Document bBN3DQaBRJZk7yq17zwb8VZ9g

Monsanto Chemical Company Organic Chemicals Division St. Louis Research Department Work done by: J. R., Darby w. G., Allen E. E., Cowell N. W,. Touchctte L. R.. Wangler J. A . Cannon HARTOLDMONOOQ5199 1. File 2. J. R. Darby 3. J. H. Lum - F. B. Zienty - File 4. Duplicate File 5. -etrctiiabe-:--ftsaoc .--and -Assl-str. Research -Directors Cr.xf*'H ''I1 -7- 6. J. A. Cannon 7. w. B. Hicks 8. H. I. Armstrong 9- H. W. Mohrman - Springfield 10. F. J . Locke - Springfield 11. Extra 12. Extra 13. Extra This report contains confidential information which is the property of the Monsanto Chemical Company and which shall be disclosed only to duly authorized persons. The recipient is held accountable for the filing and safe custody of the report which must be returned on demand. 0690765 HARTOLDMON0005200 Page No. j . INTRODUCTION................................................................................................1 II. SUMMARY............................................................................................................1 III. CONCLUSIONS..................................................................................................1, 2 IV. RECOMMENDATIONS.............................................................. V. PATENT STATUS ........................................................................................... 3 VI. REFERENCES.................................................................................................... 3 VII. EXPERIMENTAL WORK ........................................................................... A. Quality Control ........................................................................... 3 1. Santiolzer160.........................................................................4 2. Santiolzer141........................................................................ 4 B. Compatibility of Carbide and Carbon's Monomer MG-.1........................................................................................................ 4 C. Volatility of Santiolzer 213 and Santiolzer 214...........................................................................................................5 D. Effect of Mixing Incompatible Plasticizers of Opposite Polarity........................................................................ 5> E. Intensive Evaluation of Experimental Product 6004.................................................................................................... 1. Properties evaluation .................................................... b 2. Compatibility ........................................................................ 6 3. Tensile Properties ............................................................. 6 4. Migration.............................................................................. 6, 7 3- Soapy Water Extraction ................................................... 7 G. Dry Blending and Extrusion...........................................8 7- Heat and Light Stability............................................... 8 F. Odor Masking of Aroclor 1232 in PVAc Adhesives . 8 G. Migration of Aroclor 1262 and HB-40................................ 9, 10 H. Volatility of Chlorinated DDB vs. DDB........................... 10, 11 I. Work Covered In Other Reports.............................................11, 12 VIII. DISCUSSION...................................................................................................... 12, 13 IX. EXPERIMENTAL PROCEDURES......................................................................... 13 X. APPENDIX........................................................................................................... 13 3 HARTOLDMON0005201 Figure 1 Table I Table II Table 111 Table xv Tabic V Table VI Table VII Table VIII Table IX Table X Table XI Table XII General Motors Lacquer Test for Aroclor 1262 and HB-40 Volatility of Chlorinated DDB vs. DDB Per Se Volatility of Chlorinated DDB vs. DDB Volatility and Mill Loss of Stabilized Chlorinated DDB vo. DDB HARTOLDMON0005202 1. I. INTRODUCTION Successful participation in the competitive plasticizer market depends not only upon maintenance of production of current products and the introduction of new plasticizers but also upon the adapta tion of present products to various applications. The burden of proof for product performance in any given application rests with the producer. It is basic, then, that present products and by products be evaluated both generally. In order to observe proper ties which might be advantageous, t d particularly to see if re quirements are met for specific applications. The objectives of this Job number, therefore, are the evalua tion of plasticizers for quality control, intensive evaluation of new plasticizers which have shown promising properties during screening, direct comparison of Monsanto plasticizers with specific competitive products and the evaluation of Monsanto products and by-products in respect to performance in new applications. II. SUMMARY This Job number covers a number of problems rather than a closely kr,lt major program. Santlclzer 141 and Santlclzer 160 processes modifications were checked for quality of products in regards to heat and light sta bility. A polymerizable plasticizer. Monomer MG-1 (Carbide and Carbon), was checked for compatibility. The volatility (per se) of Santlclzer 212 and Santlclzer 214 were determined. Incompatible plasticizers of opposite polarity were mixed to determine possible synergistic compatibllizing effects. Blends of dodecylbenzene with di-2-ethylhexyl phthalate, di-lsodecyl phthalate and Santlclzer 141 were evaluated as possible primary plasticizers. Odor masking of Aroclor 12J2 in polyvinyl acetate adhesives ar.d migration of Aroclor 1262 and HB-40 were studied. Work was initiated on the retention of physical properties during aging of electrical formu lations. The volatility of chlorinated dodecylbenzene was compared with that of dodecylbenzene. III. CONCLUSIONS The following conclusions are draw:, from the details of the evaluations on the various problems. A. Quality Control 1. Santlclzer 160 Charcoal refined Santlclzer 160 (butybenzyl phthalate) 13 completely equivalent in light stability and very slightly superior in heat stability to regular production S-160. 0690768 HARTOLDMON0005203 2. The trlethylamlne process yielded S-160 with heat and light stabilities equivalent to control 3-160. 2. Santlclzer 141 Santlcizer 141 made by the reverse addition method of preparation of the Intermediate sodium phenate Is comparable to regular S-141. Santlclzer 141 washed only with hot water Instead of lye water to reduce emulsion formation has satisfactory heat stability. B. Monomer MG-1 is incompatible as a plasticizer for PVC. Polymerization by the addition of two percent of benzoyl peroxide results in compatible, brittle systems of poor heat stability. C. The 24 hour per se volatility test indicates that the percent plasticizer lost from Santlcizer 213 and Santlclzer 214 la only slightly lower than the percent of dodecyl benzene ori ginally present. D. Although compatibility was not achieved by mixing benzyl stearate with each of several more polar esters, no conclusions can be made here as to the general possibilities of this procedure. E. Experimental Product 6004 (one part dodecylbenzene and three parts Santlclzer 141) Is compatible with PVC to give formula tions with flexlbilizing efficiency equivalent to DOP. Volatility and water sensitivity are higher for E.P. 6004 than for DOP. Heat and light stability are fairly comparable with DOP. The tendencies of E.P. 6004 to migrate to furniture lacquer, nitrocellulose sheeting and styrene wall tile are serious deterrents to applica tions In which there might be possibilities of contacts with these surfaces. F. Poliak and Swartz's masking agents Nn 1004 (camphor odor) and No. 1066 (fruity odor) are effective In neutralizing the odor of Aroclor 1232 in polyvinyl acetate adhesives. 0. A compound containing a monomeric plasticizer (DOP) with 20 parts HB-40 or Aroclor 1262 will not mar or soften nltrocellulose film and will probably pass the General Motors Lacquer test. H. Chlorinated dodecylbenzene has higher boiling range and lower per se volatility than dodecylbenzene, but the volatility of chlorinated DDB In plasticizer PVC is higher than that cf DDB. 0690769 j '] | | 8 1 ' ! ' I | HARTOLDMON0005204 3- IV. RECOMMENDATIONS This type of application research should be continued so that new and varied applications iay be found for Monsanto products through the extensive knowledge obtained on plasticizer properties. General information is essential in keeping abreast with competi tors in filling requirements of the industry. V. PATENT STATUS The nature of the work covered by this report is that of further investigation of materials previously considered and it is felt that patentable features have been or are being evaluated by those concerned with the original Inventions, if any. No dis closures were filed from the Applications Group as a result of the work covered by this report. VI. REFERENCES Final reports on Job No. 2-02-750.01-3129, Part I, "The Intensive Evaluation of Santlclzer 214 and Experimental Product 6002" by J. A. Cannon and Part II, "The Evaluation of Isophthalates as Plasticizers for Polyvinyl Chloride" by N. W. Touchette are the other reports written for this Job in 1936. The Pinal Report on Job No. 2-02-750.01-2896, Part II, "Appli cation Work on Present Plasticizers", by P. R. Graham and Final Report, Job No. 2-02-750.01-2616, Part V by J. A. Cannon contain references to all prior reports written concerning application of present plasticizers. VII. EXPERIMENTAL WORK The work covered by this Job number consists of various prob lems rather chan one specific type. Therefore, the details are recorded here in individual sections for each particular problem. A. Quality Control The continuous scrutiny of economic performance and product quality of production items results in process modifications from time to time. Plasticizers produced after altering the method of preparation must be evaluated for performance, at least in the areas which might be affected most. 0690770 HARTOLDMON0005205 4. 1. Santiclzer 160 Heat and light stability tests on Santiclzer 160 pre pared with two different process modifications were equivalent to standard production S-160. The one preparation utilized charcoal refining as compared to permanganatlon and the other process In volved the use of the trlethylamlne salt of butyl acid phthalate. 2. Santiclzer 141 Samples of Santiclzer 141 (reverse phenate preparation method) and S-141 (hot water wash instead of lye water) were formu lated at 50 PHR In Opalon 300 unstabilized, and stabilized with the lead system (POS-C, DS-207) and with the epoxy system (0-60, Mark XI and Mark XX). Both S-141 samples were tested for heat stability and found to be satisfactory. Light stability of S-141 (reverse phenate method) was found to be equivalent to control S-141. B. Compatibility of Carbide and Carbon's Monomer MO-1 Screening evaluation of Monomer MO-1 indicated limited com patibility in replacing DOP. To check the compatibility in plastisols the following formulations were prepared with Opalon 410 and plasticizer concentration of 80 PHR. Monomer MO-1 is a polymerizable plasticizer and in the formulations indicated two percent benzoyl peroxide was added as catalyst, based on the weight of MG-1. TABLE I Loop and Window Exposure Compatibility of MO-1 Plasticizer, 8p PHR Loop Test Window Exposure MO-1 MO-1 t- Catalyst MO-l/DOP (5:1) MO-l/DOP (3:1)+Catalyst MO-l/DOP (1:1) MO-l/DOP (l:l)+Catalyst MO-l/DOP (1:5) MG-l/DOP (1:5)+Catalyst DOP Incompatible Brlttle-no loop Incompatible Brittle-no loop Compatible Compatible Compatible Compatible Compatible Incompatlble-1 week Decomposed in mold Slight exudatlon- 3 weeks Decomposed in mold Slight exudatlon- 3 weeks Wo exudatlon-3 months Slight exudation- 3 weeks No exudatlon-3 months Very slightly tacky- 3 months The exudant reslnlfied on the surface of the incompatible formula tions after continued exposure in the window. 0690771 HARTOLDMON0005206 D. Effect of Mixing Incompatible Plasticizers of Opposite Polarity &^ In an effort to obtain a compatible plasticizer system by mixing two incompatible materials of opposite polarity, five samples (50:50 mixtures by weight) were prepared using the non polar benzyl stearate, an incompatible plasticizer, with several polar esters ranging from incompatible, through compounds of limited compatibility, to compounds of borderline compatibility. The plasticizer mixtures were: 1. Benzyl stearate with diethylene glycol bls(o-benzyl glycolate) Benzyl stearate with diethylene glycol bis(butyl phthalyl glycolate) Benzyl stearate with diethylene glycol dl(butyl succlnyl glycolate) H Benzyl stearate with ethylene glycol bis(butyl phthalyl glycolate) Benzyl stearate with 2,6-dl-lsopropyl phenol . All five were incompatible. Nos. 1 and A showed slight exudation almost immediately. Humber 5 would not completely fuse on the roll mill. 0690772 HARTOLDMON0005207 6. E. Intensive Evaluation of Experimental Product SCO1! 1. Properties Evaluation The properties of Opalon 300 plasticized with E.P. 6004 at 20#, JOJC, 40# and 50% plasticizer concentrations are compared with DOP in Table III In the Appendix. 2. Compatibility Compatibility testing of E.P. 6004 consisted of loop test and window exposure on 20%, 30%, 40# and 50# unstabilized formulations and on 40# formulations stabilized with the lead system (POS-C, DS-207), the epoxy system (G-62, Mark XI and Mark XX), Staycin I and dibutyl tin dllaurate. No exudation was observed for any of the formulations In the loop test for one week In the case of the unstabilized and two weeks for those stabilized. The unstabilized samples did not exude during the four months of window exposure. Of the stabilized formulations, E.P. 6004 sta bilized with dibutyl tin dllaurate exuded in one week, whereas the others have given no Indication of incompatibility for four months. 3. Tensile Properties Tensile strength, 100# modulus and elongation were determined for 20%, 30%, 40# and 50# E.P. 6004 formulations in comparison with DOP. The results are displayed In Figure 1 In the Appendix. 4. Migration Experimental Product 6004 was tested for tendencies to migrate to polystyrene wall tile, nitrocellulose film and nitrocellulose furniture lacquer. E.P. 6004 and DOP were formu lated at 40# plasticizer concentration and placed in contact with the various surfaces. The results of the testing are recorded below. TABLE IV Migration Tests on E.P. 6004 Duration of Test Polystyrene, 50C. Nitrocellulose Lacquer, 50C. Nitrocellulose Film, 50C. E.P.6004 POP E.P.6004 DOP E.P.6004 DOP 1 week 2 weeks 3 weeks 4 weeks 3-4 3-3 C-4 B-3 C-4 A-3 3-4 3-3 C-4 3-3 C-4 A-3 B-4 B-3 C-4 3-3 -C-4 A-3 B-4 3-3 C-4 3-3 C-l A-3 0690773 HARTOLDMON0005208 7. The alphabetical and numerical ratings above are interpreted as follows: 0 None 1 Very slight 2 Slight 5 Moderate A Severe A Marking (surface marred but not sticky) B Softening (surface marred and sticky) C Lifting (surface removed from panel) E.P. 6004 was compared to DOP at various plasticizer concentrations with respect to migration to Linde Silica. The results of this testing are recorded below. TABLE V Linde Silica Test $ Loss After 1 day $ Loss After 3 days 20$ 0 50$ 0.50 40$ 2-5 50$ 4.5 0 0.70 4.5 9.6 20$ 50$ 40$ 50$ 0.30 0.47 1.2 2.0 0.16 1.0 2.7 4.7 5- Soapy Water Extraction $ Loss After 7 days 0.06 1-3 7.3 16 0.27 1.8 5.0 9-0 The formulations listed in the Linde Silica Test were tested for extraction by 1$ Ivory Soap solution at 30C. for 24 hours. The results are listed below: TABLE VI Soapy Water Extraction E.P. 6004 DOP 20$ 50a 40$ 60`S 20$ 50$ 40$ 30$ $ Plasticizer Lost 2.5 7.1 13 22 1.1 l.A l.l 1.2 0690774 HARTOLDMON0005209 3. 6. Dry Blending and Extrusion The dry blending and extrusion characteristics of E.P. 6004 were compared with DOP. Formulations of 50 PHR of each plasticizer were tested as shown in the following table: TABLE VII Dry Blending and Extrusion of E.P. 6004 1254 Opalon 500 FM Opalon 500 E.P. 6004 DOP POS-C DS-207 100 50 5 0-5 100 50 5 0.5 100 50 3 0-5 100 50 3 0.5 Time to dry blend (min.) Temp, at dryness Extrusion rate (g./mln.) 25 75C. 14.1 45 75C. 16.4 '(5 120 75C. 75C 15-2 17-9 7 Heat and Light Stability E.P. 6004 and DOP were evaluated for heat and light stability in formulations stabilized with the lead system (POS-C, DS-207) and the epoxy system (0-60, Mark M and Mark PL). Heat degradation occurred slightly earlier for E.P. 6004 than for DOP in the lead system and much earlier in the epoxy system (i.e., 60 minutes vs. 180 minutes at 170C.). Exposure in the Padeometer caused degradation of ".P. 6004 and DOP after 200 hours in the lead system and not until 300 hours with the epoxy system. F. Odor Masking of Aroclor 1252 in Polyvinyl Acetate Adhesives Odor masking agents used were: LeFevre Chemical Co. LeFevre Chemical Co. Coumarln Poliak and Swartz Poliak and Swartz No. 14-2 No. 15-5 No. 1004 No. 1066 Films containing 0.005/6 and less masking agent (based on resin content) were aged for 40 hours at 150"F. After these aging conditions the films still retained the odor of the masking agent. M Cg 0690775 9. G. Migration of Aroelor 1262 and HB-40 Migration of Aroelor 1262 and HB-40 to nitrocellulose film was tested using the following formulations. ' 1 " "2" 5 ...4... 5 --6 7 8 9 Opalon J00 100 100 100 100 100 100 100 100 100 DOP 68 55 -- 52 55 27 55 65 55 G-55 -- 55 75 52 55 27 55 -- G-52 666 6666 6 6 Aroelor 1262 -- -- -- -- 10 -- 20 20 HB-40 -- -- -- 10 ... 20 ____ 20 Ferro 1823 55 555555 Atomite 25 25 25 25 25 25 25 25 25 Shore "A" Hardness 72 7?.5 77 75 75 75 72 72 70 Films 1 in. x 1 in.. were placed on nitrocellulose sheets under one psi pressure at room temperature and at 50C. The results are listed below: TABLE VIII Migration to Nitrocellulose Films at Room Temperature Formulation 1 week 2 weeks 3 weeks 4 weeks 5 weeks 10 week3 00 0 0 0 2A 2A 2A 2A 2A 2A 2A 5A 5A 5A 00 1A- 1A- 1A- 00 0 0 0 1A- 1A- 1A- 1A- 1A 00 1A- 1A 1A 00 0 0 0 00 0 0 0 0 2A 5A 1A 0 1A 1A 0 0 50C. n/c Films 2k 2A 2A 5A ID- 1B- 2B 2B 13- 1B- 5B 5B M A 4 A 2B 2B 2A 5A 5A IB 3A 5 A 1B- 2B 2A 4a 1B- 23 00 0 0 00 0 0 5A 2B 5B 2B IB 2B 2B 0 0 5A 5B 4B 5B 2B 2B 2B 0 0 0690776 } HARTOLDMONOOQ5211 10. Rating Code: 0 No Change 1 Very slight 2 Slight 3 Moderate 4 Severe A Marking B Softening C Lifting The General Motors test for migration to automobile lacquer was also run for the above formulations. TABLE IX General Motors Lacquer Test Formulation 1 2. 3 A 5 6 7 3 9 Remarks Extreme softening Extreme softening Lifting Extreme softening Lifting Softening Lifting Indentation - very slight softening Indentation - very slight softening H. Comparison of the Volatility of Dodecylbenzene (DDB) and Chlorinated Dodecylbenzene Chlorinated DDB and DDB were formulated to equal hardness as 1:2 mixtures with DOP. Specimens of each were subjected to charcoal volatility and circulating air volatility tests. TABLE X Volatility of Chlorinated DDB and DDB Chlorinated DDB-DOP (1:2) DDB-DOP (1:2) Percent Plasticizer Volatility: [% Plast.Lost) Charcoal Method Circulating Air Method Shore "A" Hardness: Before Volatility After Charcoal Volatility After Circulating Air Volatility 40 25-S 41.5 82 83 ?9 42.5 13.7 33-6 82 33 o7 0690777 HARTOLDMONOOQ5212 .11 The per se volatilities were determined for chlorinated DDB and DDB and for 1:2 mixtures with DOP. TABLE XI Per Se Volatility of Chlorinated DDB and DDB Time (hours) Cl. DDB # Plasticizer Lost DDB Cl. DM-DOP DDB-DOP 2 5-5 9-5 2.4 6.9 J) 9.4 22.2 4.0 11.2 24 51-7 85.8 13-8 28.1 Chlorinated DDB and DDB were formulated in 1:2 mixtures with DOP (33-1/3 percent plasticizer) in epoxy stabilized formula tions. The milling loss was determined and the stabilized sanples were tested for volatility. TABLE XII Volatility and Mill Loss of Stabilized Chlorinated DDB and DDB Chlorinated DDB-DOP (1:2) Percent Plasticizer 33-1/3 Milling Loss: P---e---r-c--e--n-t o^---f Secondary Plasticizer Percent Total Plasticizer 27 9 Volatility: Plast. Lost) Charcoal Method Circulating Air Method 22.2 38.8 Shore "A" Hardness: Before Volatility After Charcoal Volatility After Clrc. Air Volatility 87 92 92 I. Work Covered In Other Reports DDB-DOP (1:2) 33-1/2 49 16 18.8 33-1 88 93 93 The Intensive evaluation of Santlclzer 213 and Experimental Product 6002 has been reported In Final Report No. 2-02-730.01-3129, Part I by J. A. Cannon. 0690778 HARTOLDMONOOQ5213 12. Testing of electrical formulations for the retention of physical properties during heat aging was initiated under this Job number and continued under Job No. 2-02-750.01-3254 and will be covered in reports for that Job number. This work includes: 1. Stabilizing DIDP with Blsphenol A and TCP 2. Stabilization of Santicizer 300 3. Retention of physical properties upon heat aging of secondary plasticizers, Kendex 0869X, Socony XT-1045A, Halowax 4004 and Aroclors 1248, 1254 and 5460. vm. DISCUSSION In replacing 0NB (o-nitro biphenyl) in polyvinyl acetate adhesives with the Aroclors a serious objection, that of odor, developed. The approach taken was that of using commercial masking agents to neutralize or replace the disagreeable odor. Success was achieved by the use of the Poliak and Swartz agents. Incompatible plasticizers fall into two general categories, the polar and the non-polar. The objective of one segment of the work under this Job number was to see if mixing polar and non-polar Incompatible plasticizers would result in compatibility. The work initiated for benzyl stearate and several glycolates although unsuccessful has been continued to Include other systems under an exploratory Job number. Quality control evaluations are necessitated by the require ments for consistent performance characteristics of production items. Thus, as processes are changed due to shifting raw material sources and/or modification of manufacturing techniques, the products resulting from such changes must be evaluated for effects upon the ultimate end uses. During the period covered by this report, the modifications of Santicizer 160 and Santicizer 141 processes yielded products comparable to their predecessors. Monomer MG-1 (Carbide and Carbon's polymerizable plasticizer, dipropylene glycol dimethacrylate) is proposed by Carbide and Carbon Chemical Co. to make it possible to obtain harder formulatlo 3 than have previously been attainable through plastisol techniques. Their literature claims performance comparable to DOP when used as partial or full replacement for DOP. Compati bility studies showed MG-1 to be incompatible as a replacement for DOP. When catalyzed by 2^5 benzoyl .peroxide, compatible formulations are obtained. 0690779 .1 s HARTOLDMONOOQ5214 15- The program of blending dodecylbenzene with primary plasticizers was continued to include Santlclzer 214 and E.P. 6002 (Final Report No. 2-02-750.01-3129, Part I) and Experimental Product 6004 (one part dodecylbenzene and three parts Santlclzer 141). The intensive evaluation given these products included properties evaluations on plasticized PVC at various concentrations, compa tibility studies, evaluations of tensile properties, migration, soapy water extraction, dry blending and extrusion and evaluation of heat and light stability. During the screening of chlorinated dodecylbenzene a volatility higher than that of dodecylbenzene was obtained. The boiling range of chlorinated DDB is higher than for DDB. Per se volatility was determined for both compounds and showed chlorinated DDB to be lower in volatility than DDB. Since all tests indicated lower per se volatility and higher volatility from the plasticized sheet for chlorinated DDB other tests were proposed to help explain the cross-over. Volatility tests were run on stabilized chlorinated DDB and DDB with results comparable to those on unstabilized formu lations; chlorinated DDB still showed higher volatility than DDB. The determination of plasticizer lost during milling showed that about three times more DDB was lost than chlorinated DDB. This higher mill loss could result in apparently higher volatility for chlorinated DDB because of errors in calculating the volatile loss of DDB. Further work to explain this cross-over was abandoned due to the unattractive volatility and economic factors of chlorinated DDB. IX. EXPERIMENTAL PROCEDURES All test methods used in this work are contained in the test method manual entitled, "Standard Test Methods of the Organic Division, Plasticizer Applications Laboratory". This manual is kept up to date with revisions as old tests are improved or new ones developed. X. APPENDIX The original notes for the work covered by this report may be found on notebook pages; 79104, 79114, 80620, 80623, 80628, 30631, 80637, 8063S, 80639, 80641, 80646, 80643, 83364, 83365, 83367, 83368, 83369, 83370 J. A. Cannon nd 5-21-57 Darby 0690780 HARTOLDMONOOQ5215 PROPERTIES IIZED OPALON 300 Plettlclser 40( 'irUess ^p^ciri*d E.f.6004 as CU61- -160 1:3) ` e;p;60O4 sox E.F.6004 401 E.1.6004 OOP 0{ BOX Kt mm rn *'lit i i4ol ded et If*c- X y u9. t* 0 oX3 t0. r> u a Hm u ma c oVc ooh4 It. si. yel nod. mod, aa- iloua, noa lo bo r nod. mod. It. aa- si. ;loud; nod. el lo ber It. si. y.i vod. mod, aa- sloudj od. low ber BiOd,' it. 1. yel to nod, aa- Houdj noa. low heavy ter si. yei, BOd. nod. cnar SlOUdJ od. low IT -IS -38 -58 n 7 ** -< V -*04' > 'a4. ^ ---------r dnessj Host itsblll ty un t0- -4 o 9i m Ini -r 1 Abt**oi* r *o ptlof u ry Cl 4r1tj. > <*hW1 < * EtC 0 "Sc -4 r\ f> o <V aI4?<. -*44 u V zz *.3 r> a < 4<>1 *-4 jv? *v *ri 5 25 6.7 100 100 0.04 0,95 4,2 16 62 96 21 72 83 0.33 1.6 10 0.64 i.s 22 17 66 73 4.8 98 94 0.50 8.6 38 -- C.89 8.5 D0P OOP SOX 40.C yel el. BOd. nod. low cloudjl BOd. low Tel BOd. nod nil cloud BOd, low -19 -39 S.4 86 86 5.7 74 76 ... 1.0 8,0 U 0.01 1.0 46 19 1. yel 001 50< aod. nod nil cloud aod, low -53 4*6 64 57 0.05 1.6 80 _______i 0690781 PI i1 HARTOLDMONOOQ5216 3000 2000 FIGURE 1 (lCOOl'.oau^us) ' E. 1.6004 ocr 20 40 50 0690782 HARTOLDMONOOQ5217 1000