Document bBpo9x9Ggq2wMG8DGQm9rrqoZ

' ;# v* retains asbestos -T\.. Note the high opacity and brightness of the paper on which this reprint was made. It is a 70-lb. offset grade produced by P. H. Glatfelter Co., Spring Grove, Pa. The rigid opacity and brightness specifications for this high-quality paper were maintained when asbestos "T" was substituted for part of the TiOL, in the furnish. r a high-purity pairing: asbestos- titania H I help are all (he appearances of a solid future for asbestos in papermaking. So Union Carbide Corp s Mining and Metals Div. iNew York) thinks. For proof, the division points to over 200 mills that have used the fiber for retention, pitch control, saceall recoveries and softness. Now the company, confident about its markets, has brought out a modification of the original high-puritv asbestos -- what it calls asbestos "T". with the fiber intimately bonded lo titanium dioxide. This bonding, says Carbide, means that Tiff. retention is at the same level as that of asbestos, said to be tbe highest of all furnish fillers. There are two other features also important lo asbestos "T. ' The titania in the new product is dis persed uniformly throughout the fiber and doe# not agglomerate in use, yielding maximum optical efficien cy. And at the same time, asbestos "T" improves the retention of separately added TiO-j. clay, cellulose fines and dvestufls in the furnish. i d'lTisn r- \ l ! ^ v r The reason asbestos acts this wav lies with its elec trostatic charge. At most pH's, the positively charged asbestos has a strong attraction for negatively charged TiCb. This pull is great enough to hold the titania contained in the product and still attract particles of separately added TiCC that come in contact with the asbestos in the furnish -- and the bond holds up un der severe agitation. This effect is also responsible for tbe ability of asbestos to optimize the optical efficiency of Ti02. Without asbestos in the s vstem, the TiO_. particles tend to agglomerate, reducing their optical effi ciency. But the strong opposite charge between as bestos and Ti02 helps keep titania scattered uniformly throughout the sheet, and this uniform distribution retains the optimum surface area and size for optica) efficiency. Result-, mills have found less TiO- is needed in the sheet lo obtain a given opacity. Mill experience has shown that asbestos "T" im proves tbe retention and optical properties of Ti02 Ao^U UCC 014810 * f /tfin ifit f 2 ii AVERAGE ANALYSIS IN PAPERMAKING SYSTEM 50 LB. OFFSET BEFORE TRIAL % TOTAL FILLERS DURING RUN WITH ASBESTOS "T" 72.09 40.92 STUFF GATE HEAD BOX mm16-5615,17 PAPER TRAY WATER STUFF GATE HEAD BOX PAPER TRAY WATER Figure 1. During this production trial, 50 lbs- of Union Carbide's asbestos "T" (4.3%) replaced the equivalent amount of titanium dioxide in preparation of the furnish. Carbide's California mine supplies high-purity asbestos. to such an extent that in many Furnishes, 1 lb. of asbestos "T" can replace 1 lb. of Ti02 without sacrificing opacity or brightness. Carbide now figures that since asbestos "T" costs about two-thirds as much as Ti02, the substitution can yield significant savings. By making a complete or partial replace ment, says Carbide, mills have cut papermaking costs by $3-8/ton. And they can achieve these savings by using the compound in much the same manner as the company's high-purity asbestos. How the prod uct's handled: the "T" pellets (used for compactness in shipping) are added to the pulper or beater, where they open up into short fibers that mix with the fur nish components. (Carbide recommends that asbestos "T" at first replace up to 50% of Tt02 content, but not exceed a 5% addition, based on cellulose content. With experience mills can replace more than 50% of Ti02.) Once in the system, asbestos "T" provides im proved retention by reducing solids losses to the tray water and the subsequent buildup of solids in the head box -- and it improves solids recoveries in the saveall, thereby reducing their loss in the mill effluent. The end-product, says Carbide, could he a paper with such pluses as better sheet formation, smoothness and printability. Such benefits from asbestos "T" have often resulted from mills which first started with the high-purity grade and then graduated to the new formulation. What follows, then, are detailed results from several mills with experience in both these re tention aids. ON TO OFFSET One of the first production runs using asbestos "T" was at an operation making 50-lb. offset paper. Mill goal: to replace part of the TiOo in the furnish with asbestos "T" on a pound-for-pound basis. Thus, dur ing this production run, 50 lbs. of asbestos "T" (4.3%) replaced 50 lbs. of Ti02 added to the beater, and specifications for the paper were maintained. Trial run results showed the presence of asbestos "T" improved the retention of separately added TiO- bv 18% while retention of all fillers improved by 16%. And the single-pass retention of asbestos "T" (includ ing both the asbestos and TiCK. in the product) was 57.1% -- higher than the other components. (Figure 1 shows the total filler and TiOt percentages at various points in the papermaking system before and during asbestos usage; single-pass retention figures determined from these numbers are indicated in figure 2.) For the overall system, asbestos "T" improved the retention of separately added TiOa by 9.6% --- from 76.2% to 83.5% -- with asbestos "T" retention (both components) at 79%. Mill analysis shows that 75 min. after additions of the retention aid were stopped, the head box contained 4.5% asbestos "T" and the sheet, 2.6%. On the basis of this information, Car bide says, the asbestos remaining in the recycle system continued to work effectively long after it was re moved as an additive. UCC 014811 JULY 1966 <r ' The improved retention provided by the asbestos reduced the loading of inorganic solids in the head box and buildup in the tray water. At the same time, the presence of asbestos "T" in the saveall improved re covery there. At the head box, the total filler content was reduced from 41% to 30%. As for the solids con tent in the tray water and saveall: Total solids, Ibs./lOOO gallons No With asbestos asbestos Tray water 26.54 17.14 Saveall influent 18.08 13.60 Saveall effluent 0.34 0.11 Thus the solids in the tray water were reduced by 34%, while the saveall influent and effluent were re duced by 25% and 68%, respectively. Overall re brightness averaged 85.3% compared to 85.5% be fore. Moreover, claims Carbide, high values wrere maintained despite a drop in the Ti02 content of the sheet from 8.66% to 7.34 % when asbestos "T" was substituted for part of the titanium dioxide in the furnish. Supplier and customer conclusion: data con firm the ability of asbestos "T" to optimize the lightscattering efficiency of Ti02, yielding improved opacity and brightness at lower filler levels. IT'S A GIFT Asbestos "T" has yielded similar results in other production runs. For example, a mill producing 25-lb. white gift wrap used 30 lbs. of asbestos ilT" to re place the same amount (or 50%) of the Ti02 going into the furnish. According to mill information (see figure 3), the new asbestos formulation improved across-the-wire retention of ash by 28% and sepa rately-added Ti02 by 6%. Retention improvements for the entire system were 50% and 15%, respectively. Retention of the asbestos "T" (both the asbestos and the Ti02 in the product) was much higher than the other components -- 41% across the wire and 76% overall, mill personnel reported. SINGLE-PASS RETENTION. PER CENT 50-LB. OFFSET f^BEFORE TRIAL coveries in this flotation saveall increased from 98.1% to 99.2% in the presence of asbestos. This mill, says Carbide, was most concerned with the maintenance of its opacity and brightness specifica tions. However, all quality specifications were met opacity was Icept at 91.0%/ vs. a prior 90.7% and TOTAL FILTERS TiO* (SEPARATELY A0DED) CLAY ASBESTOS "T" Electron micrograph (left) shows the dispersed par ticles of titanium dioxide clinging to the asbestos fibers. Asbestos "T" itself (figure 2, above) improved the single-pass retention of filters and titanium dioxide. UCC 014812 A07646 4'hvniivul 2H These results reduced solids in the tray water from 7.8 lbs./lOOO gallons lo 6.4 lbs./lOOO gallons and saveall effluent content from 0.79 lbs./l,000 gallons to 0.53 Ibs./l.OOO gallons. The brightness of the paper increased 3.5% with the addition of asbestos "T" -- rising from 79.3% to 82.8'%, making it possible for the mill to replace even more Ti02 while maintaining the original 79% level. Opacity with asbestos, how ever, was down slightly- This was due in part to a 2-lb. higher basis weight when no retention aid was present in the system. GOVERNMENT ISSUE Meanwhile, Union Carbide's regular high-purity asbestos has been proving itself as another means for reducing day and Ti02 input. Some mills, says the company, take advantage of the improved retention to obtain quality improvements without adding addition al fillers -- and Carbide claims either objective can be accomplished with considerable savings in fur nish costs by the use of asbestos. One mill which obtained such improvements used asbestos in the production of 40-lb. government off set. An average of 2.20% asbestos was fed into the machine, replacing an equivalent amount of clay, and TiOi additions came to 3%. Results: asbestos im proved ash retention from 23.4% to 25.6% across the wire and from 40% to 51.5% overall. (The total ash AVERAGE RETENTION, PER CENT 25-LB. WHITE GIFT WRAP content at various points in the papermaking system over a three-day period is shown in figure 4.) Because of this improved retention, the Ti02 content of the reel was increased from 1.16% to 1.40%. This meant an increase in opacity from 89.3% to 91.2%, while brightness remained the same and all other sheet specifications were met. This mill also obtained a substantial reduction in traywater and saveall losses: Total solids, lbs./1000 gallons No With asbestos asbestos Tray water 149.9 113.7 Cloudy effluent 28,0 13.0 Clear effluent 17.7 6.2 The addition of asbestos led to a 20% reduction of tray-water solids (Ti02, clay, cellulose fines). And at the same time, the solids in the cloudy and clear save all effluents were cut back by 55% and 65%, re spectively. TAKING OUT TITANTA Another mill producing 40-lb. white opaque paper used the improved retention obtained from asbestos to reduce Ti02 addition. Initially, 3% high-purity as- ASH T.Oj ASBESTOS (Separte)y 'T" Added) ASH Ti0? ASBESTOS (Separately "T" Added) Figure 3. Asbestos "T" (which come* In the rod-shaped pellets shown on the right) at this mill boosted the retention of ash and titanium dioxide across the wire. UCC 014813 40764? JULY 1966 1 bestos was used to replace a similar amount of clav. Then the TiOi additions were reduced from 8% to 6.8%. This resulted in an ash retention increase during the production run from 38.4% to 40.6% across the wire and from 68.1% to 71.8% overall. (Data on this analysis throughout an 11-hour period are shouin in figure 5.) But despite the reduction in TiOj, the ash and titania contents of the paper at the couch remained about the same as before the trial. The TiO; content averaged 6.26% with asbestos compared to 6.12% before, and opacity and brightness were therefore kept at 92% and 81.5%, respectively. As at the other mills, tray-water and saveall efflu ent solids were markedly reduced: What all this data {>oint up, Carbide hopes, is something the company has claimed over the past few years -- that asbestos isn't as foreign an aid to papermaking as its industrial history would seem to imply. AVERAGE ASH ANALYSIS IN PAPERMAKING SYSTEM, PER CENT 40-LB. GOVERNMENT OFFSET YffiA BEFORE TRIAL Total solids, lbs./lOOO gallons No With asbestos asbestos Tray-water 30.3 25.5 Saveall influent 22-0 19.2 Saveall effluent 11.7 8.9 MACHINE CHEST HEAD BOX REEL TRAY WATER From the figures, the mill estimates that traywater solids were reduced by over 15% while losses from the saveall were slashed by 24%. Saveall re Figure 4- Carbide's high-purity asbestos does well also. This furnish held 2.2% of the liber, enough to raise ash retention by 10% across the wire and 30% overall. coveries improved from 47.0% to 53.7% with asbestos in the system. Asbestos' contributions apparently have not been limited to paper. Board producers also report signif AVERAGE ASH ANALYSIS IN PAPERMAKING SYSTEM, PER CENT 40-LB. WHITE OPAQUE icant improvements in retention by using the high- ! purity variety. One mill producing 28-35 pt. white vat- lined chipboard increased the retention of pigments i in both the topliner and underliner, as measured by the decrease in solids in the white water. 4" In the topliner system, 1.9% asbestos was added to the furnish without any other change in the furnish J) components. White-water solids were sharply reduced from 20.5 ibs./IOOO gallons to 3.8 lbs./lOOO gallons. As foT the underlineT, a 1.4% asbestos addition meant a reduction in white-water solids from 17.7 Ibs./IOO0 gallons to 4.9 lbs./lOOO gallons. Clay addition was then cut from 3.8% to 2.5%', further reducing white- water solids to 4.1 lbs./lOOO gallons. Besides obtain ing an improvement in pigment retention, mill per sonnel reported better smoothness with asbestos pres ent in the liner -- an improvement that could lead to better printability. STUFF BOX HEAD BOX COUCH TRAY WATER Figure 5. Paper formed during this production run con tained 3% high-purity asbestos and maintained its ash content despite a reduction in TiO> and clay additions. i UCC 014814 reduces furnish costs LOW-COST WET-END ADDITIVE Asbestos "T" is a special combination of asbestos and Ti02. The product gives unusually high reten tion--not only of its own components but also of separately added Ti02 and fillers. Thus, 1 lb. of asbestos "T" can often replace 1 lb. of TiOz with out sacrificing opacity or brightness. Since asbes tos "T" costs about 60 per cent as much as Ti02, substantial savings can be made. IMPROVED RETENTION OF FURNISH Positively charged asbestos "T" strongly attracts negatively charged pigments and fillers. A typical mill improved overall retention of separately add ed Ti02 from 76 to 84%. Retention of asbestos "T" was highest of all fillers. EFFECTIVE T0, EXTENDER Asbestos "T" improves opacity by optimizing the light-scattering efficiency of Ti02. Thus, higher opacity can be obtained at lower Ti02 levels, re ducing Ti02 costs. A typical mill reduced the Ti02 content of its sheet from 8.7 to 7.3% without any loss of opacity. BETTER SAVEALL A. ,-70^ EFFICIENCY A 0 / b 4 d With asbestos "T" in the papermaking system, mills have improved their recoveries of Ti02 and other solids in the saveall. Improvements have been made in flotation, filtration, and sedimenta tion savealls. One mill reduced losses of solids in the saveall effluent by 68%. By discharging a clearer effluent, it also reduced river pollution. UNION CARBIDE CORPORATION MINING AND METALS DIVISION 270 Park Avenue. New York, N. Y. .......................................... 212-LL1-4420 1371 Peachtree St., N.E., Atlanta, Ga.................................................. 404-876-3331 6855 W. 65th St., Chicago, III................................................................ 312-581-5000 22 Battery St., San Francisco. Cal........................................................ 415-982-1360 F-66-080 UCC 014815 ASBESTOS Lithographed in U.S.A.