Ter. a ahort time, but hitherto no eempoeltloa having the required characteristics of beat resistance and flameproofness has given sufficient voter re sistance to vlthsthatt lasers Ion for prolonged periods. . An improved method of impregnating asbestos is described In 0. 9. Patent *,162,953. assigned tv Rocfcbestoe Products Corporation, vhlch depends on the use of a phenolic resin la conjunction vlth . a chlorinated diphenyl. Xt hee already been proposed'to use each of these cubetaaeec separately for a similar purpose, but alone the first leeks flameproofness end the second.reelatpaee to voter.' WATER PCB-SD0000067081 XOIOAHTO CHBCICAL CCKPAWf 10-1--M The phenolic resin used for this purpose ihould 1m thanoplaetio, olid end rather brittle at ordinary temperatures, vlth a flow point of 105C. Bakelite XR 8430 it suggested ee a suitable typo. The beet thlorinatod diphenyl for this process is stated to Pa on*, bavin* a rieeoelty of 9 tea. Mrbolt at 100*0, and, of oouroa, it nuat nix roadlly with tho phenolic raain. Om containing about 62 par cant chlorine la aald to ba satisfactory, for axaMple, Aro- oIdf 1262. , The two lngrediente aro mixed in equal parta by weight at 160^C, preferably with tha addition of $ par eant by weight of a plastialter auoh at Triereayl Phosphate, tha raaultlng Mixture la atabla and oan ba stored. in aonufaoturlnc tha cable tha individual aonduotora are insulated, ' tviatad and covered vlth tha layer* of impregnated aabaatoa and vamiahad oaabrlc (or tha like) in tha Mannar wall undaratood in tha art. A layer oT looaaly felted dry aabaatoa of auitabla thlet na at la than applied around the thua aaaeablad cable, and a dry aabaatoa braid la applied over tha felted layer of aabaatoa. the o-oovarad eabla la than paaaad through tha impregnating compound (Mixture of reilnoua phanolio eondanaatlon produot and chlorinated diphenyl) while Maintaining tha compound at a temperature of about 155C. Tha tiaa required to impregnate tha layer of felted eebeotoa and aabaatoa braid will depend on tha thleknaea of the layer. As tha cable anorgea froH tha heated bath of impregnating ootapour.il, . it la paaaad through auitable anubblng device* to reaove the exeeet compound from its outer eurfaoa. In order to prevent Migration of the outer eurfaoa eompdund whoa the finiehed wire or cable ia subjected to high temperature# in service, it has been found advantagaoua in aooa inatancaa to ap ply to the impregnated layer of aebeetoe a aaeond coot of the impregnating compound to vhioh baa bean added about 15 to 20d of ground aloa or other finely, divided lndrt eolld material. Tha impregnating compound on tha outer aurfaee of the impregnated tsbeetoe than eentaina diaporaed finely divided particles of the inert eolld Material which aot to thicken the cca^ound and rander it loaa auaoaptlbla to flow. Tho admixture of aiea or tho ilka ia not required or dealrable in the compound uaod to impregnate tho aebeetee layer, ainoe tha aabaatoa fibre# themaalvea latlafao- torily perform tha function of-retaining tha ccMpound within tha meet by capillary attraction. ` . Tha ineuiatod conductor or oabla of the invention poeeeeeis all tho seoeasary eharaatorlatiee of heat reelntaMa, flaaeproofneee, pliability, dielectric ctrength end rcelctanea to water, Tha outar insulating layer'of aabaatoa impregnated-with a Mixture of reatnous phenolic condensation produet and chlorinated diphenyl - ( ia eubatanttally waterproof, even when submerged in water for ex tended periods of. time or subjected to hydrostatic pressure as * high aa 2$ pounds per square inch. In fioerel, tha use of asbestos M0HS 0,4654 ., JBWfc.____ -- WATER PCB-SD0000067082 lo-i-tt " Monjurro chwical ct*?Ajnr a> an elactrleal intulating natarlal hqp haratofor* b*an liaitad to location* vhara high tanparaturaa or tho haaord of lnnoaaablt notarial nad* tho ubo of ordinary fom* of insulation (auoh * m^bor, wamiabad onnbrlc, papar, ato.) undteirabl* or prohibitive. It'Vlll, tharafor*, bo avldant that tha lnvtntlon vldaly axtanda tha uaantlaaaa of aabaatoo inoulatad vlraa and oablaa. - Condanaar* A rapidly growing uaa of Aroalor la ltt tha nanufaetura of tha taall oondenaara aapleyad In fluoraaaaat lighting flxtur##, for offieta, bualnaaa houtaa and faetorlaa. , . ,' i* ` * AhOCLOB BWL5I0H fOBKULA Id pound* of Aroalor - liquid ? pounds of Vatar . ouneaa of gtaarla Aold ' t ounota of Triathanolaain* r4 Tha Aroalor la baatad to a vorkabla vlseeaity abova 82C (l8or) and tha gtaarla Aold la addad and aeaiplataly atlrrad In. tho vatar la haatad to 97C {207F) and tha Trlathaaolamlna addad and thoroughly atlrrad In. Aftar both of tha a a oparatlona hava baan carried out, tha Aroclor-gtcarlc Acid eonblnatlon la poured intu tha votar nlxtura whlla tha lattar la vail agltatad and thanTE# whole nlxtura ip prootaaad through a colloid nill. deed reaulta nay avan bo obtalntd without tha uaa of a aollold nlll, provldwd tha nlxtura la agltatad with a glgh.apaad anulsifylng atlrr*r. . '*. . Tha Aroolera ara not lnflaanabl* and vhan nlxad In auffiolantly largo proportion with nony otbar notarial* hart randarad tha oon> pitta coupound non.lnflannabla. far lnataneo, a nlxtura of about equal partp of Aroalor 2569 and aapholt glvaa a raaultlng ecnpouM that vlll not parait tha. apraad of flan*. Vood nay ba Inpragnatad lurfieiontiy vith ooa of tha hlghtr ohiorlna Aroclor*. aueh aa **o5, that it vlll past tho naot rigid taata now appliad to vood which baa baan traatad for flanaproofoaaa, aueh oa the taata uaad by tha Foraat frodueta laboratory and by tho building Papartnant of tha City .of lav Tort* i* . - , Wa hava not yat found a nsrfcat far Aroalor In tha flald of rian*. proofing wood baaauaa In anat eaaaa vhara tha wood la traatad, for . flantproofnaaa it la wad lndoorv vhara it la not axpoaad to , latching by rain, to that on* of tha phoaphata aalta la ganorally . uaad, Iowa war, thara nay ba apaalal uaaa whore that* notarial*, era not aaaaptablo ,atq| where tha prlat of Aroolpr la Jyatiflad. WATER PCB-SD0000067083 1 10-1 -u r. KOBAKTO CHEMICAL COMPAUf There If throughout tb o cuntry a trenendouf sericet for coapounded ui for all acnner of utff. It U tery llktlf that in low of tho application* of tbtft notarial* it would bo doslnblo to haw* then non-inflABnable. It if also likely that tho Incorporation of Arcelor vltb icm other roaineuf or waxy notorial* would civ* other dctlrablo proportiff. fhoae application* oould probably bo work'd out in conjunction with ocapaniee who aro sow In tho bullnos* of , ccapoundlrt* and telling *uch naterlalo. Tbfro aro oom of thoto ttoapanioo in each of our oaiot territorial! , Arooloro and 5W0 aro tbe'noct likely onto in this appliontion. Toots aro undor war to dotoniino tho suitability of tho eubatitution of Aroolor l?bO for ohlorlnatod paraffin in tho troatafot of paullna aad tentage for uao by tho Any Thif la for tho purpoe* of produeint non-Inna**obility, iaprowlng aoioturo reiifUnce, aad alldew proofing* Tho Arooloro aro remarkably itablo and thalr ouporlority in thlo roopoot to ohlorlnatod paraffin ouetoaarlly employed for thlo pur- ?ooo la dononatratod In tho following rotulti reported by our aboratory. . * Light Stability Tootf In order to bo certain that tho taoto ware ccaparable in trary reapoot, they ware oonductod by ptraonael of tho A* French Textile School, Georgia School of Technology, Atlanta, Oeorgia, The aaapleo used in thoaa teat* had boon prepared at Anniaten prior to thit tifit, They eonalftfd of eootloee of fclorbollod cotton cheating inprognated with oaapooltiona ao ohown In tho tabulation below. Approximately lQjf of ohlorlnatod hydrocarbon vai applied to each of tho Impregnated aaapleo. Tho chlorinated paraffin used had the following characterletloot - Aa win bo noted, loworal pigoonta, namely, FejOj, and CaCOj, wore also applied bo .the fabrle. Thooe pigments wore ueod , in tfio relieving proportional .- Fogpj 10 porpi FoyOy to 8 port* chlorine in t'he ohlor- inntetf hydrocarbon. , . SbjOj - 10 part* SbyO; to S' parts chlorine, 1 WATER PCB-SD0000067084 ' mojbaxto cawxoii coHftunr 10-1-t* In th# tiiti with the plgeented mixture!, to* pigment adhered to th# surface of th* eloth and woe not very evenly distributed. The actual tests Mdt at Georgia Tech. involved exposure Top tvo hours 1a a Qoopar-lovatt lamp cabinet, then conditioning at 700p and 65# *.X. for four hour* or lent*r and finally totting fop warpvla* tontllo strength by tbo grab method with a Soott too tar. Th# Cooper-Hevett cabinet had a Drier* (fuetd quartt mercury are) lup a* tbo course of aitra>Tlolot light. Ob tbo baa it of dyo fading taata eonduotod at Oeorfla Toon, over an extentlv period aovorei yoara ago. two hour** exposure in th* Ooepor-Bovatt cabinet la roughly equivalent to 80 dayi* average outdoor leathering. This relation doee not neoeaeerlly apply to tontllo etraagth deteriora tion toate. Judging by tbo deterioration of the tenelle atrength of unimpregnated aanplte, it would appear that 8 hours* expooure in the Coopor-Eewefet vae equivalent to much nor* than 80 day#1 out side expooure. '' Sumarlted data for the tenelle strength teat* vere at ehown in th* following tabulation! ... . ' . Impregnation Wixtur* / Tenelle atrength fXI Pnexpoeed Exposed Chlonrinated * Paraffin m * * 8*803 o steo) * CtCOJ xroofitor 18ft 5* ft tl * Aroeftlor 12ft 60 n # ft ` ft * 8*803 * 6b803 ft 0aC03 , . ft 8*803 ft 8b803 ft 0*003 Arovlor 5f*t *8 :. ft 8*803 ft *0803 ft OaCOT 57-75 .. 60.9 57.0 . 57.9 M.5 60,1 . . _ . 53.75 ! ______ 59** 58.0 63.* 59.85 : w. . . . . ............- 6o.i 5*5 5*9 68.* ` .. . * ., 15.1 . IT-75 18.85 2* ,0 87.1 2*. 5 25.9 85.75 30.1 3*.9 30,9 33.5 3*.l *0.6 *0.9 (X) Unite arc in.pound# end, except for throe inetaneoe, the valuta shown' ar.e avm..g.oe of 8 feoat i, -*<v - The conoluelcn from thee* teeta wee that the Aroolere contributed little, if any, to tbo deterioration of tenelle strength or th# cloth upon exposure to ultra-violet light, vbereaa' chlorinated paraffin did appreciably accelerate deterioration under the acne WATER PCB-SD0000067085 ` 10-1-44 r MOJOAjrrO CHEMICAL CGKPART * condition!. Also, under the conditions of thee* teets, *11 or the plgnente tried decreased to icu extent the tendering effeet of the ultra-violet light, Thle ie probably not ebnoroal, ainoo the plgventa should here reflected e portion of the light rays. It hea boon reported that certain plpeenta deereeee the heat eta. ' blllty of ehlorineted paraffinj thus accelerating tendering or treated cotton goods upon exposure in hot ellaatee. Beet futil ity testa on ell of the inpregnation mixtures tried aa outlined above are nov being run in the laboratory at Annie too. ' *4 ,, Ccnpored vlth plain cloth wexpoeed (lOQg) the bydrooerben treat- ante alone effected the following improvement in tcncllc strengths: Chlorinated Paraffin . Aroclor 1254 Aroclof 1260 Aroclor $442 7.5g . l.Jp 10. 11.op . This tnorecce in tensile strength through inpregnation le oempencted for In the folloving calculation. Vhen the "Exposed Tensile Strength" Is expressed as per cent of "Onexpoetd Tensile,Strength* the folloving relationship le evident: ( Per cent Reelstanoe to ' Deterioration on Exposure ` to Oltre-vlolet Llxht Dntretted Cloth 51,9 Chlorinated * H Perftcffin * H1 ft t 4 Fe203 Sb20$ CeC03 Aroelor 12tt 54 mt m m * ft203 k 30203 It CaC03 Aro*elor 1260 ft 9 n _v 4 fe203 * Sb203 * CeC03 _* ' 26.10 *9.15. 31.40 . _ 31.52 44.0$ 45.10 43.62 . 44.19 43.36 5561.*00 52.10 ' Are*alor .$442 * 4 Pe203 4 Sb203 * 55.70 52.05 , 3.53 ' __________________ Si*52__________ (. The advantage of the Arselore ' In ecmperieai with Chlorinated far. offln as a aen-lnflsnmeble, vaterproOf impregnant for cotton fob. no es aeeeured by reoistaheo to lose of tonelie strength on' . - , vV`7 - H0NS WATER PCB-SD0000067086 MOJOAJTTO CHDUCAL CQKfAXT u10-1 expoaura to uitra-vioiat light it axprataad in tha foilerving ra- lationahip, bMl aqulralent Chlorlnatad Paraffin traatatnc i* 100#* far eant Zaprovaaant In Haalttanoa to Datarloration ovtr Oeaparabla Traataant with Chlorlnatad Paraffin Arotoo lor n it 12to54 to to k * * rtso3 BbS03 CaC03 Avaraga , '56.7 ` *4*7. ;.i - to.i r 48,4 Aroolor ft 1t2o 60 to to * * It ?0203 BbSO> CiCO? .' . Avaraga Aronolor * to 5*to4S int k faSQS asbsos k CaCOS . Avaroga 5*.> Ji 98*2 78.6 102.2 lOT.p . 68.9 96.7 Haat Stability T*tl . Thaat taata vim and* by abaorbing and titrating tha HC1 avolvad from so groat of ohlorinatad hydrocarbon vhan bold at 1?5C and blovn vith air at tha ntt of 0.01 oublc foot par alnuta for four hourt. fhia la tb* aatbod ootlinad on pagaa 37S-37B of tbt Aug- uat 30, 1?A>, laaua of tba Aaarloan DyaatuTf Raportar, Vol. 32, Ho. 18, Jaaaa H. Radaand, taxttla Tachnologlat, Jafftraonrllla, O.K. Dapot, vaa tha author of tha artlela. ;- Data for tha taats that hava baan ocaplatad vara aa follovai Chlorlnatad Hydrocarbon Coapoaltlon . . # HCl Hvolvad In . a hra. at 175C SO SO 20 SO fU. gm.` gat. gu. Chlorlnatad * IT *. Paraffin V * . / V / ' a.O 10.5 6.3 ' gai. gM. CM. ' FaSOJ Obsoj 0*003 0.4l 20.00 0.29 , . .0.29 SO 20 !S2O pu. EM. *ga"u. Ar.cteo lor to n 12% 54 to to . 0.00 / s pu. PaS03 0.01 A 9 W* W0S , ',,0.01 ft ^a. OaCO* / .. !Vi, 0.02 -}-< - -Vr-\r hiik1 moms otaaf -,"J&U.BhXi- S WATER_PCB- . 10-1-44 < . M0N3AXT0 CHEMICAL CQMPAHf Chlorinated Hydrocarbon Coiooiltlcn % HC1 Evolved In 4 hre. at I75e 20 gau. Aroolor 1260 20 gw. * * / P pae. P*2M 20 PM. " " / 2 pu. 8b205 20 pee. * * / 2 pu. CaC05 0.002 . - 0.02 0.005 0.01 20 gse, Aroolor 5442 20 pee. * " / 2 pie, Pa203 20fM. * " A 2 CM. Sb203 20 pae. " ' / 2 g. CeCOj . 0.00 0.00 0.02 0.02 That* data clearly deeonetrate the nartcedly tuperlor heat atability of the Aroolor* *a oenpared to ehlerinatid paraffin, Particularly l*niricant it tho accelerating action of Fe205 on the decomposition nt of chlorinated paraffin. Ho inch accelerating action vaa noted vlth the Aroolort. While Id meat of the teete with the Aroolorequr titration* lndl- e*ted the evolution of HC1 ranging up to 0.02%, the titration* vert o snail u to possibly toe vlthln the range of experluntal error. At any rate, ve ere Quite oure that 0,02% HC1 evolution represent* the uxinua SCI loee under the oonditlona of the teete. ( Chlorinated Hydrocarbon % HC1 Xvolved In Mixture 4 too, at 175C 20 pu, Chlorinated Paramo end 2 pu, Zlno Borate #5167 , 20 pae. Aroolor 1254 and 2 fne. lino Borate #J16T ' 12 cm. Aroolor 544a and S gne. trlereayl Phosphate 12 pae. Aroolor 5442 and S cm. frlereeyl Phosphate and 2 pi. Pe205 . 12 CM,.Aroolor 5442 and 8 faa. trlereayl Phosphate and 2 pea. b205 ,. . ' ' . 15.6 0,01 0.02 0.00 O.oi 8 pm, Trlereayl*Phosphate and 2 pee. CaOOj ' 0.00 8 pee. Trlereayl Phosphate and 2 pee. Zlne Berate #516? . `- 0.01 Again It will be noted that the Aroolore are far note etable than Chlorinated Paraffin ij\ the pretense of. Zlao Borate. . HONS **bb0 WATER PCB-SD0000067088 KOtOAMTO COMICAL CQHPAR 10-1-M BEAT TBAJOFBB MBPICH Aroolor hu been used far a number of Tun at Anniston u a Heat transfer medium. it is now employed as such In tha HB-tO plant. Company (075050) used Aroelor at a heat transfer Medium in min* talning a aoltan load bath in vhleh thej soaked lb insh amour plotting projeetilea. They operated on* unit using Aroolor and onother using Dovtherm. Both of thaaa unita vara uaad for several year*. They than dlioentlnuad the uaa of Aroalor aftar dlaoovar* ins corrosion in tha Aroolor system, vhleh did not ooeur in the Dovtherm eye tern. - .a * A company developed aoan equipment for heating pyrltaa in vhleh they intended using Aroolor aa tha heat transfer medium. Slnea tha equipment vaa never sold ooeenerelelly, none of thaaa unite involving Aroelor are nov in operation . Many people considering Aroelor as a heat transfer aedlua gave it up either because it vould not stand tha temperature they required, or on account of fumes ocming fron the'Aroelor, or baeauaa it eoat nor* than oil normally used for thla purpose. Favoroble features to the use of Aroolor for this purpose are t 1, Liquid at roan temperature. 2, Does not oxidise. " 5. Bae nearly tvise the specifla heat of petroleum oils generally used for thla purpose. *. Boo-infloanable. afPRAPLiO PLOXO Company (57$,*50) operating a high praseup* stem-electric gener ating plant use Aroolor 1248 oa an hydraulic medium in their gov ernor system. They do not use it ax h lubricant. The Aroolor is used Instead of oil, Merely because of its non-inflammability. When oil Is used in the governor system. It' la euetmary to use the erne oil reservoir, both for tha lubricating and governor ays tecs. When Aroolor it used in the governor eystom and petroleue oil in the lubrieotlng systea, it Is necessary to atgrigato tbs tvs sys tems and use eeparote pumps far the lubrieotlng and governor eye- veetinghouse have been the principal promoters of tha use of Aro elor in the governor system as * result of having the. oil in a foveraor system notch hr* in one of the Jersey Central Light and over Company's stations vhlle Veetlngbouse engineer* vero working with the unit. . .. . ____ HONS 092M1 3w. .VSto' **<*; V-\ WATER PCB-SD0000067089 i* io-i-a* ^ MOJOANTO csatXCAL COKTUTt ilABU Ceapeny (10**60) ha* obtained iom interesting result* with bakedon onsaela containing Aroelor 125*. Aeryloid Main and Trlcrwoyl Fho*photo, plgMntvd with Titanlu* Dioxide and Zino oxido. Tho ' onanol- la baked on at 1350 (2T5k)* tThT have found that Trl~ oresyl Riocphate alda the Aroelor oa halting, .giving a hard surface. Thlf aiao ocnpany hai found that alua of Aroelor and Vlitanex (Ho. 6 B-flO and 8*100) or Aroelor And Tixtae (Bo, 1 and No. 2) glvo lntaroatlng properties .*enevh*t Ilk* shellac. 'They a tat* that these product* havo good adhtolon. . LAOQOBM . Vo havo a Tory good goitoral lino-up on tho uaa of Aroolor In laeauora la tho booklet P-115 vhleh va havo publlahod for distribu tion. Thil booklet givoa tha Halts of acapatlblllty of Aroolora 185* and 1868 in ftltroeolluloao lacquer*. Since this booklat ho* boon publlahod, a nuabor of ooapanloa havo atartod uaing Aroelor 12*8 in apeeial flexible lacquer*, aueh aa art uaod on high tenaion cables, ate. Tho compatibility Halta of Aroelor 12*? are highor than thooo of tho hightr ohlorlno Aroelor* ao that it la poaslblo to Incorporate enough of tho Aroelor to glvo It extretso { flexibility, you havo tho fomule for Aroelor Lacquer Ho. J* which givoa tha detail* of tha uat of this Aroelor In cable lac quer. Tho work don* in our laboratory uaing'Aroelor la laoquer* indi cate* that vo get soaevbat loaf chalking with tho Aroelor lacquer* than with those aado up by-other fuvulas. Vo got practical frta- doa fra* ohoelclng and or*eking and, wa bellevo, bettor color re tention in tho white and light colored laequart. The** ar* lapor- tant considerations In lacquer nanufaeturs, and Aroelor eheuld bo given noh aoro consideration froa now ca for general ut* *ueh ac an automobile iaequor, etc., than It has received in the peat bccauac or the riling prleto of other resin* which ar* g*n*rally uaad. ' . V* have maber of euatoscre who use Aroolora 1?*2, 185* and 1862 . la tha.aaaufacture of lacquer. 1 ' , Lacquer yomulatlon Chart Hon-Volatile Constituent! 1. A resin '. , 2. Hltroeelluloee (cellulose nitrate) >. A plaatlsiaer or oftoner . . ' .4^ SONS WATER PCB-SD0000067090 BOSBASTO CHWICAL CCM?AMY ( Volatile Conetltuent* ' 10-1-M - 1, The Alcohol constituent 2. The eater constituent 3. Tb# hydrocarbon constituent Finished Lacquer ' .' - Z per cent of the non-volatile (100 -I) per cent of the volatile The percent*!* X, of the non-volatile or fila-fomlng constituent!, My vary betveen 200 and 30$ of the valght of tb* finished lacquir Won-Volatile Conetitucnt* . . . At bit bem tbovn by the title, the non-volatll# ecuponenta of t lacquer eontltt of a ret In, eelluloe* nitrate and a plaatlelaer or softener, for the ream, too* one of tboee of synthetic origin nay be employed, or a natural ream tueb *a Him Dinar nay be used. Gun Dtnar la a generally uted realn in lacquer fomulatlon, and it can be taken at the nutter one eonponent. The nuiber tvo component la the oelluloae nitrate Itaalf. It la aleo kaovn a* Hltrocelluloee, pyroxylin and "FX." To tb* Indue try In general It ie "cotton." it can fee purchased In tvo klndt, tb# A3 and As grade*. Tha latter t grada la tb* one that la obitfly uted by laequer aanufaeturere. The initial* indioat* a difference in tb* nethod of manufacture, AS neanlng tbit tb* eotton la aleohol-aolubl#,' and RS neanlng that It la regularly soluble. . ... Both grade* are uaually bought vet vlth denatured alcohol. Tb* vlaooelty of tb* eotton la another detemining factor vlth regard to Ita us*. Tb* eotton tbat.lt covonly enploytd by the industry hat a Tiaeosity of ona-balf aaeond and la known at "half-ascend cotton.*- Per the third component dlbutyl phthalate, trloreeyl phosphate or eaator oil nay be used. ,' ` ' At thu point an explanation of tha terms "plaatlelser" and "sof tener* beecu** neeetaary. The average laequer technologist usee these tame aynonynoualy, and for this reaaoa they ba*e ecu# to ean almost on* and the earn* thing In tbit industry. Strictly peaking, a true plMtlelaer should be a solvent for tb* "cotton" and tbs ream. In addition, It should hove e lev vaporisation lost and should confer eueh properties a* flexibility, pliability, and durability on the lacquer film. Both dlbutyl phthalate end trloreeyl phosphate Met thee* requirement!, Castor ell, on the other hand, doss hot. In that it le only a partial advent for "eotton." Zt does, hovevar,'give to the.fllm the oualitle* al ready MntloMd, in abort, it exerta a aortanlng effect - hence {. the name "softener.* ' The difference, then, betveem a plaatlelaer and a "softener* la that tha former la,a true ..solvent, for the . -f V- >' * . ' ir . .* MOHS 0**3 WATER PCB-SD0000067091 . * 1Q-1-A* NoA)rro eanjCAL comfjuit ( non-volatile constituents of a laeguar, while tho letter 1* * noniclvent, or, at bolt, only a partial solvent. Cm tor oil la typi* cal of this letter elan and la widely used aa a laequar "aottonar." Volatile Constituents Tha rolatlla conatltuanta foim whet la Inown aa a balanced aolvant ' mixture, the purpose of which la to bo used aa a solvent or thinner for tho non-volatile constituent*. Tha component* of this mixture must bo In ouch a proportion to o&oh other ao aa to insure a uni fora evaporation rata when tho laeguor filn drloa, and alao to make aura that no precipitation of tho "cotton" will occur at tho tint of thinning. 1 Tho number one, or tho .alcohol, component la generally composed of ethyl alcohol - gjjt and batyl alcohol Tha oator component le made up in general of ethyl acetate end butyl acetate, while the hydro* carbon component usually eonelati of eaeo.compound such ae toluol or, for special leeguere euoh aa eablo dopes, bentol. Finished Lacquer ' The finished lacquer le prepared by taking a given weight of the non-volatile constituents and dissolving them is a given weight cl' the volatile constituents. t Competition , The queetlon of competition will have to be viewed from two angles; first with rfcgard to -the Areolor* aa resins, and aeeond with regrr.l to them aa softoners, 81ms tha Arcelor* have aort the properties of softoners than of reelne, the softeners are nearly competitive with the Aroelors than are the reelne. Competing Bealna - Synthetic name Humber ` Kanufacturer . Amberol 801 tha Beslnoua Froduota * Chomloe}* Cc. Rilladalphia, Fennaylvanla 1 Bokellte ra-xw Bakell t# Corporation ' . ' hew Tnfe, hew Torfc ' -- Beaked te (1110) (m*) Beck, toiler k Company, Xno. Detroit, Michigan Olyptel General tieetrie Company Schenectady, hew Tort * ( Lewisel If)' John D. Lewie, Inc. ' ' 'f F.r.o.v.iden..oe,*-fI.no--d,e. ';I,s.land i. . .. _ A-,-.. r .. .. V--08*. tfp.insa KOHi 001*6^ l .b . ic WATER PCB-SD0000067092 MOIBAHTO CHEMICAL COMPAffiT * conatinc Raalna - Synthetio io-i-a Naae Umber Manufacturer Paraplex* itt) The Raalnoua Product* 4 Chenleale Co. Philadelphia. Panaaylvanla tillResyl Aaarloan Cyanaald k Chemical Corp. Rev York* Rev Tort Resyl Balaaaa Aaarloan Cyanaald * Chanleal Corp. Rav York, lev York Taglaea - American Cyanaald li Choaioal Corp. Rav York. Rav York Peroplax can probably bo conaldorad a softener aa vail as a raaln. Cmoatln* Raiiot - Soml-STBthotle . HamaMmbarMtiwfaaturor later Oua Kona (One of Thar# ara many manufacturer* the Boat ' generally'- ' i used r#*lna.) - Natural Realna . Qua Dammar /Batavia) (Singapore) Imported - obtained through broker* -1 Cawpatlnn Plaatleliar* or 8oftanara Ran* 'OradaTrade llaaaManufacturer Bibutyl Phthalata* Monaonto Cbenical Co. St. Lout*. Missouri Tricraayl Phosphate* _ - Honainto Chanlsal po. St. Loula, Kiaaourl .Kronltsx Kavalao Produst*, Jnc. . Ifltro, Veat Virginia ' Lindol Celluloid Corporation Bevark. * Jersey Abalyn - (A roala produet . Hareulea Povdar Conpany . ' rteoHaendad for . Wilmington, Deliver* f laoquar formulation) ' '" -23- * MOHS ........................* .* >a*Lij... y*w- f'. ' * -Skt-SE' 1A.----;.'. : .inmo.- * WATER PCB-SD0000067093 lO-l-M r MOBAirro CHEMICAL COWART competing flaaticitaro of Boftanara Want Orad* Trad* Kama Hanufaoturar ABM-100 (A Modified lina**d ell for laoouar formulation) Areber-Danlala Midland Ca Milwaukee, Vlaeonain Cat tor Oil (Baker*)* thabar 4 Rwber 15 ffunber 16 AA Blown Tha Baktr Caator Oil Co. Blown Joraay city Raw Joraey Blown Unblown Spenear-Rollogg Oil (A aodifiad aaator Spencer-Kellogg k Bona oil for laequwr . Buffalo. Raw York formation) ` Vhar* art other aanufacturara of tbaaa produot* thia Hat la by no aaaha oanplata. In Hating thaaa produeta, only tboac that in in aora or ltaa son- oral ub* havo boon inelvdod. Thoro aro aoaa notablo axoaptlona, bowavar, in tho eaaaa of aueh aatorlala at Abalyn, ASM-100 Oil, and Spanoor-Callogg Oil. o ^ Tha natoriala 11atad In thaaa tablaa auat not ba thought of an- tlraly at competing produeta baoauaa thay aay bo aora important aa alda or auxillarla* in oo-davalopaent wore with tha Arodtor*. In foot, it la ballotad profarablo to ragard thaa aora in thia light than aa eoapatltora. ' Advantage* In thinking of aay advantage* tha Arcelor* any bav*, tha atatannt< soda In tha final paragraph under "Coapatltlon" auat ba borna m alnd, it la profarablo to confine onaaalf to a dlaeutalon of tha outstanding propartlaeof tha Arcolor*, for it ia ballavod that it la only through tb*.development of aoaa apaoiflo proparty thot pragraaa ia going to ba mad*. . Tha proportioa of tho Aroolora that should b* emphasised nrot 1. Low waperiaatlsB loot ?. hi* oolor . . ' 3. Adhaaloa *. Chwleei Stability a. . to light b. ta water, acide and alkallta o. to boat -. ( d.. to oxidation '" a. to ahoaical aotlon in general MONS Otltb* . V : ?' .. . w.-w. 1 -c WATER PCB-SD0000067094 NOMSAJTTO CBXKICAL COHfAJtY 10-1-44 ( 5. Xcn-lnflaaBablllty 6. Kon-corroeiveneae 7. Solubility in oonnooly used lacquer solvents A resins of tha properties that Aroelora lapart to lacquers and the type* or ltequar* for vhleh they ere rectnoended nay ba given briefly ii followsi ' . Zn a Deanar-type laoquar tha plaatieier-*ofttnsr combination, such aa tha uaual dibutyl phtholete-eastor oil combination, may ba sdvantageoudy raplaead by an Aroolor alona. Tha resulting laequar la laaa cubiect to enaoking and cracking on outalda u> poeure and retains its gloat. t ' Aroolor 1262 nay alto ba aubatltutad antInly ror tha rat In In eartain typaa oT laequar. Tha elaar laequar, ao produced, la praotlcally colona*a and provide* an excellent bate for whiteenamels. Such enamels, howavar, do not vlthftand weathering aa wall at tboaa containing Danner in addition to the Aroolor. The advantageous propartlaa of tha Aroelora In imparting added weather resistance to properly foranilatad laoquere nay be traced to their reelataaee to the notion of sunlight..to their perman ency la tha flla, and to their axtrena ehcmloal atabillty. The c Aroelora do hot oxldlta, "dry," or harden. Tha Aroelora are un affected by dilute aelda 'and even by hot oauatie aolutlona. They are not eubject to polynerlaation, rancidity oT other change, aa far aa la known. '. When added to a nitroeelluloae aolutlon, tha Aroelora reduce the vleooelty alightly, This change la viscosity takes place at once and no further change due to the proaenee of tha Aroolor oceure on several months aging In eloaad containsra. By virtue of thtlr high refmotive index, they impart apparent depth to tha laequar flla. Aroolor 1262 hoa adhealve propartlaa and the ltequera containing It have good adhealon, Laoquere con taining tha Aroelora dry normally and give a hard, non-tacky, durable flla of excellent gloaa- . Certain laequar teehaeloglata have found that a laoquar contaltohg Aroslor eaa ba poilehed with a ainiaua of rubbing and, furthermore, that tha Aroolor aeeat to lapart a harder finleh to a lacquer flla than ollt, trleretyl phoephate, or dibutyl phthalato. It hae also been reported that properly formulated laoquere containing Aroolor chow no tendency to "epee" or "event out" whan buffed. - in addition .to'tha propartlaa of general interest,) other proper ties of the Arcdors nro of \luv in femulating lacquers to fit pedal requirement*, Aroolor* 1254, 4165, 5460 and 1262 do not ( cupport ceaboatlon, and when present in nitrocellulose fline they -25" * 'i .. t \ J* homs oeia*7 , D'eMitMT^e'* ^ * . -- WATER PCB-SD0000067095 HOSAirro chekical cwpaky . retard the rata of burning. The Aroelcre retard tha rat.* of traris- far of moisture and of gaaaa through a nitrocellulose film, and by virtue of thia fact have already found extensive uaa in protective lacquer* for application over thoee type* of eleotrlcal insulating material*, such a* rubber, that deteriorate rapidly in contaot . vitb oxygen, osone, moisture or other vapor*. ' Procedure . . Upon visiting a lacquer company, even effort-should be made to , eoe the chemiet in charge of formulation or production. In largo oompaniaa the director of roeeareh ehould tlvays be eeen. Ac a ; general rule, a great deal vlll not be accomplished until these ' respective individuals are eeen. i . . ; * A complete diecue*ion of the properties of the Aroolort should be given, emphasis being pleeed upon the possible formulation of a new lacquer vitb some one of theee properties as the background. Vhen discussing the use of Aroolort in lacquers, the talesman ehould remember that the Aroolort are not eolventt for nltrooel- luloee and that for this reason an exceeslve amount or Aroclor must never be used in the formulation or a lacquer.. The limiting percentages that can be used for suceeeeful results have been carefully vorked out by a large number of expdrimente. The feu simple rules that must be rolloved in formulating lacquers vitl, the Aroclor* are tiSeffied in a booklet entitled "The Properties of Tuo Aroclor* of Special interest to Manufacturer* of Lacquer*." Oopiee of this booklet may be bad on application to our sales offices, it is rseonmtnded that the talesman offer oopiee or this booklet and the bulletin "ttasticlsera ft Resins - Organic Division" to interested lacquer manufacturers. . Attempts should be made to determine vhat particular lacquers n manufacturer specialises in and vhat problem* he is etudylng at tie time of the call, . .- Aroolort have fair or good compatibility vlth nitrocellulose, pom* var, Butvar, vinyl copolymers, polyvinyl acetate, polystyrene, chlorinated rubber and ethyl cellulose. In general, tha liquid or eml-solid Aroolort aet like true reelne. One principal value is thtlr bhemlcal inertness. Vbere great flexibility is to be ob tained, It may be neeeaeary to employ auxiliary plasticisers. Sofcj of the exceptions are in chlorinated rubber and in ethyl ocliuiota vhere flexibility or hardness mt be varied simply by seltotlng as Aroclor of the proper physical eharaeterlstlos The liquid Aroclor* such 'as 1242, 1248 or 1254 vlll greatly in crease flexibility but vlll cause softnes*.. .The etmi-eolids such as i60 or 5442 vlll Impart tom* flexibility, vlthcut the marked ( softening effect. Tho brittle, resinous Aroolort such *e 4*65 or 5460 produce very hard ccmpositlona vlth excellent adhesion end HONS 092666 AfiSSfiW-Jff . . .:.k WATER PCB-SD0000067096 JtOIBAirro CHEMICAL COKfAXT .* *f weathering qualities. If m tingle Aroolor do** not inpart th# d- aired combination of propertl#*, uaually iom Mixture of Aroeior* vill do to. It would nn that la polyatyrane adding conpoal* tion*, tna realnou* Arcclora could b* uaed 4* 4 flux or flow pjo- ooter 4t adding tanparatura* without causing oftn*aa and flop, at noraal tanperature*. 9om Mixture of Aroelora or a seablnatlon of an Aroolor with another plaatloltar aithar aolld or liquid < sight b* required for thla purpose. . ' ' Of court*, it la vail known that for alkali re'aiaunt coating*, . combinations of Arooloro (125b-1260 and 5*60) vitb chlorinated rubber have b**n uaad for a long tint. At th* present time, the ua* or equal part* of Aroolor 5b60 and ethyl aelluloa* 1* b*ing pushed by Company (331650) at a vaatbar raaiatant coating. 5 in liar coatlnga of lew vlaeeslty polyatyran* and Aroolor* would probably ba of value, -. AJBCf-mVY AERONAUTICAL SPECIflCATIOH LACOPTO - CAHOUTLAO* AH-L-21 , 6 October ISO - Pag* lb . TABUS rv . Control Formula - Clear Vehicle ------------------ WelaEt------- Weight-- iba. par ingradiant* farcant 100 gal. voium* *01*par 100 sal. Pareplex BO-2 ' (1006) 11.1 90 m Anbarlac B-9b Arcdor 5b6o (806 in XTlaaa) 5.6 - *5 ___________ (1006) b,3______ _ 55 - e> Eton CalluloaefP to b seeHl006) b.3 Cellulo.a-inr.t*(Jg^JJi) ,.g 35 75 * %' "*T1 Ajqohol Eth/l Acetate ' - `* .. .-a ` * ~ Sutrl Alcohol ' *. i2.b ' n m Butyl Acetate ' _____gg.b__________ #e Aroawtld' Patroleua naphtha Ttp* 1, Orade B T 22.5 ' \ ` ' b" 5 15 " 25 * * " 85'' .r--H*-` St* ..v.ifSstefcfcliie* ---.-te.v.A-;, MOWS 0016*9 \w iWP2sfiJMhj*jwapw*a3V.# MJ ..V WATER PCB-SD0000067097 MORSARTO CHEMICAL COM?AW 20*1.44 It la also or value in other reslni where a highly alkali r. slatsnt plasticiser la required. Papers by Sovran, Paint . Technology (reference for December 1936* dated January 1937) indicate many possible application* for tb Aroclora, Sale* to lacquer trade at present- are oonflnsd to specialty msaufao- turert. -' The compatibility of Aroclor 2*65 In 1/2 second nitrocellulose is indicated ast ., .; 1. Seteeen 22.20 and 26.50 by lnepeotione for bluah in thin aged films. - ,' 2. Between 13,70 and 16.60 by inspection for loss of gloat In thin aged filna. '. - The presence of a mutual solvent sueh as dibutyl pbthalate raises the compatibility. ', The formulation of a flexible lacquer designed for oven drying le given aa follows) - Ron-Volatile 250 Volatile 750 (15*20 See. B.S. Kltroeelluloae [Tricresyl Phosphate (Arcelor 1242 -e (Beneol ' (Alcohol (Ethyl Acetate ' ' ft 280 620 220 1S0 This fomula la intended for application followed by oven drying. Air drying at atmospheric temperature causes blushing. . A modi fication of the volatile portion Is suggested whan air drying le used. > ' Volatile Alcohol' Itbyl Acetate .Butanol Butyl Acetate Toluol 6.20 6.20 6.20 30.80 50.00 Ixperlmante on neck Insulation and lacquers for aircraft indi cated trlereayl Phosphate as a aheioe over Aroclora in Ethyl Cellulose laequore, especially sines there la no tandency to settle oat when Triorseyl Phosphate le used. Aroolor le mere effective in flame retarding, however.,, - - . Stop-Off Lacauere . . . Rather dtailed information la given In the iteneanto (tirgante Product* Piviaion) Plasticisers and Begins Booklet oh the preparatlea of tritreeellulose leequaro oootaining Aroolera. A - r' * . . ".T'yJiftSA HONS 092*10 WATER PCB- . ,, MONSAXTO CHEMICAL COMMIT* 10-1-** ugg*eted'formulation it ae follovt* . 1/2 secondJTltrooelluloee, Dry Aroolor 1260 . Trloreeyl Phosphate Saatlclter B-le may be substituted for Trloreeyl Phosphate * 100 30*70 39-70 Xf the Mtrooeiluloee ltttlf does not hot# sufficient resistance, a competition of Aroolor with a chlorinated rubber, Ithyi Ceilu. lot* or t Vinyl Satin again utlng Aroolor It suggested, and if ' tho flexibility It not tuffleltnt, it can bt improved by tht addltlan of a small Mount of on* of tho liquid Aroolor* tuh at 12*2 or 125*, although again Trtorosyl Phosphate or Santlelser B-16*oeuld bo used. In ooatlngt, at a general rule, the hard retlnout Aroolor* will produce very .hard end very reel*taut compositions, but thee* viu be brittle. The liquid Aroolor* vlli tend to produce flexibility but may be leaking icoevhat in adhealon* It le for thet re*ton that vs have euggetted Aroolor 1260, which le about half-way between end will produce a combination of flexibility and adhe lon. it will be obvlou* that herdnete eon then be Increased by the addition of a harder Aroolor euoh ae 5*60 or the flexibility, can be inereaeed by tht uee of a liquid Aroolor. The Aroclort ^ themeeivee are unaffeoted by aeld and alkali. Stop-Off Voxee ` The ehcreoterletlee of a 1 top*off wax ehould be * follows! a. Tightly adherent to metal surfaces; ' b. Should not be removed at a bathr temperature of l6oy. 0. Should not be'affooted by the add* or alkallet of electrolytic bathe. , d. Should prevent eleotrolytie aetlvlty on the surface covered. - e. Should be capable of roeioval by oelveat vapor phato . cleansing baths, by molting in boiling wattr, or ordinary cleaning Solu> tions. . ' Suggested eaepeoltleris are at follow*t -' Softening Point Methlde (Monsanto Merrlmae) Aroolor 5**2 ' *0* 60* 118C. Methlde (Monsanto'Merrlmac) 20*' Aroolor **65 . - BO*. ios^c. An attempt was made *0 use theme compositions in solution form by dissolving them in turpentine. fhle woe not particularly WATER PCB-SD0000067099 NCMAXTO CHSMICAt. COKPAW 10-1-44 successful ilno* at roes tenparatur* th* degree or eolublllty vs* l**i than 120. It might be possible to u* 35% eonoen- tration of vox in turpentine at 50-75C> palatine th* metal j aurfae* vlth th* hot tolutlon. ' , ' j, . PAIlfTS Paint* containing Aroolor have ihwo remarkable durability;Tar bttr than any other .paint* against vMeh they ear# Uitn. . ,J#f ; * ' , '* On* **riou drawback* hov*v*r, la that paint* eoniatntng Aroelor do not broth * readily a* th* normal haute point*. Point manu facturer* iatr*t*d in quick drying paint* thould b* *neourcg*d to try Aroelor.. Under var condition* there la great inter**t in th* manufacture of rir-preof painting for tb* interior ef chip*. Aroelor* should b* a definite contribution to their formulation. Aroelor 5460 le successfully used .in camouflage paint vhar* it Impart* flameproofness , ' ' ` VAPWI8KCS Th*r ha* been only a llaittd amount of work don* in our labora tory on the subject of Aroelor in varnishes and frem that work u ^ haa b**n concluded that the moat likely field for Aroolor in arnlahee le In conjunction vlth *ome other retin euoh a* tettr Oum or Damar. or one of th* other commonly u**d gum*, ainee th* u*e of Arpolor alone haa, In our experience at least, -given a t&ekln*** to th* film. . , `- Aroolor 1262 mixed vlth Seat India Oum and eut vlth naphtha fur- nlahe* a varnish beat. . The Aroolor* may be u**d in alkali-proof Varnishes by incorpor ating them a* a cold eut or a* a chill bade -- and for the pur pose ve reecaaeend Aroelor 1262. The Aroelor may be *ald to function either a* reala or at an ell. Xa other word*, by th* addition of tb* Aroelor, e abort oil varnish take* on many of the phytioal characteristics of a long oil vamleh. Our work along this, line haa indicated that th* beat preoedur* le to oook ' (la the 'usual manner) using a* a realn bee* a pure pbenolle realn but using cnly half tb* usual amount ef ehiaa-veod ell, Vb*n the varnish attain* proper body, th* Aroolor may be added directly aa a ahtll back ead the vamleh then tMnmd ii> the usual eanner. *f * * ' Since Aroc)or 1262 la 'semi-solid reeln/ it le beet heated until liquid before introducing a* tb* chili beak. , - An optional method ie.te diaaolve it in the thinner end add in the uaual thinning operation. - Tbie vee vorkad out aa a possible aaana ef axteadlng the euppU*i:ar ehiaa-vood ell. Za ether word*. It acts me an.oil.aubatttuta nor* tb*a,ap_*.r**la *ub-. atltute. -- -............. WATER PCB-SD0000067100 MOnAJTTQ CHEMICAL COMPART 10.1*44 In ragard to th* alkali rasistanoa, vs have found that prevldad tha other natarlals have, of thtuilm, considerable alkali mmtnct, than th* Aroelor vill add to that raalatane*. It la not poiaibla, hovavar. to uaa a raaln auch aa llMd roam or aatar Buai having poor alkali raalatane* and impart high alkali rails, tanca by th* addition of th* Aroelor, - .. Aroslor 126? ean be used to rtplaea up to 50% of th* ehlM.veod oil in varniahaa, -- 1. Xf aatar gun, roain, or other ehrap raaln la uaad, th* vimlah vill b* aultabl* only for Interior vork. 2. Xf a good 100% phenolic r**in la uaad, th* varnish vill b* satisfactory for axtarlor purposes, Varniahaa containing Aroelor 1262 ar* not superior In Quality to tinllar varniahaa nada vlth tung oil alma, vlth th* poeaibla ex* coptlon of a vary alight Improvssant in alkali raalatane*, flvxi- bllity and adhaalon In bob* formulation*, < - Varniahaa containing Aroslor 1262 toftsn at lovpr tamperaturas `than do varniahaa tnplaying only tung oil, and so ar* nor* sub* Jcet to "printing" and narring when vam, . ' The advantage of increased flexibility of Aroelor varniahaa la loaf at lov temperature* due to embrittlement of th* Aroelor, Beteui* Aroelora valgh aor* p*r gallon than ehlna.vood oil, they increase the coat of varniahaa (vhloh ar* sold by the gallon) *v*n If put at.th* **m price p*r pound aa th* Dll, . l^OBHICAWa ' An outstanding aarvie* la parfomad by Aroolor 1254 aa a lubricant for high praaaur* air eompressore operating at 4400 pounOa par square inch preaaufe., Besides avoiding flaambllity, It la elalned that feha lubricant 1* tuparlor to oil, no oorroalon da* rcalta result, and thare la no exoaasive vear an the equipment Company 15650). . . Conpany (297950) la using Aroolor la a apeclei droving ocnpound\ Company (541970) tasted Aroolor 1240 in one'of their punpa operat Ing at 2500 pound* praaau, r* vlth tb*, followin# g retuitai . ' , CcBpreaaiblllty ehanga it 0,5% compared to 0,5% for petroleum oil. The vear rate of tha pump va* moaaured by observing the slip of the pump at intervals during tbs anduranea run, Xnapastlon of th* pustp shoved th* veer, to have ooeurred on th*. platen holt valla in th* oyllndar and on th* hardened aurfaoe of th* plntl*, tha aur<* face of tb* plntl* f*lt vavy - not emooth." A vaap pat*'of 22% per 1000 hour* vaa found to axlat, Tha via coal ty 'slop* of Aroelor 1248 vaa poor. . . . ......... ................................................1....*.*.*.*.*..'.... : \ V. HONt 2fc73 ' WATER PCB-SD0000067101 '. HOUSAUTO CHEMICAL COMPART 10-1-44 The conclusion of these tests is reported u follovsi Arocior 1248 is not s very satisfactory fluid for general use in oil sr pumps at 2500 pounds per square Inch, It is expensive as the pump requires special paint on the Outside and inside; the oper ating range Is liarro* and the veer rate on the puap teste was , per 1000 hours at 1009 and 25 pounds pressure. Our experimental vortc In using Arocior ss a lubricant In steam ' turbines was not successful, due principally to the fact that the Aroolor le cf such high density that it plain up any bit of grit that nay be In the system end floats it up la. ^he bearing, Petroleum oil having so much lover density allove aoet of these partidee to settle in the bettesi or the r1taervoir, United States Patent #2,245,649* assigned io Celluloid Corooratlon, describes a steea turbine iubrleant eonalstlng of 50-parti of chlorinated diphenyl .end 50 parte .of trleryi phosphate, E. P, Lubricants ' Much attention is being given by lubricating sen to the utter of Increasing the flla strength or load carrying capacity of lubri cants, particularly sc as to be eble to use smaller gears for a given load .- There ere a great many such lubricating compounds now on the market. As a class they are called "Extrema Pressure* or B. P. Lubricants. : ' . It is veil accepted In the lubricating industry that by the addi tions of certain elements as Chlorine, Sulphur end others in the proper form to a lubricating oil, a certain ohemloal combination takes place vith the Iron or steel metal bearing surfaces. Tnese surface compositions tend to prevent, eelaure of the rubbing sur faces under extreme loads and under vhleh loads, if the sole lubricant vee a pure mineral oil, eelaure or scoring would result at once through film failure * , * In attesting to discuss Arcelor as an extreme pressure bass, it la very difficult to evaluate-its comparative, load-carrying . capaoitiee..vith.other extreme pressure bases,, such as lead soap, active sulphur, saponifiable oils, sulphur chloride, etc., without actual result# from exhaustive teste not only of the various E. P, testing machines# but also from actual sarvioe under normal operating conditions; .It le recognised by the lubricating indus try that results obtained oa testing machines; such as Ilmen machine, Timken machine and ethers, mean very little unless the results are correlated and proved by service conditions. It is true that la the paet Arealor has been tested as ea I, P, base on the Timken aaealne at Timken Boiler Bearing and on the Osneral '* * i `Vt `VHpS.t'fsir .t` '.`Ai'Vj-vi V is- ViJ'`ufc'st WATER PCB-SD0000067102 MOfBAXTC CBSH1CAL COMPAJH 10-1.** . Kotor* machine at Oentral Kotor* B***arch, and is *sch os** the Aroelor addition ha* shove a marked inersat* in load carrying capacity. . - . . . Several companies art purchasing Aroolor today for uso In 1. r. Lubricant*, but indications art that they iMtUt add other trasnt* along vlth tb* Aroolor to achieve ccmmereiel result* at a lover pries. Sine* v* has* never run service test* os the Aro olor oursslT** and th* fa* companies ourchasing Aroolor aro naturally veryreluotant to divulge their experience along vlth vhat other chemicals; if any, they are using in conjunction vlth the Aroelor, the beat that can be done ie to offer consents by several of the ocmpanles vho have tested the Aroelor and possibly give a general interpretation'or suggestion* aa to vhere It night find nor* general present day application, . * ` Top Cylinder Labrieent , ` * Beoently the practice of putting a Xubrleaht in motor gaeollne has beone Quito general. This la, of oourse, to lubrleata the top section of the cylinder. . . We have tvs oust oner* vho purchase Aroelor regularly for uss in the top cylinder lubricant, which they noire and sell. We do not lenov the function of the Aroelor in this us* other then that.these eusteners tell us that it prevents tb* depoelt of carbon on th* velvet, Ve understand that they use a relatively snail percentage of Arcelor in the lubricant. On* or these cue toner* uses 'Aroelor 13*8 and th* other usee Aroelor 115*. . W# have-dons very little vork vlth th* Aroelor as a top cylinder lubricant but vould suggest that Aroelor 12*8 be used in snsll percentages. This Aroolor vill brfound completely soluble in lev visooeity oil and should not cause any appreciable difference in its cold test. This is often added to the gaeollne to achieve top-cylinder lubrication, . , -. . ` Caepaay (735900} obtained excellent results wing Aroelor 125* . on a bearing teat, operating in straight Aroelor at. 255-260? {12*-1290) for tve veeke. Jtueh lees carbonisation and decom position than vlth the usual spindle oil under the tame condition*. PLASTICS Compatibility of iroelors vlth Celluloe* Acetate Ixpsrlmental Wort. The ecapatibillty liait* of.^Aroelor 1369 var* oetaxminsd 'vytn rive grade of .celluloe* aestate, Per these . WATER PCB-SD0000067103 P ` homahto chemical cckpaw . io-i'-44 cellulose acetates the limits vere M follovt ' Eactmaa Cellulose Acetate Bomber Compatibility Limit of Aroclor 1262 (par cantl a70im between 1Q.0 bid 13.6 between 16.2 and IT.9 between 13.1 and 16.6 Between 17.8 and 19.7 .between 16.r and 1B.1 " That* figures, aa vail aa ail tba ecnpetiMllty limits'given in this report, refer to the limite aa detorrlned on thin films dried aiowly in dry air and depoeitog fraa solutions containing, .aa ia cueternary, 0.1 cram of "tollda* per euble centimeter of solution. The solvant vac a mixture of 80s by weight of ethylana dlchloride sod 20jf of alcohol (denatured, formula JA). Another eolvent mixture comprising 33.30 acetonei 33-30 ethyl laotate; 16.70 alcohol and 16.70 ethyl acetate (all pereentagaa by weight) vaa leaa auitabla than tha advent given above, and gava lover compatibility limits in the cases tried. The compatibility limits or several Aroclora with one cellulose seetate (#10296) vtre determined. Tbs observed limits vara as follows : * -. ' Aroclor Ho.Limit ? Per cent! 12*9 Pra 'to' 98.7 from 2| to 29.1 Prta lo.4 te lB.l Prom 14.2 to io.6 Proa 10.1 to 13.0 The ternary aye teas, eompriaing a eelluloae seetate, Aroclor 1251, and a ccomon plaetlclaar, vere lnveatlgated. . A -.V-* ; ' ' Tbs oonetents of tbs eelluloee acetates, as given by Eastman . Kodak Company, are aa folAovsi ; ' .Cellulose ` Aostyl ^Viscosity;**', W.-'. Acatata So,: (Par pent) . (Beoondci .; j.- W *. ` . 702? - Jo'l'i;.' 7 . , ?S ; &* ' ^ -; . 10296 .... V .t-Oapreaponda lb biasesitf .' - Sc., v sbaraotar(atiee appro*., , ' Sr-i u- : 'SSm .tbO,5.aaacnd7Ltcquar,, ..... . . ... -V. -.. > Xitrooelieioae.7 ...... . ->^!P" -V.*? V *I ` was 09**7* WATER PCB-SD0000067104 KOHBAKTQ CKSKICAL COHfAW 10-1-M Conclmlon* Th* compatibility limit* of varlou* Aroolor* in 4 ipaelflo oelluIom aoutt* and of on* Aroolor in varlcu* etllulo** iciutti or* oomparativaly lov. Th* typ* of *olv#nt employed tffet th* ob served 11*11* <th* tolvent vhioh give* th nor* ftvorabl* r**ulta being th* mlstur* of thyl*n* dlanlorld* and aloohol. Th* com patibility llalta of tb* Aroolor* In ooilulot* ooatot* or*, in general, nor* difficult to detemln# and l**a readily eh*ok*d than th* llalta In nltrooallulot*. Th* actual- observed Unit apparently d*pnda upon tb* rat* of drying, th* thiokhes* of th* dpo*lt*d flla, tb* huaidlty of tb* air, and th* aolvont employed. la th* t*tt* of compatibility sad* by Saataaa Kodak Company, th* llalta vr* found to be 50 to 100 (kittenhouce). Th*lr lov r* aulta vara probably du* to tbalr aotbod of datotlng Incompati bility, In vblb d*11eat* optlsal-method* were employed to detect baa* In th* flla. Thr verk on tb* *ff*at of Aroolor* upon tb* rat* of burning of celluloM aoatat* film*, a* glw*n in tb* tabl*, lead* to th* following oonolualonat 1. Ctlluloa* Aeatat* alon*'burn* alovly, 2. Th* rat* of burning, where burning take* plaoa at all, 1* aec*l*rat*d by aoh of th* *ub*tane*a triad. 3. Vhlle th* Aroolor* iner*a** tbarat* of burning, tb*y at tb* tan* tla* glv* a fllokarlng uncertain flam*' which . tend* to go out, that la, they t*nd tb queaeb tb* flan*. >1. Triphenyl Fboapbat* la an *ff*tlw*' flameproof*r, it be. lag impo**lbl* to Ignite th* film containing 25ft of It. 5* If flexibility and laek of tendency of tb* flla to vrlnkl* or burl on drying If taken a* a orltarloa of plasticising power, -th* Aroolor* art nor* *ffaetlr plasticiser* than ` either dibutyl pbtbalat* or Tr^oroayl fboipbat*. 6. The thick flla containing 290 Aroolor 135* {slightly btlov th* ecnpetlblllty Unit for thin flla*) va* biuihed. This 1* in aooord with th* *arll*r observation* of th* ffaet of film tblefca*** on th* compatibility Halt. Company (756595) ba* found that aixturss'of deeachlorodiphenyl ' ,and_*tyr*n* ar* non-lnfleamable and bar* a beat dietertian point aoTP higher than polystyrene. ' ... ' . United but** rataatgo.2,*27,657, aatlgMd to Lv*rku**n-l.O, . v*rk, describes a composition of natter ecmprlclng a r*sla-llk* chlorinated diphenyl of an average ehl orin* conUnt of about 62J ' ' V ? t ' <k ......... *. ' ' ! *. * ' ,,/ . ; At) *- . V- * * ` ,Sar' WATER PCB-SD0000067105 M0R8AKT0 CSZKZCAL CWfAJCf - 10-1.44 and. bout 7.5Jf of polyvinyl oapbcaolt. ' TOBBtH 1 ; ' Company (297100) htri found that Aroolor 1262 it tht bast plat. ticlMP for rubber hydrochloride. It la eoapatlblo up to 1006 ' rubber hydrochloride, although tht utual voicing rang* it 5 to 106 of Aroclor 1262 baaed on tht wight of tha chlorinated rubber. Belov 506 Arcelor no difficulty it onoounttptd vith brittlaneaa. Apoelop tandt to lnoraaet tha gloat of rubber `hydrochloride nine, . e.g., Tliofora, Pliofilm, niolitt. Pitt pop oaat rubber hydro* chloride addad to Aroolor padueat tha took. 'v ' On tho othor hand, Company (331850) rooceawnde tha uaa of Aroolor 1251 vith chlorinated rubber, e.g.p Parlon, jcsssKyt^rT' A rubbar composition of raduead flammability .ecnprlieit^'''**'*' '*"** Rubber . Chlorlnatad rubber Aroelort Sulfur Zlne Oxlda ' Vulcanising Aooalarator Anaoniw Borate 100 partt 35 partt 65 parti 2.8 partt 5 partt .1 part 40 partt Ttu; competition ahova a float retlatenet' and a notabla abtanea of salting around tha burning material. Aroolor 1268 it uttd ih tha aanufaotura of Callula* rubbar of lov fleaaability for tha aircraft induttry. ' _ Coapany (284114) bat found that ISf of Aroolor 1242 addad to Viatintx (pel7butane) aaktt a de-ielng coating for alrplana pro- pa11ara that look! pponialng. By tha addition of plaatloltar C-2V or plaatloltar BO, lot taaparaturt eharaettrittlet ean b* obtained, ... . . . It it indioattd that Aroolor 12l2 may oet at a aolvtnt for ona of tht nattrialt vhloh it producing taek in Bqna S., . - Tha ehapMtarlttloi of Typo B Beoprenc eoapoaltiont art aald to b improved by tht addition of Aroolor, 1251 inopooting vatar raalatanea. (Company 16917) Tht uaa of Aroolor 5180 is undap invettlgatloh at an axttndar for Htct> OB. ' \ ' : Tharo art atTtral different applloatlona for'Aroolor in rubbar at follavai ' . j. aacv-.v' . , , ' , ~`-r' * - "*** .'.pCl . 'V WATER PCB-SD0000067106 H0J3AHT0 CBBHJCAL COKMITY 10-1-4* As a plasticiser for hard rubber Aroolor 126? baa been used as a plaetlelasr for hard rubber m dental pittee, eto*. fop a oouple of years. It should bo equally useful-in pleatIdling bard rubber for otbtr purposes vhare brittleness la undoalrabla, ' . To render rubber psnaanently taekr . '* Aroelors 126? and 125* arc killed Into rubbop' ao aa to oak* a . hcaogeneoue coopound vhlch baa poraanant tacklneis or adhesion. To flaneproof robber. Esoprena. and other wathatlo rubbers Aroolor 1269 la a bard crystalline utarial of high Waiting point. It nay be ground very fine. This finely ground Aroelor la allied Into the rubber Just a* any inert filler would be. The allling teaperature la not high enough to aelt thle-Aroolor and to there le no eolvent action. It has bean found that the Incorporation or aufflolent Aroolor 1269 In rubber prevent# the epreed of flu*. Thla le euggeeted especially for flaaeprooflng rubber for uee on Inaulated wire. ' . , . THEJM08TATS Aroolor 12*0 le being used by several ahnufaoturers of themoetate as the expanding medlua In the bulb.' Aroolor haa been uaed in this eervlee Sr one auufaeturer for the last ten yeare. Aroolor*hat proved entirely eatlefaetory. Avery precaution suet be taken to eliminate the poeeiblllty of moisture or othor for eign natter getting Into the Aroolor. The themoetat equipment auat bo thoroughly oloanod before filling. We do not reocaaend the use of Aroelor at `twpernturea above 6ooop (31500). ... ' TBXTUZg Company (6*5300) report* that Aroeloro , although aore expensive, eurt better fire retardant effect than ohlorlnated paraffine and eaaller uounte are required. . > 4i...........................&...... . Company (0*9900) claimed that Aroolor* 1262 and 5*60 ehovod a 10k increase in ten*lie strength then substituted for the stand ard Jeffersonville Quartermaster hepot apaaiflod inpregnant for rope, vbleh le tha*4relies v*ing fo. rmu*la*. rV f* , 1 tig Copper VaphtDenote 800-8 98k 1*5 Asphalt * > rr'. 30g Hraffin Viz . -...n-UtP*'?# 13k Klaarai Seal oil *v-.s; >. op WATER PCB-SD0000067107 HOBAXTO CKWICAl# COMPAHT 10-1U4 Aroelor i960 la proposed a flameprooftug, waterproofing, nlidavproofln* agent in tha production or J.Q.P.'a pacification 242 peullna and tinuff for amy uat. Zxact fotnuiation1 and approval of th Quartern*tar Corpa has not yet boon worked out. ' -voop- * Aroalor aa an Introflar for Sulfur In Wood Incremation ' < It baa btan found daalroblo for iom purpoaaa 'to-impregnate vood and other flbroui natorialo with tulfur. however, sulfur dooa not go Into that# natarlala without difficulty. The uat of 10% . of Aroelor 4465 nixed with the tulfur acta aa aa Introflar. caus ing thorough paaatratlon. - . . Tha impregnation la performed aa followsi ' ' A mixture of 906 eulftr and 10% Aroclor 4465 1* melted and nixed '**! A. and plaotd In an autoolava or pressure tank with tha wood or other a&tarlal to bo Impregnated and bald at a tonporatura of 125C to l4oC and a prataura of 100 pounda par square Inch. Tha tint nacaatary dopandi upon tha kind of vood or other notarial Paine treated. The initial fretting point of tbia nlxtura la 107.5C. , Tha vlacoolty at l25C la reported aa 97 Second* Saybolt Dnlveranl. / A typical impregnation of a yellow- pin* 2* X 8" plank gave an increase In weight of 127% and about 1000 in tanall* atrength. The valuable quailtiae contributed by thla treatment are added atrength, rigidity, resistance to moisture, to aelda and to splintering. The eleetrlael insulating properties ere Increased. The wood la node practically free frea tha affect of weather and roc leta attack by Intacta, the treated wood is practically free frcai shrinkage and swelling.* .'. . feasible uaaa of wood treated la thla way arai trananlaalon line eroasaxma,' . tanka to recict adds, ana. . . . Equipment In whidi availing or splintering la objactlonabl*. Timbers llksly to be attaeksd by termites, ate. Perhaps nany other applleatiohs where the qualities described above arc desirable> , i. - Tha requirement la that the wood so treated should stand being 1 . uaed 15 or 90 tinea in caoereta rorne, that.lt nuat remain smooth, and not ahoe annular ring or grain strueturei an tha concrete. - . . * * v + > <*v 4*av n . - - WATER PCB- c JtOJBAJTTO CMM1CAL CCWAJII from Mother isrlss of taata conducted on hickory fishing polo handles It is ooncluded that the boot results will he obtained using the followInf eoDdltionst , . Traperature Vacuus Ataoaphario pressure 90-1000 16-100 m. for 95 mi*. 5 ala. , Senate, drain and dry ' ' .!* ' .. iuBcttMmooa* Purdue Oniversity found that Arcelor 1943 wee eery useful as a baas upon which to flow gelatin solutions for the production of nine, thus asking it possible to oliaUMtt.asreury for this purpose. ,* . As a result of interest aroused la the Aroelors, several sugges tions have been nods regarding uses which nay prove of value* 1. Ardelor 1360 as an adhesive in a joint eenpound for glass building blocks. , . 2. A water emulsion of Aroelor 1263 for use in leather* paper) r%. textiles, rubber and casein paints. . 7. As a protective coating 00 certain pigaents to prevent "llvering" of paints sontaining rsslns of a high acid nuabsr. Specifically, sine oxide plgaent in veter ami- sion of 'Aguaples? * water swlsiftable slkyd resin. 4. A waterproofing for concrete, * '. 5. Aroelor 1969 or 5460 as an ingredient of soiling' eoapoel- tioaa aade with such natorisis as ethyl cellulose, bsmyl ' cellulose, soy bean asal and com protein. > (. WATER PCB-SD0000067109 MOSAirrO COMICAL COMPAJTY 10-1-M aoocnnD fomcolas fox xoiaTowtyxocruo ___________ OOMFOOIPB________- . Coapound A t Coapound X. ` Coapound 0 Qeapouad'D 96,Of Arodler J^O .Oft lard. Paraffin 96,Of Arpaler **$5 4.Op lard Paraffin 96.0ft Aroalor 5060 *.CJt lard Hraffla 96.06 Aroaior *065 .Op Bard Paraffin Whan a ralatlvalf lc* (oftanlns point aatarlal la da- alrad, a* ucfat tboaa ooapounda. using APoalor Ato5. Vban a talfhar aoftanlnt point la rsquirad, %a outcast tte ooepouada uainf Aroolor $460. ' Compounds C and D ara felsdk aatarlala aad.ara uaaful ' whara oolor la of no laportaaoa. . Va do not prapara that# ooapounds. . ' ^ . . . . / J. Tw *T5v tt' nONS 0020*3 . -A.. IJ* . xv * ;\"i: WATER PCB-SD0000067110 four retiusst for toxielty d* for reply. has teen referred to sc The following constitute* the have for Aroalor 1221, Au.ii.fa - r.tfc - jynrw* - Undi7ut*d - 33C0 ks/tyj. Clawed as Acute mninwl Lethal Done - KsbV.lt - fomalss CUrped Intact Cl.in > wJw <. jiui a^'i;,;," diajie<l as silently toxic, 20 m? Dorsal - Kabbit - 12,5J solution in corn oil - Drily appllsati-a IMJ iz`Sk/ ucy - moutreto adverse offsets ii body welGnt, wit;', wok;*, w, lucslcude, and loss 01* appetite, . 390 mc/ks/daj - This was ostabllshed so the ttosn ID50 by elan ubeorptlon, nitre was only slight adverse effect on body weight. Ito taaAvA^S - There uore no untoward offeets in any or these anisalc, Hscatologla studies and Urine onaly&os rrca tho treated anlsoiln . eoapared veil with thoce of the treated control group. - There were no significant gross or aloroseopie patholcvic ti-m-.- alteration* noted oneni the surviving test anlsals whJ.ua were wtortflcod. 9 X trust till* 11 the infoinetlon that you seek* Slneorsly yours. MBS bi W.S. Clarv Wllllea H. i!vtnt, Pil.n. Taaioolo^lut 1-k.tlteal lopurtwent I WATER_PCB-SD0000067111 DRATT LETTER fflOCMB.,U4t Aroelor 1342, Monsanto's modified capeditorfluid is replacing Aroelor 1242 in the manufacture of capwitors. This new chlorinated biphanyl product i i idantical to Aroelor 1242, functionally, bat has ba a modified to raduca tha content of highly chlorinated coapc >ants. The reason for this change is that environmental * .udies suggest that tha more highly chlorinated components especially those containing five and six chlorine atoms |er molecule, are store pars latent and therefore mors likely to|| accumulate in the environment. Aroelor 1342 will comply with new racooj endstions by C1CRE that capacitor askarsls should not contain mi re than 3.5X pentaehlor and more highly chlorinated biphenyla. To ensure that Aroelor 1342 complies with this specification s phisticated analytical methods will ba employed to monitor tha oduct. Sinee the Aroelor 1342 retains the fune ional characteristics of Aroelor 1242 it is unlikely that any ch igea will be necessary in capacitor impregnation processes, no| will the performance characteristica of finished capacitors changed. Therefore Aroelor 1342 will be supplied igainst your orders for Aroelor 1242 received on or after July it 1974 when production of Aroelor 1342 is expected to commence It la not our intention to charge a premium for Aroelor 1342. 09za*j WATER PCB-SD0000067112