COMPARISON .TESTING MONITORING FOR AIRBORNE ASBESTOS FIBERS: SHEET VINYL FLOOR COVERING WET VERSUS DRY SCRAPING
yd
PLAINTIFF'S EXHIBIT CON-26
Final Report November 1970
By: Richard Walcott, Industrial Hygienist Jamas Warrick. Industrial Hypianist
I
\
Praparad for: Rasiliant Floor Covering institute 103018th St. N.W.
Suita aeo
Washington, O.C. 20008
SRI Project 7988
SRI International
1911 N. Kent Street Arlington, Virginia 22209
V
SRI International
COMPARISON TESTING MONITORING FOR AIRBORNE ASBESTOS FIBERS: SHEET VINYL FLOOR COVERING, WET VERSUS DRY SCRAPING
Final Report November 1979
By: Richard Walcott, Industrial Hygianin Jamas Warrick. Industrial Hygianin
Prepared for: Resilient Floor Covering Institute 1030 15th St. NW. Suita 360 Washington, D.C. 20005
SRI Project 7988
Sherry J. Hanen, Associate Director Canter for Occupational and Environmental Safety and Health
*
SRI INTERNATIONAL
SRI International Is a problem-solving organization that provides consulting and research under contract for clients In business and government throughout the world.
Since SRI was founded In 194$, the problems confronting It's clients have so Increased In complexity that few of them can be solved within the confines of a single discipline. The organization Is uniquely qualified to deal with such Intricate problems. Professionals representing more than 100 disciplines comprise nearly two-thirds of the 3,000 staff members.
SRI performs consulting and research for the public sector In such areas as urban management; health, education, and welfare; environmental management, and national security. In addition to broad-ranging activities for the U.S. and other national governments. SRI serves city, state, and county goverments In the U.S., and also their International equivalents. One of the most attractive aspects of life at SRI for the staff Is the opportunity to share In Important work In the public Interest.
For private commercial and Industrial clients, SRI engages In management consulting and corporate strategy determination; technoeconomlc, market, and operational studies; new product, process, and equipment development; and the provision of Information services. A significant percentage of SRI's professional staff have had a number of years of major responsibility In business prior to joining SRI.
SRI Is an Independent, nonprofit corporation, using revenues In excess of operating costs to purchase advanced scientific equipment and to enhance Its ability to continue to provide the highest quality consulting and research for its clients. SRI International has no shareholders and no endowment.
SRI's annual revenues for consulting and research contracts exceed $125 million.
A
SRI's headquarters are on a 70-acre site In Merit* Park, California, a suburban community about 20 miles south of the. San Francisco International Airport and a few miles from the campus of Stanford University. Other offices and laboratories are located In major centers In North America, Europe, East Asia, and the Middle East.
**
STATEMENT OF OBJECTIVE The principal objective of this study ms to monitor for airborne asbestos fibers. If any, that were generated during the complete removal of sheet vinyl floor covering when different methods of removal (Met versus dry scraping) Mere th used. The effect of using different length handles .3? on the scraping Instrument Mas also measured.
i
i
c
t
TABLE OF CONTENTS
I. II. III. IV. V. VI. VIII.
Page Introduction, Sheet Vinyl Floor Covering ................. .... 1
Test Site Location ..... ........................................................... 2
Methodology ............................................................................................. 4
Summary of Results....................................................................... .... . 5
Conclusions.........................
6
Complete Removal ..................................................................................... 7
Attachments:
A. RFCI Work Practices
B. NIOSH Analytical Method
C. Representative Ambient Air Asbestos Concentrations In Cities
t* Copyright 1979 by Resilient Floor Covering Institute
I
**
I. INTRODUCTION
Sheet vinyl floor coverings are widely used in many residential, institutional, and commercial locations. Asbestos Is used as a constituent in the felt backing of many sheet vinyl floor coverings, but there Is no asbestos In the various types of top or wear layers. Attention has recently been centered on the health effects resulting from certain exposures to asbestos. SRI was retained to measure whether or not airborne asbestos fibers were produced under certain conditions of sheet vinyl floor covering removal. RFCI recommends that the felt backing of the sheet vinyl be removed from the subflooring by a method known as "wet scraping" (See Attactaaent "A"). Vet scraping Is essentially a wetting of the felt remaining after the wear layer has been removed and a careful scraping of the moistened felt by a suitable Instrument (wide-bladed putty knife). In the past, dry scraping, that is the scraping of the felt without prior wetting, has been done. In this test both methods were used pnd the asbestos fibers collected and counted. RFCI Recommended Work Practices strongly advise against sanding an existing floor or sweeping, dry-scraping or sanding residual felt.
I
II. TEST SITE LOCATION
The site for these evaluations was a six-year-old home located In a suburban Maryland community. The attic Insulation material In this home was, according to the occupant, a pink fiber-glass material. This could not be confirmed since access to the attic was not feasible. The heating system In this house was forced-air ventilation, and the air was filtered by the furnace unit. This operation was performed In the kitchen of the home. The total floor surface area was approximately 350 square feet. The tests were done In the Spring (March 15 and 16) of 1979. A diagram of the test site Is Included as Figure 1, page 3.
A
Refrigerator end Cabinet* -- To Dining Room
Dry Scrape Section
To Family Room . 1w
Electric Range
Sink and Dith Washer
Wt Scrape Section'
Figure 1 SITE PLAN
3
III. METHODOLOGY
1. Complete Removal
The operations were not done according to RFCI Recommended Work Practices (see Attachment "A") In that dry scraping was also done.
2. Determination of Airborne Asbestos Fibers
The NIOSH method for determining asbestos fibers In the air was employed (See Attachment "B", NIOSH Method No. P4CAM 239, "Asbestos Fibers In Air*).
IV. SUMMARY OF RESULTS
The following Table lists the TWA concentrations of airborne asbestos fibers measured at the test site for the specified operations. TWA concentrations are stated assuming a full-day exposure to the conditions that existed during the test period.
MOTE:
The OSHA Standard for a safe workplace allows a concentration of 2 fibers per cc of air on an 8-hour time-weighted average (TWA).
Operation
Wear Layer Removal Wet Scrape Ory Scrape Dry Scrape
Table No. 1
8 Hr. TWA (Asbestos Flbers/cc) Mechanic 1 Mechanic 2
0.1637
0.0844
0.4093
HA
2.0248
1.1207
0.8279
1.0583
** V. CONCLUSIONS Deviation from the recommended RFCI work practice (wet scraping) resulted In a two to fivefold Increase In asbestos exposure. These data reinforce the need to follow the recommended practice of wetting the felt backing prior to scraping. Dry scraping should never be done.
i* 6
Discussion
VI. COMPLETE REMOVAL
An existing sheet vinyl floor covering was removed by using both wet and dry scraping. First the wear layer was removed according to standard practice and part of the floor was dry scraped and the rest was wet scraped. A water-detergent solution was used for wetting the felt. Two different length handles were also used In the scraping: Mechanic 1 used a regular handle on a stiff bladed putty knife while Mechanic 2 used a handle of 3-4 feet.
Sampling Procedure:
The sampling protocol was designed to:
1. Evaluate the background asbestos levels In the home and outside ambient air. This was accomplished using area samples taken several days before the test sampling.
2. Determine any Increase above background concentrations of . asbestos fibers. Personal samples were taken for each worker during the operation. Separate filters were used for each phase of the operation. Dry scraping was done In two phases so there are two samples .for each worker for dry scraping.
See Figure 1, page 3t for a diagram of the sampllngarea. .
Sampling Results;
The results of the Individual-filter analyses are shown below In Table 2
Table 2
I*
Description
Background Samples Outside Outside Kitchen
Wear Layer Removal Mechanic 1 Mechanic 2
Wet Scrape Mechanic 1
Dry Scrape Mechanic 1 Mechanic 1 Mechanic 2 Mechanic 2
Filter Air Vol. Time Fibers/ Total
Asbestos** 8-Hr.
No. (liters) (min) SShJStL Flbers/cc Flbers/cc TWA
AB-9 C-1089 XX009
760 766 748
380 383 374
00 00 00
0
0 0
AB-12 AB-2
AB-14
ISO 140
110
75
39
0.218
0.1637
0.1637
70
14
0.0844 0.0844
0.0844
i 55 96 0.4837 0.4093 * 0.4093
AB-13 AB-11 AB-10 AB-15
126 80
126 90
63 327 40 96 63 191 45 121
2.168 1.0035 1.2669 1.1259
2.0248 0.8279 1.1207 1.0583
2.0248 0.8279 1.1207 1.0583
Fibers/sq mm of total filter surface area. Analyst estimated that about 90% of the fibers were asbestos.
8
I t
t
Evaluation
i The background samples obtained prior to and on the day of the test showed no asbestos fibers. Asbestos fiber concentrations found during the wear-layer removal were very low (0.1637 and 0.0844 flbers/cc). As sometimes happens when the wear layer Is removed, a good deal of the felt was separated
i from the subfloor and removed with the wear layer. The strips of wear layer were rolled and placed In trash bags for disposal. The higher concentration was from the worker who bagged the material.
' Wet scraping, which took 55 minutes, resulted In a concentration of 0.4093 flbers/cc. Dry scraping samples, however, showed concentrations ranging from 0.8279 to 2.0248 flbers/cc. Dry scraping was done with two different-length handles. The results from the worker using the longer handle (1.1207 and 1.0583) are, on the average, a good deal lower than the results from the worker using the short handle (2.0248 and 0.8279). The longer handle does provide, as would be expected, some protection from the asbestos concentration.
Conclusion
The contrast between the asbestos fiber concentration values found ' ' following wet versus dry scraping clearly Indicates the need and desirability
of following the recommended RFC! work practice of wet scraping. The comparison between long and short handles, while not showing as great a difference as that between wet and dry scraping, shows that longer handles are also more desirable If they can be practically used.
9
c
t* S-
ATTACHMENT A RECOWENDED WORK PRACTICES FOR RESILIENT FLOOR COVERINGS
i* REVISED 10/31/79
Pre-Publication Copt RECOMMENDED
WORK PRACTICES FOR
RESILIENT FLOOR COVERINGS
c
CONTENTS
Introduction ............................................................................
2
Why Asbestos in Resilient Floor Coverings? ................................................................... 2
What About Asbestos? ................................................ Recommended Work Practices
2
*i.
Preparation of Floors, General Information ................................................................... 3
Sheet Vinyl Floor Covering
General Information and Preparation ........................................................................... 4
Complete Removal* (Jo-Adhered .......................................................................................... S
Partial Removal, Adhered............. ....................................................................................... 5
Complete Removal, Adhered.............................
8
Resilient Tile Floor Covering
General Information..............................................................................
11
Complete Removal of Existing Resilient Tile Floor Covering.................. 11
Copyright^ 1979 by Resilient Floor Covering Institute Printed in USA
IMPORTANT INFORMATION FOR INSTALLERS OF RESILIENT FLOOR COVERINGS
Introduction The member companies of the RESILIENT FLOOR COVERING INSTITUTE are
manufacturers of the following forms of resilient floor coverings which may contain some asbestos:
1. Sheet Vinyl 2. Vinyl Asbestos Tile 3. Asphalt Tile Why Asbestos In Resilient Floor Coverings? Asbestos fibers have been used In the manufacture of resilient floor covering products for more than 50 years. Asbestos fibers are used to provide
durability to tile products. In addition, asbestos fibers In sheet vinyl backings permit these products to be Installed on all grade levels. The presence of "locked-ln" asbestos fibers In resilient floor coverings provide the versatility and econoiqy for which they have been noted throughout the years. What about Asbestos?
It has been determined that Inhalation of free airborne asbestos fibers nay be injurious to health. However, the asbestos fibers contained In the above types of resilient floor coverings are not free, but firmly encapsulated or locked1n the product during the manufacturing process. Asbestos contained therein will not become airborne during the lifetime of the product when these products are used and maintained as recooinended by the manufacturer*
See "Monitoring for Airborne Asbestos Fibers: Vinyl Asbestos Floor Tile" and "Monitoring for Airborne Asbestos Fibers: Sheet Vinyl Floor Covering," report prepared by SRI International, 1978-79. (Available on request from the Resilient Floor Covering Institute, 1030 15th Street, NW - Suite 350, Washington, DC 20005).
2
.0
It Is essential that certain precautions be observed* however, when Install* ing a resilient floor covering or when preparing or removing an existing resilient floor covering. It Is the purpose of this Uork Practices Manual to provide those precautionary steps necessary to assure the safest way to accomplish the work Involved.
PREPARATION OF FLOORS WITH EXISTING RESILIENT FLOOR c5vRIh6S TO RECEIVE NEW RESILIENT FLOOft 'COVERINGS
Follow the Installation Instructions published by the manufacturer of the new floor covering when a new resilient sheet or tile floor covering is to b| installed on a surface presently covered with a resilient floor covering. These instructions will tell you what must be done to the existing surface before the new resilient floor covering can be Installed.
Of the four general procedures listed below, Items 1 and 2 are covered by manufacturers' Instructions; Item 3 and 4 are covered specifically In this Work Practices Manual*:
Resilient Floor Covering Installed Over ............. 1. The Existing Surface. Follow the manufacturer's instructions for
removing wee, filling in low spots, etc. Use wet scrubbing. Never sand an existing resilient floor covering. 2. New Under! aymnt. Nall panels on top. of the existing surface (wood subfloors only) and apply new floor covering directly over this. Follow the manufacturer's Instructions.
*In case of minor variations, the manufacturer's Instructions should be followed.
(SKETCHES - one for item 1 & 2 above)
3
I
3. Partially Removed Existing Adhered Sfieet Vinyl Flooring Covering. See
Instructions below under heading "Partial Removal of Existing Adhered
Sheet Vinyl Floor Covering," page 6.
4. Completely Removed Existing Resilient Floor Covering
(a) Sheet Vinyl -- See instructions below: .
1. "Complete Removal of an Unadhered (Loose-Lay) or Peripherally
Adhered Sheet Vlpyl Floor Covering," page 5.
2. "Complete Removal of an Existing Adhered Sheet Vinyl Floor
Covering," page 8.
(b) Tile -- See Instructions under heading "Complete Removal of an Existing Resilient Tile Floor Covering," page 11.
f
SHEET VINYL FLOOR COVERING
Preparation of Floors with Existing Sheet Vinyl Floor Covering To Receive A :iaw jjy
Resilient Floor Covering.
Sheet vinyl floor covering Is installed In several ways:
1. Un-adhered or Loose-Lay. 2. Adhered or Cemented.. 3. Peripherally adhered.
Some resilient floor covering can be installed over existing resilient sheet
(
vinyl floor covering under certain conditions. 8e sure to fOllov: the floor covering
manufacturer's Instructions, regarding the conditions and floor preparation
required. {
If partial or complete removal of the existing sheet Vinyl floor covering is
required, the following instructions are to be followed:
SUPPLIES AND TOOLS
1. 8road, stlff-bladed wall scraper, or floor scraper.
2. Utility or hook knife.
3. Tank type vacuum cleaner with disposable dust bag and metal floor > tool .(no brush).
4'
c
4. large size heavy duty trash bags with ties, tapes, or string to tie shut, and tags for labeling. *
c 5. Hand sprayer or-sprinkling can.
6. Liquid dishwashing detergent or 1 /quid wallpaper remover mixed with
water to make a dilute solution (1 oz. liquid In one gallon of water),
L SPECIAL PRECAUTIONS
1. Never sweep.
2. Never dry scrape adhered areas of floor covering.
3. Never sand an existing floor covering.
4. Never sand or dry scraoe residual felt.
Complete Removal of an Un-adhered (Loose-Lay) or Peripherally Adhered Sheet Vinyl
Floor Covering.
,
a. Remove any binding strips or other restrictive moldings from doorways,
walls, etc.
IB b. Cut a strip the length of the floor and about 18" wide along one wall.
.,?.V
Remove this strip, gently turn It over and roll face out into a tight
roll. Tie or tape securely so It will not unroll. Place it in a heavy
duty plastic bag, big enough to accomodate several rolls, for disposition.
c. Clean the exposed floor with a vacuum cleaner positioned so that exhaust
air does not blow over the unclean area. DO NOT SHEEP.
d. Repeat the above, cutting, removing, rolling, disposing of one.strip at
a time and cleaning the newly exposed area Immediately until the whole
floor covering has been removed and thr whole floor vacuumed clean. ( e. If seams or door openings have been adhered with double faced tape,
remove the tape and place In the plastic trash bag.
(SKETCHES-(l) after Item 6, depicting all supplies. (2) Under "b", roll face out in a tight roll. (3) Under HcM, show vacuum cleaner exhaust and (4) undarHSpecial Precautions," illustrate each Iteafl.
i 5
c
f. If ar\y floor covering areas have been adhered with adhesive and remain
stuck to the floor, they should be removed by the wet scraping method
. explained on page 7-f.
DO NOT DRY SCRAPE OR SAND.
( g. Carefully remove the dust bag from the cleaner and place it In the trash bag.
h. Close and seal the trash bags tightly for disposal. Identify contents
with a label stating - "Caution - Contains Asbestos - Dispose in an
approved land fill only."
1. Wash hands Immediately before eating and at the end of the work day.
j. Install the new resilient floor covering according to the manufacturer's
instructions.
\
Partial Removal of Existing Adhered Sheet Vinyl Floor Covering.
`tost felt backed sheet floor coverings can be separated In the backing or
felt layer. The felt left on the floor presents a smooth surface on which some
new sheet floor coverings can be directly Installed. Be sure to follow the man
ufacturer's instructions. Use the following procedure to partially remove
the existing adhered floor covering.
REMINDER? NEVER SAND AN EXISTING FLOOR CQVERIN6
a. Remove any binding strips or other restrictive moldings from doorways
walls* etc.
b. flake a series of parallel cuts 4 to 8 inches apart' through the top
layers and about halfway through the backing, parallel to the wall.
c. Start at the end of the room farthest from the entrance door and pry
up the corner of a strip, separating the backing layer. Pull the top
layer back upon itself slowly and evenly at the angle that permits the
best separation, and half the backing and the top layers will pull free.
(SKETCHES: (1) Under "f", show wet scraping method. (2) Under "h", show bag l sealing. (3) Uoder "c", show top layer pulled back.)
6
c
After it Is removed* roll up the strip face out into a tight roll. Tie or tape securely and place in the heavy duty trash bag for
disposal.
Each succeeding strip should be removed in the above manner. Avoid
walking on the exposed felt as much as possible. Boll up each strip
as it is is removed and place it In thp trash bag. Close full bags
tightly and seal securely for disposal. Identify with a label stating
"Caution - contains asbestos. Olspose in an approved land fill only."
Occasionally, parts of the top layers will stick to the backing. This
can often be eliminated by peeling from the opposite direction. The
stiff bladed scraper will help in stubborn areas.
'i
Any high spots of felt on the floor can be levelled by wet scraping.
REMINDER: NEVER SAND OR DRY SCRAPE RESIDUAL PELT
Wet scraping is done as follows:
1. Pour the detergent solution into the sprayer or sprinkling can. f 2. Thoroughly wet the high felt spot with this solution. Wait a few
minutes to allow the solution to soak into the felt.
3. Use the stiff bladed scraper to remove the excess felt. If felt 1 dries out* or dry felt is exposed during scraping, re-wet with
more solution.
. Pick up the larger pieces by hand and. place in the trash bag
immediately. Wash your hands.
fion-adhered felt left on the floor can be cut open and re-adhered
to the floor with adhesive.
If small areas of backing pull free from the floor, the depression
should be filled with latex patching compound, as recommended by the
floor covering manufacturer.
(t) Top of gage, show tight roll tied. (2) Under "f-3, show wetted scraped and (3) Under "h", show filling of depression).
c
1. Clean the floor with the vacuum cleaner using the metal floor tool.
DO NOT SWEEP VHTH A BROOM.
Position the vacuum cleaner so that discharge air does not blow on
the felt. Carefully remove the dust bag from the cleaner Immediately
and place In the plastic trash bag.
j. Close and seal trash bags tightly for disposal.- identify contents
with a label: "Caution -- contains asbestos. Dispose in an approved
land fill only."
k. Do not walk over the felt unnecessarily, as this might scuff the felt and raise dust.
l. Install the new resilient floor covering Immediately, following the %
manufacturer's instructions.
;
Complete Removal of an Existing Adhered Sheet Vinyl Floor Covering.
If complete removal is required, follow these instructions:
REMINDER: NEVER SAND AH EXISTING FLOOR COVERING '
a. Remove any binding strips or other restrictive moldings from doer-ways, walls, etc.
b. Make a series of parallel cuts 4 to 8 inches apart and almost through the backing, parallel to a wall.
c. Start at the end of the room farthest from the entrance door, and pry up the corner of the first strip, separating the backing layer. Pull the top layer back upon Itself slowly and evenly at an angle that permits the best separation and most of the backing and top layers will pull free.
Remove this strip, gently turn it over and roll face out into a tight roll. Tie or tape securely and place in the heavy duty trash bag for disposal. (SKETCHES: Under "c", show separation of backing & top layers pulling free.).
1
t3
d. Repeat the above on the next two strips but do not remove anymore than *
a total of three strips at this time.
e. Remove the felt remaining on the floor In the stripped area by wet scraping.
REMINDER: NEVER SAND OR DRY SCRAPE RESIDUAL FELT Wet scraping Is done as follows:
1. Pour the detergent solution Into the sprayer or sprinkling can.
2. Thoroughly wet the residual felt with this solution. Halt a few
minutes to allow the solution to soak Into the felt.
3. Stand on the remaining floor covering (not the felt) and use the
stiff bladed scraper to scrape up the wet felt.
^
REMINDER: DO NOT SCRAPE DRY FELT
\
Re-wet the felt If It dries out or If dry felt Is exposed during scraping. Pick up the scrapings as they are removed from the floor and place in the plastic trash bag. Scrape all_ felt from this floor area before proceeding further.
4. Repeat the above on the next series of strips. Do only one threestrip area at a time. Stand on the remaining floor covering or clean floor (do not stand on the felt)to scrape up the felt.
5. Repeat this operation until the felt has bepn removed from the whole
floor. Close full bags tightly, and seal securely for disposal.
Identify with a label stating "Caution - Contains Asbestos. Dispose In an approved land fill only."
f. Wash your hands Immediately before eating and at the end of the work day. g. When the whole floor has been cleaned free of felt, let it dry and vacuum
up any dirt using the vacuum cleaner with the metal floor tool.
REMIHOER: DO NOT SHEEP.
(SKETCHES: Under *e-3", show standing on floor covering not felt to scrape.)
9
Position the vacuum cleaner so that*the discharge air does not blow on the floor being cleaned. h. Carefully remove the dust bag from the cleaner and glace In the plastic trash bag for later disposal. 1. '..'hen the floor Is dry* It Is ready to have a new resilient floor covering Installed. Follow the floor covering manufacturer's Instructions.
RESILIENT TILE FLOOR COVERING
Preparation of Floors with Existing Resilient Tiles to Receive New Resilient Floor Covering.
Some resilient floor coverings can be installed over existing resilient tile installations. Follow the installation Instructions published by the manufacturer of the new floor covering when a new resilient floor covering is to be installed on a surface presently covered with a resilient floor covering. These Instructions will tell you what must be done to the existing surface before the new resilient floor covering can be Installed.
CAuriON: Never Sand an Existing Tile Installation.
Complete Removal of Existing Resilient Tile Floor Covering.
i
SUPPLIES ANO TOOLS 1. Heavy duty wall scraper with approximately 4" blade and 6" to 8M handle. 2. Hamner 3. Commercial type hand held hot air blower. 4. Heavy duty plastic trash bag(s), ties and labels.
a. Those areas normally exposed to heavy foot traffic patterns usually have tiles adhered the tightest. As a matter of good practice in starting the tile removal* those sections which receive least traffic should be the locations selected for starting the removal of the tile. Since tiles are normally in a 9" X 9" or 12" X 12" dimension* it should be the goal to remove individual tiles as a complete unit.
b. Start the removal by carefully wedging the wall scraper in the seam of two adjoining tiles and gradually forcing the edge of one of the tiles up and away from the floor. Do not break off pieces of the tile but continue to force the balance of the tile up by working the scraper beneath the tile and exerting both a forward pressure and a twisting action on the blade to promote release of the tile from the adhesive and the floor.
c. When the first tile Is removed place It, without breaking it into smaller pieces, in the plastic bag which will be used for disposal.
(SKETCHES: After #4 under Supplies A Tools, show supply Itcms. And under MbM,
sOow how tile is to be forced up.)
11
c
d. With the removal of the first tile, accessibility of other tiles Is c Improved. Force the wall scraper under the exposed edge of another
tile and continue to exert a prying twisting force to the scraper as
It Is moved under the tile until the tile releases from the floor.
c
Again, dispose of the tile* and succeeding tiles by placing In the
plastic bag without additional breaking.
e.. Some tiles will release-quite easily while others require varying c
degrees of force. Where the adhesive Is spread heavy or Is quite
hard. It may prove easier to force the scraper through the tightly
adhered areas by striking the scraper handle with a hammer using
<
blows of moderate force while maintaining the scraper at a 25* -30%
angle to the floor.
I
f. If some areas are encountered where even the technique detailed In the
previous paragraph proves to be Inadequate, the removal procedure can be simplified by thoroughly heating the tlle(s) with a hot air blower
until the heat penetrates through the tile and softens the adhesive. MOTE: Handle the hot air blower carefully to avoid personal burns.
g. As small areas of subfloor are cleared of tile the adhesive remaining
on the floor must be scraped up with the 4" hand scraper until only a c thin, smooth film remains. In those areas where deposits are .heavy or
difficult to scrape the removal can be expedited by heating with the hot
air-blower prior to scraping. Oeposlt scrapings In a plastic trash bag. h. Where the existing floor consists of a tile over tile installation it
is recommended that removal be accomplished layer by layer in small areas -Instead of attempting to remove both layers simultaneously. Less tile s' breakage Is encountered with single tsySFremoval.
V
(SKETCHES: Under V, "f*. "g" and "h". use appropriate Illustrations.).
C
12
.p 1. As Indicated In previous paragraphs, tiles should be placed Immediately
In a plastic trash bag. Do not attempt to break tiles after they are In the bag. j. When all tiles have been removed from the floor and placed In plastic bags; seal the bags by any convenient means and mark: "Caution - Contains Asbestos - Dispose In an approved land fill only."
WARNING DO NOT SAND EXISTING RESILIENT FLOORING, BACKING, OR LINING FELT. THESE PRODUCTS MAY CONTAIN ASBESTOS FIBERS THAT ARE NOT . READILY IDENTIFIABLE, SANOING OF ASBESTOS CONTAINING MATERIAL CAN PLACE FINE PARTICLES OF ASBESTOS IN THE AIR. THESE ASBESTOS PARTICLES IF INHALED MAY CAUSE SERIOUS . BODILY HARM.
i* 13
MANUFACTURER MEMBERS RESILIENT FLOOR COVERING INSTITUTE
AMTICO FLOORING DIVISION AMERICAN BILTRITE, INC. TRENTON, NO 00607
AZROCK FLOOR PRODUCTS DIVISION UVALOE ROCK ASPHALT COMPANY SAN ANTONIO* TX 78233
CQNGOLEUM CORPORATION RESILIENT FLOORING DIVISION KEARNY, NJ 07032
FLINTKOTE COMPANY, THE FLOORING 01VISION DALLAS, TX 75221
GAF CORPORATION CONSUMER PRODUCTS GROUP NEW YORK, NY 10020
KENTILE FLOORS, INC. BROOKLYN, NY 11215
MANNINGTOH MILLS, INC. SALEM, NJ 08079
NATIONAL FLOOR PRODUCTS CO., INC FLORENCE, AL 35630
t
( (.
ATTACHMENT B ASBESTOS FIBERS IN AIR
ASBESTOS FIBERS IN AIR National Institute for Occupational Safety and Health
Analytical Method
Analyte Matrix: Procedure:
Date Issued: Data Revised:
Asbestos fibers
Air Filter collection, microscopic count 3/30/77
Method N
P&CAM239
Range:
0.1-60 fibers/cm*
Precision (CV*): 0.24 to 0
Classification: D (Operational)
1. 'Principle of the Method
1.1 This method describes the equipment end procedures for collecting, mounting, end counting xsbestos fibers on cellulose ester membrane filters in the evaluation of personal samples of airborne asbestos fibers. The purpose of the method is to determine an employee's index of
exposure to airborne asbestos fibers. The method Is primarily e personal monitoring tech nique, but can be used for area monitoring.
| f
1.2 The sample it collected by drawing air through a membrane filter by means of a battery powered personal sampling pump. The filter is transformed from an opaque solid membrane to a transparent optically homogeneous get The fibers are sized and counted using a phasecontrast microscope at 400-450X magnification.
1.3 Definitions. Asbestos fiber, for counting purposes, means a particulate which has a physical
dimension longer than 5 micrometers and with a length to diameter ratio of 3 to 1 or greater. i Asbestos includes chrysotile, cummingtonite-grunerite (amosite), crocidolite, fibrous tremo-
lite, fibrous anthophyllite, and fibrous actinolit*.
1.4 Any laboratory attempting to use this procedure should have at least one counter attend a
training course conducted by an experienced, proficient laboratory. Novice, untutored counters, using only published instructions, can easily obtain counts of half those performed by experi
c enced, proficient counters. Large differences between laboratories can be caused by: 1) dif
ferences in technique and observing ability among counters and 2) small, but significant, dif
ferences between microscopes meeting the basic specifications of Section 6.2. The following procedures are recommended:
1.4.1 All mkroscopists who perform asbestos counting should meet together for an "asbestos
c counting workshop" it least quarterly.' This Is best accomplished with counters from several laboratories using their own microscopes.
1.4.2 Each microscopist should count the same series of slides and with the results being compared.
1.4.3 Differences between counters should be resolved with stde-by-sidt counting of the
c fields by the different counters. 1.4.4 Individuals who are found to be persistent outliers over several sessions should be encouraged to seek other tasks in their respective laboratories.
C 239-1
t
I'
2. Rang* Seaslttvlfy
2.1 The stable range b primarily a function of ample volume, microscope count field area, and
background airborne particulates. The influence of these variables is discussed in 1.1.3. For
a microscope count field area of 0.003 mm* (see Figure 1) and a pump flow rate of 1.7 1pm,
1 the optimal fiber densities would be produced over the range of 0.4 fiber/cm* (8-hour sent. pie) to about 60 fibcts/cm* (IS-minute sample). For a field area of 0.006 mm* (sec Figure 2) and a pump flow rate of 1.7 1pm, the optimal range is 0.2 fiber/cm* (8-hour sample) to about 30 fibers/cm* (IS-minute sample). In each case, the optimal detection limits are in versely proportional to pump flow rate. The upper detection limit can be extended by using sample times less than IS minutes or using lower flow rates. The lower detection limit can be extended by increasing the flow rale up to about 2.51pm. Filter surface fiber densities less than optimal (less than about 0.S to 1.0 fiber per count field) are still adequate, but will lead to decreased precision for the method (in creased coefficient of variation, see Section 4). The minimum total fiber count in 100 fields considered adequate for reliable quantitation is 10 fibers. Thus, the lower limit of reliable quantitation b 0.1 fiber/cm* (100,000 fibers/
m*). For this level, a flow rate of about 2.S tpm is recommended. For a field area of
0.003 mm*, the minimum sample time would be-about 2 hours. For a field area of 0.006 mm*, the minimum sample time would be about 1 hour.
2.2 This method considers only fibers with a length to diameter ratio of 3 to 1 or greater and a
length greater than 5 micrometers.
i
3. Interferences
i
In an atmosphere known to contain asbestos, all particulates with a length to diameter ratio o1 3 to 1 or greater, and a length greater than S micrometers should, in the absence of other information,
, ii be considered to be asbestos fibers and counted as such.
4. Precision and Accuracy
4.1 In the past decade, there have appeared a number of articles examining sources of variation in the asbestos sampling and counting procedure. These include: Lynch et a!. (11.1), Weidner and Ayer (11.2), Conway and Holland (11.3), Lcidel and Busch (11.4), Beckett and Attfield (Hi), and Rajhans and Bragg (11.6). The sources of variation will be discussed by stages in the membrane filter evaluation procedure.
4.2 Sources of Variation In the Sampling Process. These Include variations in pump flow rate, proximity of the filter to the employee's body, and filter location (left to right) in the em ployee's breathing zone.
42.1
Section 9.1 requires that the personal sampling pump be calibrated with sufficient accuracy such that the 95% confidence limits on the flow rate are db 10%. This is
equivalent to a coefficient of variation (CV) of about 5%. However, this CV makes
a negligible contribution to the total CV for the method due to the relatively large CV
of the counting procedure.
I 4.2.2 Conway and Holland (11.3) concluded that positioning of the filter eassette on the wearer (regarding the angular portions of the filter and their proximity to the wearer) is not a significant factor in determining the fiber distribution on filters.
.i 4.2.3 Weidncr and Ayer (11.2) concluded that there is no appreciable difference between samples collected on either the right or left sides of a breathing zone or between samples collected. sidc-by-sidc, especially for samples with concentrations less than 2.5 ffbers/cm*.
239-2
*
4.3 Sources of Variation In tfi Counting htcdwi
4.3.1
Random variations exist in the fiber distribution on a filter tvedg* (intra-wedg* variability). The Industrial hyfieae literature has seen considerable debate in the last 20 years concerning whether or not the distribution of mineral dust or asbestos fiber* on a fitter surface is adequately*described by a Poisson distribution probability density
function. .Leidel and Busch (11.4) found excellent agreement between empirical error variance and theoretical variance calculated from the assumption of Poisson distributed true counts. They concluded that there was not excessive variation among count fields for a filter wedge and that clumping of fibers (non-random coalescence) did not occur.
4.3.2 Variations exist in the fiber distribution on the total filter surface (inter-wedgt vari ability) due to the random or non-random distribution of fibers across the total sur face of the filter. This type of variation is easily confused with intra-wedge variations. The count procedure does not' require counting of multiple sectors of the filter. There may be significant differences between average counts for different wedges, or the fiber distribution variations for the total fitter surface may be greater than the variations of the Poisson distribution. If either of these occur experimentally, one must use the
* experimental variations to estimate the minimum precision of the count procedure. The minimum precision is governed by the variations of the fiber distribution on the total surface of the filter. Conway and Holland (11.3) concluded the distribution of fibers on filters is not uni form and the distribution of fiber counts is more disperse than Poisson. For their
. filters which had significant variations in fiber concentrations between sectors (as much as 30-60% of the total fitter mean), they described the following relation for the standard deviation of the total number of fibers counted on a wedge (N)
empirical s(N) - 1.6 (N)1'*
where N is about 100. The Poisson standard deviation would be:
Poisson # (N) (N)'s
Rajhans and Bragg (11.6) in Series I of their study found significant variation between filter segments and rejected the Poisson distribution for the total filter surface. How ever, in Series II of their study, utilizing various experimental modifications, they found no significant variation between fitter segments and no reason to reject the assumption of Poisson distributed fiber counts.
4.3.3
Systematic variations due to differences between microscopes were studied by Leidel and Busch (11.4). In their study using five different brands of microscopes, they found no significant differences among four, but the fifth gave counts approximately 43% higher on the avenge than the other four.
4.3.4 Variations doc to differences between counters should be examined at three levels: experienced counters occasionally counting, experienced counters routinely counting, and inexperienced (new or untutored) count**. Leidel and Busch (M.4) studied five experienced counters, with one counting only, occasionally. There were no significant differences among three of the counters, but a fourth was 16% lower than the first three. The fifth, who occasionally counted, averaged 27% higher than the first three. Conway and Holland (11.3) studied three experienced counters and three inexperienced counters. They found statistically significant differences between the means of both the experienced and inexperienced counters that typically were in the range plus or minus 5 to 13%. They concluded that experience as a fiber counter is not a significant parameter affecting intcrcountcr variations.
239-3
c
Rajhans and Brats (l1.6) found no significant differences among means of five experi enced counters la Series I of their study. But in their carefully controlled Series II, an analysis of variance showed significant variations between counters that were plus or minus 1 to 15%.
4.3.5 Variations between laboratories are most likely due to systematic biases and arc not a significant additional source of random variations. Any additional variations are most likely due to differences in counting technique. Beckett and Attfield {113) ob served that standard counters improved greatly after personal instruction; also new counters, after instruction, tended to overcompensate and get exceedingly high counts.
t Additionally, they found that counts from an experienced laboratory that had not had contact with other laboratories performing the same analysis were as far from the standard values as were the counts by new counters.
4.4 Sources of variations between samples taken at different times on one employee during one work shift can affect the exposure estimate for that employee. These arc primarily due to e) differences in exposure concentrations during the day, b) differences in location of the employee within the plant, and c) differences In work operation performed by the employee during the day. These sources of variation can be controlled by proper choice of sampling strategy. Refer to Leidei and Busch (11.7) and Leidel, Busch, and Lynch (11.8) for an extended discussion of sampling strategies. Interday temporal variations can affect the ex posure estimates obtained on different days. Refer to Leidel, Busch, and Crouse (11.9) for a discussion of this type of variation.
4.5 Until recently, the total coefficient of variation (CVT) for the sampling and counting proce dure was best estimated from the work of Conway and Holland (11.3). The conclusions of their study included:
4.5.1 The precision of their procedure for filters not containing an abundance of fine fibers can be estimated by a coefficient of variation of 16.2%. This value includes variation among counters and observed interaction effects.
' 4.5.2 The accuracy of the procedure for similar filters may be estimated for a 100-fiber count by a coefficient of variation of 21.4%. This assumes that the contribution
of the overall variance from the nonuniform fiber distribution is additive.
4.5.3 A high percentage of very fine fibers on the filter can significandy.affect the standard v. deviation and confidence limits for counts by different counters. After combining
variations in fiber concentrations over the entire filter with those for different counters, it was concluded:
a. For filters with a low concentration of fine fibers, the coefficient of variation is estimated at 21% and the 95% confidence interval is :fc 43%.
t. b. For filters with a high concentration of fine fibers, the coefficient of variation is estimated at 23% and the 95% confidence interval is :fc 50%.
Lynch. Kroooveter, and Leidel (1 l.I) have also reported on variations of the method.
Their intralaboratory study utilized the data from a large number of dust counts made
by different methods by/xpericnecd counters over a periodof years in an epidemiologic
study of tha asbestos products industry. They .concluded that the standard deviation of
C counts of fibers longer than 5 micrometers on membrane filters could be estimated
from the relation (N)*u>>. Thus for counts of about 100 fibers, the coefficient of
variation could be estimated at about 15.2% and the 95% confidence limits at m
30.4%. These values are lower than the values reported by Conway and Holland
(U.3).
---------r '
c. Recently, the Johns-Manville Corporation conducted an in-housc investigation of the asbestos count method (11.10). The study data contained tout fiber counts for over
239-4
C
!
*
*
!'
t
<i1t N
<i <;
t :!
100 (then with each filter counted by two to five couplers. From the Johns-Manville data, NIOSH calculated over 100 estimates of the count CV for the method (11.11). The NIOSH CV estimates included random intrafilter variations and intercounter variations, but did not include random pump flow rate variations. It was found that the eount coefficient of variation (all random variations except for pump variations)
1 was a function of the total fiber count. NIOSH then included a CV of 0.05 for ran* dom pump variations (see Section 9.1) in the CV*cstimator equation.to obtain a
CVt-estimator. The CVrcstimator line is plotted on Figure 3 for total fiber counts in the range 10 to 100 fibers. Or the following equation can be used:
CVT (nti!ogu(-0.213 - 0.203 (1ogtFB)) + 0.00251*
where FB is total fiber eount as discussed in Section 10. Figure 3 demonstrates that for a total fiber count of 100, tbe best CVr is attainable with the appropriate sampling times given in 8.1.3 tod the count rules in 8.3.9. When makinf decisions regarding compliance with the OSHA asbestos exposure standards in 29 CFR 1910.1001, the statistical procedures given in Leidel ct al. (11.11) should be followed. The procedures are based on statistical theory and assumptions given in References 11.12,11.13. Because of the possibility of systematic biases due to differences between microscopes, counters, and laboratories as discussed above, it is strongly recommended that any laboratory counting asbestos should participate in an intcrlaboratory quality control program that includes the counting of standard reference filters. These standard filters are available from NIOSH through the Proficiency Analytical Testing (PAT) Prt* gram. The PAT Program is used by the American Industrial Hygiene Association (A1HA) as part of its Laboratory Accreditation Program. Each laboratory's quality control program must include protocols for routinely adjusting and calibrating sampling and counting equipment plus training and evaluation programs for counters.'
5. Advantages and Disadvantages of the Method
5.1 The method is intended to give an index of employee exposure to airborne asbestos fibers of specified dimensional characteristics.
5.2 It is not meant to count all asbestos fibers in all size ranges or to differentiate asbestos from other fibrous particulates.
6. Apparatus
6.1 Sampling Equipment
The personal sampling equipment train consists of I) personal sampling pump, 2) tubing, 3) clothing spring clip, 4) tubing-to-field monitor metal adaptor, and 5) field monitor (filter and holder).
6.1.1 Personal Sampling Pump. The pump must be capable of'sampling at 1.0 to 2.5 liters per minute (Ipm) against a flow resistance of 7.5 inches of water (1.4 cm Hg) for 8 continuous hours on a fully, charged;battery.
6.1.2 Tubing. Laboratory tubing such as rubber or plastic with 6-mm bore and about 100 cm length.
6.1.3 Clothing Spring Clip. The clip, attaches the rubber tubing tothc lapel or shirt of the individual being monitored.
6.1.4 Tubing-to-ficld Monitor Adaptor. A short metal adaptor with ridges on one end to grip the inside of the tubing. The other end i designed fur a pressure lit into the field monitor.
6.1.5 Field Monitor (Filter and Holder). Tlie only field monitor currently considered acceptable by NIOSH is manufactured by the Milliporc Corporation. The unit con-
lists of 1) k three scctioo styrene plastic case designated Milliport-Aerosol Monitor Case, 2) 37-mm diameter plain white cellulose ester membrane filter designated Millipore AA (pore size of 0.8 micrometer), 3) a support pad, and 4) two plastic sealing caps. If a large number of samples are to be taken, it may be less expensive to rcusp the plastic cases. ~ Great care must be taken in the cleaning and reassembly process. The outside mating surfaces of the field monitors may be covered with a "shrink-fit** band to provide proper sealing and a writing surface for filter identifica tion.
6.2 Optical Equipment and Microscope Featam
6.2.1 Microscope body with binocular head. 6.2.2 10X Huygenian eyepieces are recommended. Other eyepieces can be substituted if
necessary. Wide field eyepieces can be used; however, wide field eyepieces may yield a count field area less than 0.003 mm* with the Portoo reticle. This ts not always desirable from the standpoint of obtaining optimum sampling times (see Sec tion 8.1.3). If wide field eyepieces are used, it is preferable to use the Patterson % Globe and Circle reticle to obtain a larger count field area. 6.2.3 Koehler illumination (preferably built-in with provisions for adjusting light intensity). 6.2.4 A Porton reticle is recommended. Others such as the Patterson Globe and Circle can be substituted. 6.2.5 Mechanical stage. 6.2.6 Phase-Contrast condenser with a numerical aperture (N.A.) equal to or greater than the N.A. of the objective. 6.2.7 40-4SX phase contrast achromatic objective (N.A. 0.65 to 0.75). 6.2.8 Phase-ring centering telescope or Bertrand lens. 6.2.9 Green or blue filter, if recommended by microscope manufacturer. 6.2.10 Stage micrometer with 0.01 mm subdivisions. 6.2.11 For general guidance on phase contrast microscopy, consult Needham (11.12), Clark (11.15) and McCrone (11.14).
6.3 Filter Mounting Equipment Experience has shown that certain equipment is useful for efficient sample mounting. The following items are recommended for extracting and mount ing a portion of the filter for counting.
6.3.1 Microscope slides. 2.5 by 7.5 cm glass slides are most commonly used. Sample number, data, initials, etc., can be conveniently written on a frosted end slide.-
6.3.2 Cover Slips. Cover slips are a necessary part of the slide mount and optical system. The shape should be appropriate for the size of the fitter wedge. The appropriate cover slip depends upon the objective to be used. Ordinarily, objectives are optically cor rected for a #1V6 (0.17 millimeter) thickness-eover slip. Improper cover glass thick ness will detract from the final image quality.'
6.3.3 Scalpel. A scalpel is needed to cut out a portion of the filter to be examined. A num ber-ten curved blade scalpel is recommended.
6.3.4 Tweezers. A pair of fine-tipped tweezers is used to remove the membrane filter slice from the field monitor and place it upon the slide.
6.3.5 Lens Tissue. To insure cleanliness, a lint-free tissue-h recommended. This tissue should also be used for wiping mounting tools and for cleaning slides and cover slips.
6.3.6 Glass Rod. A fire-polished glass rod may he used to spread the mounting solution on the slide.
r.
L r
f v
W.7 Wheaton Balsam Bottle. This special glass container has a glass top which prevents contamination of the mounting solution. A glass rod is Included for dispensing the solution.
7. Reagents
Chemicals should be reagent grade, free from particles and cotor, conforming to the specifications of the Committee on Analytical Reagents of the American Chemical Society, where such specific cations are available.
7.1 Dimethyl phthalatc
7.2 Diethyl oxalate Avoid getting the mounting solution on the skin. Wash skin promptly with soap and water if skin contact occurs.
8. Procedure
8.1 Sampling
8.1.1 General Information
Guidelines for the monitoring of employee exposures to industrial atmospheres ere
given In Reference 11.8. The Federal requirements for monitoring employee expo*
sure to airborne asbestos are found in 29 CFR 1910.1001.
8.1.2 Mounting the Sampling Pump on the Worker
i
Fasten the sampling pump to the worker's heir and fasten the field monitor to tip
lapel or shirt front (as close to the breathing zone as is practical). Remove the top
cover of the plastie monitor, then Invert the monitor making certain ihe exposed
filter is facing downward. Turn the pump on and adjust to the calibrated flow rate
(1.0 to 2J 1pm). Record the following information in a logbook.
1. Filter number
2. Pump start time and date
3. Flowrate
4. Subject's name and job title 5. Type of operation or process
6. Ventilation controls and is the worker wearing a respirator approved for asbestos?
The pump should be checked periodically during the sampling period for proper oper ation and flow rate.
8.1.3 Optimum Sampling Times The requirement for the minimum count of 100 fibers or 20 fields in 8.3.9 was determined to be the best compromise to achieve adequate precision for the airborne Itwr estimate and reasonable counting times. An optimum fiber density of about f to 5 fibers per microscope count, field is recommended. To estimate appropriate ' sampling times for feasible counting, and optimal counting, one must- consider the following constraints;
1. microscope count field area (generally 0.003 to 0.006 mm*) 2. pump Sow rate (typically 23 Ipm maximum)
3. average airborne fiber concentrations
4. counting rule range of 20 to 100 Gelds
5. adequate fiber density to obtain a minimum eount of 10 fibers in 100 fields, which is the least total fiber count that yields an scceptable count precision
6. background airborne particulate levels that can reduce the count precision due to an obscuring of fibers on the filter surfaee
239-7
(
The preceding constraints were considered in drawing Figures 1 and 2. These figures were developed from the following relationship:
t
sampling time
(FB/FL) (ECA/MFA) (FR) (AC) (1000) minutes
where:
FB/FL 1 to J fibers/field
EGA effective collecting area of filters (855 mm* for 37-mm fiilter with effec tive diameter of 33 mm)
MFA microscope field area (generally 0.003 to 0.00$ mm*)
FR " Pump flow rate (generally 1.0 to 2.5 1pm)
AC * Air concentration of fibers in fibers/cm*.
Figure 1 (microscope field area 0.003 mm*) and Figure 2 (microscope field area "* 0.006 mm*) show optimum and feasible sampling times for a pump flow rate of 1.7 1pm. Each individual responsible for sampling asbestos should prepare a similar chart for his particular pump flow rate and microscope field area before sampling b per formed to aid in estimating proper sampling times. On Figures 1 and 2, the areas with solid shading lines are generally the optimum conditions for counting. The broken shading lines are for conditions very close to optimal. ( However, feasible counting conditions may extend down to about 0.1 fiber/field and and above S fibers/field. Recommended sampling times are most strongly influenced by background airborne particulate levels, once all the other constraints have been estimated. For heavy particulate levels, it may be necessary to limit each filter to about 60 to 180 minutes sampling duration. Each individual responsible for sampling should work closely with the mieroscopist to attain as high as possible filter surface fiber densities (up to about S fibers/field), while avoiding filter surface background particulate levels that create very difficult or. impossible counting conditions. If one has very little idea of airborne fiber and particulate levels, the best procedure b to take several long samples (as one 8-hour or two consecutive 4-hour samples) in con junction with several short samples (as four consecutive 2-hour or eight consecutive i-hour samples). If the longer samples prove very difficult to count, the mieroscopist will have the shorter samples to fall back on. From Figures 1 and 2, it can be seen that there are certain sampling times which will yield optimum fiber densities on the filter for almost all airborne fiber concen trations from 1 to 10 fibers/cm*. These optimum times have been calculated and are . presented in Figure 4. Note that the optimum times given by Figure 4 are approxi ( mate and can be varied by as much as 25%. The nomogram b intended as a guide to be used where no prior knowledge of the air concentration b available.
8.1.4 End of Sampling Period Remove the field monitor, replace the plastic top cover and the smatl end caps, and store the monitor. Always shut off the pump when changing monitors to avoid
( contaminating or damaging the pump. Record the pump shutoff time ar.d flow rate in the logbook.
8.1.5 Blanks
With each batch (25 to SO filters) of samples sent for analysis, submit two unopened
field monitors which have been subjected to tlic same treatment as the samples except
l
that they were not exposed to the sampling environment. Label these as blanks. If the blanks yield fiber counts greater Hum 5 fiber*/100 fields, then the entire sam
pling procedure should be examined carefully for the cause of contamination. The
23V.8 <_
c
mounting solution of Section 8.2.1 should also be examined for contamination and/or crystal growth.
8.1.6 Shipping I The field monitors in which the samples are collected should be shipped in a rigid
* container with sufficient packing material to prevent crushing.
8.1.7 Numbers of Samples When sampling for the Federal ceiling standard of 10 fibers (>5>m)/cm\ (29 CFR 1910.1001(b) (3), effective July 7, 1972), only one sample (IS minutes maximum duration) is necessary, theoretically. However, several samples should be taken dur
f ing expected periods of peak air concentrations to allow for detection of gross sam pling or counting errors. When sampling for determination of noncompliance with the Federal 8-hour TWA standard of 2 fibers (>5jm)/em\ [29 CFR 1910.1001(b) (2)), one should contin uously sample as large a portion of the work day as is feasible for airborne concen trations of about 2 to 10 fibers/cm*. However, for a lower airborne concentration such as 0.5 fiber/cm*, one sample might require 4 to 8 hours sampling time in order to get the proper filter fiber density (Section 8.1.3). For tljis situation, the 8-hour TWA exposure would be determined from one 8-hour or two 4-hour samples as ap propriate.
( 8.2 Sample Preparation
I
8.2.1 Preparation of Mounting Solution
*
A very important part of the sample evaluation is the mounting process. This proc ess involves a special mounting medium of prescribed viscosity. The proper viscosity is important in order to expedite filter dissolving and stiU minimize particle migration.
After the sample has been mounted, an elapsed time of approximately sixty minutes '.si is needed, before the sample is ready for evaluation.
Combine the dimethyl phthalate and diethyl oxalate in a one to one ratio by volume and pour into a Wheaton balsam bottle. Add approximately 0.0S ( 0.005) grams of new membrane filter per milliliter of solution to reach the necessary viscosity. The
mixture must be stirred periodically until the filters have dissolved and a homogeneous I mixture b formed. The normal shelf life of the mounting solution is about three
months. Twenty milliliters of mounting solution wilt prepare approximately 300 samples.
8.2.2 Sample Mounting
Cleanliness b important! A dirty working area may result in sample contamination f and erroneous counts. The following steps should be followed when mounting a sample.
1. Clean the slides and cover slips with lens tissue. Lay each slide down on a clean surface with the frosted end op. It b a good practice to rest one edge of the cover slip on the slide and tha other edge on the working surface. By doing this, you keep the bottom surface (the one-which contacts the filter) from becoming contaminated.
(
2. Wipe all the mounting tools dean with lens tisshe and place them on a clean surface (such as fens tissue). AU tools should be wiped clean prior to mounting each sample.
4
3. Using the glass rod supplied with the Wheaton balsam bottle, apply a drop of mounting solution onto the center of the slide. It may bcliecessary to adjust the quantity of solution so that after the cover slip has been placed bo top, the solu
c tion extends only slightly beyond the filter boundary. If the quantity b greater than this, particle migration may occur.
239-9
I 0
A. C
4. Using another glass rod, spread (he mounting media iqto a triangular shape. The
J'>% size of (his triangle should coincide with the dimension of the filter wedge. 5. Separate the middle and bottom sections of the field monitor case to expose the filter. Cut e triangular wedge from the center to the edge of the filter using the
scalpeL The size of the wedge should approximate one-eighth of the filter surface. The filter can be very carefully removed from the cassette for cutting, but this should only be done with great care..
I 6. Grasp the filter wedge with the tweezers on the perimeter of the filter which was clamped between the mooitor case sections. Do not touch the filter with your fingers. Place the wedge, sample side up, upon the mountinf medium.
7. Pick up a clean cover slip with tweezers and carefully place it on the filter wedge. Onee this contact has been made, do not reposition the cover slip.
8. Label the slide with the sample number and current date before proceeding to die next filter. On the bottom (backside) of the slide, trace the perimeter of the fiber wedge with a felt Up marking pen. This will enable the counter, after the filter
has become transparent, to stay within the filter perimeter when counting.
9. The sample should become transparent within fifteen minutes. If the filter tppears cloudy, it may be necessary to press very lightly on the cover slip. This is rarely necessary; however, counting should not be started until an hour after the mount' inf. This allows the microscopic texture of the filter to become invisible to micro scope viewing.
10. Discard the sample mount after two days if it has not been counted. Crystals appearing similar to asbestos fibers may begin to grow at the mounting media/air interfaces. They seldom present any problems if the slide is examined before two days. In any case, stay away from the filter's edges when eounUng and sizing.
' *.3 Counting of Fibers
8.3.1 Place the slide on the mechanical stage of the microscope and position the center of
the wedge under the objective lens and focus upon the sample. Start counting from
one end of the wedge and progress along a radial line to the other end (count in
\ either direction from perimeter to wedge tip). Random fields are selected, without
looking into the eyepieces, by slightly advancing the slide in one direction with the
mechanical stage control.
8.3.2 It is essential to continually scan over a range of focal planes (generally the upper .
10 to IS micrometers of the filter surface) with the fine focus control during each
field count. This is especially necessary for asbestos fibers due to their impaction ( into the filter matrix.
8.3.3 On most airborne samples, asbestos fibers will generally have fiber diameters less than
one micrometer. Therefore, it b necessary, to look carefully for faint fiber images.
8.3.4 Regularly check phase ring alignment.
8.3.5 When an agglomerate (mass of material) covers a significant portion of the field of
( view (approx 1/6 or greater) reject the field and select another. (Do not include it in the number of fields counted.) However, report the fact as it mzy hate meaning
on other data collection.
8.3.6 Bundles of fibers are counted as one fiber unless both ends of the fiber can be
clearly resolved.
--' '
8.3.7 Count only fibers with a length to width ratio greater than or equal to 3:1. t 8.3.8 Count only fibers greater than 5 micrometers in length. (Be as accurate as possible
in accepting fibers near this length.) Measure curved fibers along the curve to esti
mate the totat length.
239-10 i
i 3 r-
rb 4
. i: * i
r
; <;
If; *
tf
i.-t1 .. i
.*\
(?
1 J;
iif 1 1
8.3.9 Count as many Adds as necessary to yield a total count of at least 100 fibers. Ex* . ceptions: a) count at least 20 fields even if you count more than 100 fibers, and b) stop at 100 fields even if you haven't reached 100 fibers.
8.3.10 For fibers that cross either one or two sides of the counting field, the following pro* cedure is used to obtain a representative count.
i COUNT any fiber greater than 5 micrometers in length, that lies entirely within the counting area. COUNT as "Vi fiber" any fiber with only one end lying within the counting area. DO NOT COUNT any fiber crossing any two sides. Reject and do not count all other fibers. Refer to Figures 5 through 10. Note that the fibers in Figures 3 through 10 are not representative of the appearance of most as bestos fibers. Most fibers have a very faint image.
9. Calibration and Standards
9.1 Sampling Train Calibration The accurate calibration of the sampling pump is essential to the correct calculation of the air volume sampled. The frequency of calibration is dependent on the use, care, and hand ling to which the pump is subjected. Pumps must be recalibrated if they have just been repaired, misused, or received from the manufacturer. If the pump receives hard usage, more frequent calibration may be necessary. Ordinarily, pumps should be calibrated in the labora tory both before they are used In the field and after they have been used to collect a large number of field samples. The accuracy of calibration is dependent upon the type of instrument used as reference The choice of a calibration instrument will depend largely on where the calibration is per? formed. For laboratory testing, a 1-liter buret used as a soap bubble flow meter or wet-test meter is recommended. Other standard calibrating instruments, such as a spirometer, Mar riott's bottle, or dry' gas meter can be used. The calibration should be of sufficient precision that the 95% confidence limits on the flow rate are m 10% (95% of the flow' rates will fall within 10% of the calibrated value). Instructions for calibration with the soap bubble flow meter follow. The sampling train used (pump, hose, filter cassette) in the pump calibration should be the same as the one used in the field.
9..1.1 Check the voltage of the pump battery with a voltmeter both with the pump off and white it is operating to assure adequate voltage for calibration. If necessary, charge the battery to manufacturer's specifications.
9.1.2 Fill a beaker with 10 ml of soap solution.
9.1.3 Connect the filter cassette inlet to the top of the buret with a length of hose.
9.1.4 Turn (he pump on and moisten the inside of the soap bubble meter by immersing the . open end of the buret Into the soap solution and drawing bubbles up the inside of the buret Perform this task until the bubbles are able to travel the entire tength of the buret without breaking.
9.!.$ Adjust the pump rotameter to provide a flow between 1.5 to 2.5 1pm.
9.1.6 With a water manometer, check that the pressure drop across the filter is less than 13 inches of water (about 1 ioch of mercury).
9.1.7 Start a soap bubble ap the buret and measure the time it takes for the bubble to travel a minimum volume of 1 liter.
9.1.8
Repeat the procedure in 9.1.7 at least three times, average the results, and calculate the calibrated flow rate by dividing the volume traveled by the soap bubble by the elapsed time. If the range between the highest end lowest of the three flow rates is greater than about 0.33 Ipm, then the calibration should be repeated since it is likely that the precision is not adequate.
239-11
9.1.9 Dali required for the calibration Include the volume measured, elapsed time, pressure drop, air temperature, atmospheric pressure (or elevation), pump serial number, date, and name of person performing the calibration.
9.1.10 Corrections to the flow rate-for pumps with rotameters may be necessary if the pres* sure (elevation) or temperature where the samples are collected (actual flow rate) differs significantly from that where the calibration was performed (indicated flow rate). Actual flow rates at time of sampling may be calculated for a linear scale rotameter by using the following correction formula:
where both pressure (P) and temperature (T) are in absolute units such as:
psia
psig + 14.7
deg Rankin TM deg Fahrenheit + 460
deg Kelvin * deg Celsius 4* 273
9.2 Microscope Setup
9.2.1 Porton Reticle and the Counting Field .The asbestos fiber count procedure consists of comparing fiber length to the diam
eters of calibrated circles of a Porton reticle, and counting all fibers greater than
S micrometers In length lying within a given counting field area. The Porton reticle
is a glass plate inscribed with a series of circles and rectangles. The left half of the
reticle is divided into six rectangles constituting the counting field. The counting field Is illustrated in Figures 5 through 10.
9.2.2 Placement in Eyepiece The Porton reticle Is placed inside the Huygcnian eyepiece where it rests on the fieldlimiting diaphragm. If other types of eyepieces are used, it may be necessary to insert a counting collar for retaining the reticle. The reticle should always be kept clean, since dirt on the reticle is in focus and could complicate the counting and siring process.
9.2.3 Stage Micrometer The Porton reticle cannot be used for counting until it has been properly calibrated
with a stage micrometer. Mast stage micrometer scales are approximately two millimeters long and are divided into units of one-hundredth of a millimeter (ten
micrometers).
9.2.4 Microscope Adjustment When adjusting the microscope, follow the manufacturer's instructions while observing the following guidelines.
1. The light source image must be in focus and centered on the condenser iris or. annular diaphragm.
2. The particulate material to be examined must'be in focus.
3. The illuminator field iris must be in focus, centered on the sample, and opened only to the point where the field of view is illuminated.
4. The phase rings (annular diaphragm and phase-shifting elements) must be con centric
9.2.5 Porton Reticle Calibration Procedure Each eycpiece-objeetivc-rcticle combination on the microscope must be calibrated. Should any of the three be changed (disassembly, replacement, zoom adjustment, etc), the combination must be recalibrated. Calibration may change if ieterpupiliary dis-
239-12
.tinea h changed. For proper calibration, the following procedure should be followed closely.
With 10X objective hi place, place the stage micrometer on the mechanical stage, focus the millimeter scale, and center the image. Change to the 40-45X objec tive and adjust the first millimeter scale division to coincide with the left boundary of 1 the Portoci rectangle. Measure the distance between the left and extreme right bound aries of the Porton rectangle, estimating any portion of the final division. This meas urement represents 200 L units. The rectangle is 100 L units on the short vertical dimension. The calculated ML" is inserted into the formula D L(2*)*'* where MNM I Is the circle number (indicated on the reticle) and "D" is the circle diameter. Since the circle diameters vary logarithmically, every other circle doubles in diameter. For example, circle number three is twice the diameter of number one; number four is twice the diameter of number two. When the circle sizes have been determined, the count ing field area which consists of the left six smelter rectangles can be calculated from the relation 10.000 L*. This completes the reticle calibration for this specific objec tive-eyepiece-reticle combination.
t 1
Example for Ponoa Retide
The following calibration was obtained for a pair of 10X Huygeaian eyepieces and a 43X objective:
200 L 0.148 am " 148 micrometers 100 L " 0.074 sun 74 micrometers
\
One L-unit * 0.74 micrometers
Thus Circle #1 has a diameter D - 142*)'* - 0.74(2,),/3 - 0.74 (1.414) - 1.0$ micrometers. Then our circle diameter calibration table looks like:
Diameter of Circle #1 1.05 micrometers #2 * 1.48 #3 - 2.09 #4 - 2.96 #$ 4.19
(
#6 - 5.92
Field area - (10,000) (L*) - (100 L) (100 L) (0.074) (0.074) * 0.0055 mm*
Thus fibers with a length greater than a distance halfw ay between the diameters of the #5 and #6 circles would be counted. If a Patterson Globe and Circle reticle is used, a different calculation procedure is required. The drcle diameters arc related as follows. The #25 circle diameter is 0X1) (retide length). The circle diameters are proportional to the ratio of their numbers. Thus the #20 circle diameter is (20/25) or 0.8 times the #25 circle diameter.
(.
10. Calculations
10.1 The average airborne asbestos fiber concentration estimated by the filter sample may be calculated from the following formula:
( AC fffB/FL) - (DFB/BFL)] (ECA) (1000) (FR) (T) (MFA)
239-13
where;
.
AC * Airborne fiber concentration in (fibers > 5 *m)/em*. BFB " Total number of fibers counted in the BFL fields of the blank or control filters
irv fibers > 5 *m. BFL * Total number of fields counted on the blank or control filters. ECA ** Effective collecting area of filter (855 mm* for a 37-mm filter with effective di
ameter of 33 mm). t FR Pump flow rate in liters/min Opm).
FB * Total number of fibers counted in the FL fields in fibers > 5 *m. FL * Total number of fields counted on the filter. MFA * Microscope count field area in mm* (generally 0.003 to 0.006). T *" Sample collection time in minutes.
10.2 Recount criteria. It is very desirable for a counter to eonduct a "Mind recount** for about 1 in every' 10 filter wedges (slides) counted. Alternatively, a second counter could perform the blind recount. In training sessions for novice counters, the trainee should conduct a blind recount for filter wedges counted by an experienced, proficient counter. In all cases, we will observe differences between the first and second counts of the same filter wedge. Most of these differences will be due to chance alone, that is, due to the random variability (precision)
1 of the count method. Statistical recount criteria enable us to decide whether observed dif ferences can reasonably be explained due to chance alone or are probably due to systematic differences between counters or microscopes or due to some other biasing factor. The following recount criterion is for a pair of counts'that estimate some airborne fiber con centration (AC) in fibers/cm*. The criterion is given at the typc-I error level. That is, there is a 5% maximum risk that we wilt reject a pair of counts for the reason that one might be biased, when the large observed difference is really due to chance. Reject a pair of counts because one might be biased if:
(AC* - AC,) exceeds 2.77(ACXCV
where: ( AC, * lower estimated airborne fiber concentration
AC* ** higher estimated airborne fiber concentration AC average of the two airborne concentration estimates CV,, * average CV for the two concentration estimates which are a function ot the total
fiber count (FB) in each ease. Use the relation in Section 4 or Figure 3.
For a pair of counts on the same filter, reject the pair because one might be biased if:
(FB, - FB,) exceeds 2.77(FB)(CV^;)
where:
t
'
FB, " lower fiber count on the filter (total fibers)
f FB, m higher fiber count on the filter (total fibers)
FB average of the two total fiber counts
CV,,, CVT for the value FB. the the relation in Section 4 or Figure 3.
11. References C lt.l Lynch. J. R., K. J. Kronowlcr, and N. A. Lcidct, "Validity of the Poisson Distribution in
Dust Counting**, unpublished. 11.2 Wculner, R. B. and H. E Ayer. "Dust Exposure in Asbestos Processing**, Transactions of the
'4
239-14
1*
J*
* e| :* i ' I'
i ;.
!I ' i
i i-
American Conference of Governmental Industrial Hygienists, May 1972, pp. 103*121, San Francisco, California.
11.3 Conway, R. E, and W. D. Holland, "Statistical Evaluation of the Procedure for Counting Asbestos Fibers on Membrane Filters", LFE Corporation, Richmond, California. Prepared fo^the Asbestos on Membrane Assoc/North America, New York, 1973.
11.4 Leidel, N. A. and K. A. Busch, "An Evaluation of Phase Contrast Microscopes for Asbestos Counting'*, presented at the 1974 American Industrial Hygiene Conference, Miami Beach, Florida, May 18, 1974, unpublished.
11.5 Beckett, S. T. and M. D. Attfield, "Inter-Laboratory Comparison of the Counting of Asbestos
Fibers Sampled on Membrane Filters", Ann Occup Hyg 17:85-96,'1974.
11.6 Rajhans, G. S. and G. M. Bragg, "A Statistical Analysis of Asbestos Fiber Counting in the Laboratory and Industrial Environment" Am Ind Hyg Assoc J 36(12):909-915, 1975.
11.7 Leidel, N. A. and K. A. Busch, "Statistical Methods for the Determination of Noncompli ance with Occupational Health Standards", KIOSH Technical Publication 75*159, 1975.
- 11.8 Leidel, N. A., K. A. Busch, and J. R. Lynch, "Occupational Exposure Sampling Strategy Manual". NIOSH Technical Publication 77*173. 1977.
11.9 Leidel, N. K. A. Busch, and W. E. Crouse, "Exposure Measurement Action Level and Occupational Environmental Variability", NIOSH Technical Publication 76*131, 1975.
11.10 Comments of the Johns-Manville Corporation with Respect to the Notice of Proposed Rule* making: Occupational Exposure to Asbestos, Federal Register, October 9, 1975. Submitted to the public record at the U. S. Department of Labor, Occupational Safety and Health Ad-f ministration, April 1976.
11.11 Leidel, N. A., S. G. Bayer, R. D. Zumwatde. and K. A. Busch. USPHS/NIOSH Membrane Filter Method for Evaluating Airborne Asbestos Fibers, to be published by NIOSH in 1977.
11.12 Needham, G. H., The Practical Use of the Microscope, Charles C. Thomas Publishing Corporation, Springfield, Illinois, 19S8.
11.13 Clark, G. L., The Encyclopedia of Microscopy, Rhomboid Publishing Corporation, New York, 1961.
11.14 McCrone, W. C. and J. G. Deity, I. The Particle Atlas, Edition Two, Ann Arbor Science Publishers, Inc., Ann Arbor, Michigan, 1973.
*
f
r VRE 1. Optimum Sampling Times (or airborne asbestos where microscopic feld ana * 0.003 mm4
230*16
sro *>4 *
sha o
T'^ /A,
f 'coo
VpfS
<*wa
** **ie.
?Jp. /?
** 0-OOc
0.40
1
i
i
*8
I
r|
s
6
lfiO `N0IXV1HVA JO 1N3DIJJ30D IVldL * 239*18
( '
!
:1< t i
I 1I
I
4, i
J 1
;t
i;
;i
fc :
V
It
i ir
c* l
i
ft i: *t ;
-f
U*
fIt 4J
1*
t
i
tf ,i
!t
i
I' !
F IG U R E 4. Nomogram o f optimom sampling times fa r airborne asbestos fibers la concentrations o f
1 to 10 fibcrs/cm*
( 2utu V3V 013U 3dOOSOdOtW - V
In i.t.m i.. n I. i?. . . I." . I . . . t . . t n , i I t t I , , , |
/
8
N
6 iOE#k
N
E
g
*-
N|
too 1i tn m 2 P CM
Q CL
y 6 l o.
<
X
Ul
<
ui tc
T -]--i *i i i-r rm-j- i i i --r rri [--r i` | i
m OJ
Sinu|Ui' 3WH ONIldWVS/WnWIldO
i
(
c wtfi *3iva moij dwnd-di
239-19 c
, ncuM$
**
(
nctmt* C
239-20
i t
I'V : %
'! t
t
I|
\I
l ?1
f
+*
LIST OF FIGURES
(S through 10) FIGURE i. DO NOT COUNT. Fiber crosses top tad bottom tides. FIGURE &, COUNT. One fiber. FIGURE 7. .COUNT. One-half fiber. Fiber crosses left side eod one end lies witbia count area. FIGURE 8. COUNT. Ooe-balf fiber. Fiber crosses bottom tide ead oae ead lies witbia count
area. FIGURE 9. DO NOT COUNT. Fiber crosses two tides. FIGURE 10. DO NOT COUNT. Fiber crosses two tides (bottom left corner).
COUNT. One-half fiber. Fiber crosses bottom side end one ead lies within count erne. COUNT. One fiber (top right corner).
239-21
I
ATTACHMENT C REPRESENTATIVE AMBIENT-AIR ASBESTOS CONCENTRATIONS
f
Representative Aobtent-Atr Asbestos Concentretlons
Location
New York Washington Miaul Cleveland Denver San Francisco Spokane
Ffbers/cc
0
0.0022 0.0027 0.0067 0.0041 0.0038 0.0154