Document bOON9YKVaEJpxgLzR55QoQy53
Memorandum
El Segundo Refinery July 5, 1978
REVISED REMOVABLE INSULATION SPECIFICATION_____________
MR. D. L. BROWN:
The latest removable pad spedStfications (March, 1978) require a layer of stainless
steel foil to cover the inner_insulating material. In the Hitco CRES ! pads, this
foil layer is the outer "skin." in contact with the valve or flange surface. This
specification was added in October, 1977, due to problems with the original Hitco
pads. The first-generation Hitco pads had a single layer of 0.001" aluminum foil
next to the surface being insulated. This foil could not stand up to normal
refinery handling and hot surfaces. It rapidly deteriorated exposing the inner
Fiberglas pad. This was considered unsafe, and the requirement for stainless steel
foil ensued.
^
.
Hitco revised their first generation pad shortly after these problems to include two layers of 0.002" aluminunrfoil as the inner skin. This is their "secondgeneration" pad. Just prior-fb changing our specifications to require;stainless steel foil, we purchased thesez double-foil pads for the Pro-Poly Plant, Coker, and No. 2 Crude Unit. Most off these pads have been in service about nine months now.
I recently checked a number o_ these second-generation Hitco pads to see how two layers of aluminum held up to^normal refinery service. Thirty pads in the PPP and Coker were inspected. Bo.th flange and valve covers, in service up to 650F and ranging from 2" to 12", were checked. Two manway covers on a PPP reactor were also inspected. The results of this inspection are as follows:
1. Of the 28 flange andjvalve pads inspected,, six had small tears through both layers ccf foil exposing the insulation. However, except for two of the^pads, all the tears were near the outer edges of the pad, and were apparently caused by stud punctures. They would not be a hazard in service, and could be reused. Two of the pads had largertears through both foil layers. Although reusable from an insulation standpoint, they would be susceptible to oil soaking, and should be replaced. (The number of times these pads had been removed and replaced is unknown.)
2. On valve covers, there were typically several small tears through one layer of foil at the edge of the valve bonnet cutout. These would not affect reliability or reusability.
3. Pads in dirty, oily/coking service (leaking flanges) showed no signs of deterioration1, and were remarkably clean inside.
Chevron BB 015160 '
2- -
4. The aluminum foil "crushes" around the valve or flange surface, creating a tight heat barrier. This is a real disadvantage to Hitco's third-generation CRES pad with its relatively nonconformable stainlessr steel foil.
5. The two PPP reactor manway covers have been removed and reinstalled
numerous times at catalyst change-outs. They take a terrific !
beating, and as expedted, both pads had several tears through both
layers of foil. There was no evidence of inner insulation deteri
oration or hydrocarbon contamination, and both pads were still
doing a fine job of insulating. In extreme cases like this, it
will probably be necerssary to replace at least some of the pads
every year.
-
Based on these inspections, I believe we have been overly conservative ;in requiring the use of stainless* steel foil in our current specifications. In the case of Hitco pads, their double-layer aluminum foil pads meet our criteria well enough to continue theirjuse. There is a considerable cost advantage in eliminating stainless steei.foil with minimal loss in reliability.
I
The attached specification has been revised to accept either stainless |steel foil or two layers of aluminum"foil. Should future inspections contradict the results -of my study, we may reimpose the stainless foil requirement. For now, we will use this newest specification in all future bidding.
Attach, cc: RMA
JPE GNM
M. A. BELL
Chevron BB 015161
REMOVABLE PAD SPECIFICATION
All removable pads must be suitable for hydrocarbon service, whether used in hydrocarbon or steam service.
1. All pads must be designed and constructed for a minimum life of two years with typical handling by refinery maintenance forces. The removable pad must be^able to withstand general refinery use with out mechanical failure.
2. Insulation inside the ^removable pad must be protected from absorbing any liquids or vapors^originating at the flange or valve surface. A water resistant outer coat and a hydrocarbon proof barrier between the equipment and the'pad insulation are minimum requirements.
3. Pad covering material JLn contact with flange or valve surfaces must allow reasonable drainage. Fiber glass cloth, stainless steel foil, or two layers of aluminum foil are acceptable as inner surface materials, consistentswith Item A.1 above.
4. Removable pads must have a permanent hole or slot in the bottom to allow drainage of liquid drips. The width of the slot must be 3/8" - 5/8".
Temperature Requirements ~
1. Removable pads must be-^nble to withstand a continuous inside surface temperature of 750F.
2. The outside surface temperature of the insulation must be less than 140F. This includes Tacing hooks or capstans.
The exterior of the removable pad must be water resistant over the life of the pad as a minimum requirement.
Inner surface material used to protect the insulation inside the removable pad from absorbing liquids ixr vapors originating on the equipment being covered, must include a layer- of stainless steel foil or two layers of
aluminum foil. This foil must cover the entire inner surface of the insulation inside the removable pad. The foil must also cover this insulation on its exterioriselong the drainage slot edge, to a distance 3" from the edge of the pad.
Fastening devices such as lacing hooks or gromets must be securely anchored into the removable pad. JThey must not pull out of the pad and they must not rip the interior or ext^'dixSEof the pad when tightened.
Sewing on Pads
-
1. All stressed seams mustlbe double stitched, at least.
2. Thread with a minimum diameter of .012" and pull strength of at least 14 lbs. must be used. ^
3. All seams must have at /Least four stitches per inch. All seams must be tested for strength inr the sample pad.
Chevron BB 015162
2- -
4. Cloth which has been fut during fabrication of the pad must be; treated, coated, or stitched so it will not unravel or fray.
G. Sharp or pointed objects on the removable pad must be shielded to avoid injury to personnel during installation and removal.
H. Each pad must be easily identifiable as to size and pressure rating (ratings) of the equipment which can be covered by the pad. This information must be stenciled onto the removable cover.
I. Wire used to lace the pads together shall be stainless steel with a minimum diameter of 0.025'!.
J. Required minimum widths on flange and reboiler covers are as follows:
Size of Elange (IN)
Width Required
3 ......................................................... 13
4 ........................ .................................13
6 7.............................; .... 14
8 ......................................................... 15
10......................................................... 15
Greater than 10"...................................... 16*
(IN)
*A width of greater rghan 16" may be specified.
Revised: 7/5/78
Chevron BB 015163