Document aBeRbrm4vomd9wq6Zbp9eXkRB

APR 1 1-1 AROCLORS IN POLYESTER AND EPOXY RESINS MONSANTO CHEMICALS LIMITED 050937 7 I TOWOLDMON0034672 WATER_PCB-00019141 AROCLORS IN POLYESTER AND EPOXY RESINS Technical Service Bulletin No. G5/1 Copyright Reserved Published I960 I Monsanto LXiJ MONSANTO CHEMICALS LIMITED MONSANTO HOUSE, 10-18 VICTORIA STREET, LONDON, S.W.l O^*78 | TOWOLDMON0034673 WATER_PCB-00019142 AROCLORS IN POLYESTER AND EPOXY RESINS Polyester glass-fibre laminates are becoming more and more widely used for the manu facture of industrial and consumer goods, their chief recommendation being their high strength-to-weight ratio and the ease with which large and complex forms can be fabri cated. Certain applications of polyester laminates call for the modification of some of their inherent characteristics. Those which most commonly require modification are fireresistance and mechanical properties, and for both purposes the Aroclors are highly suitable. The Aroclors are a range of chlorinated diphenyls and polyphenyls, three of which have proved to be economical and efficient as dual-purpose fire-retardants and plasticisers. The high proportion ofavailable chlorine they contain imparts adequate self-extinguishing properties, while their plasticising powers increase the strength of the resin to a degree equal to that gained by a more expensive plasticising polyester. The recommended Aroclors are readily mis cible with uncured polyesters at the con centrations necessary to impart fire resistance, though the solid ones dissolve more easily at 60C. Once mixed they have no tendency to separate on standing nor to migrate to the surface ofthe cured resin. In this respect they are superior to certain other chlorinated com pounds whose poor compatibility with poly esters could lead to separation after mixing and thus to unsightly blooming and greasiness on the surface ofthe cured resin. The Aroclors also have the advantage of being practically odourless. acaoclor h a Rc The Aroclors may be used to similar effect in epoxy resins as well as polyesters, being com patible with both types. Full details of all the Aroclors, which range in physical form from mobile, oily liquids to hard, opaque resins, are given in Technical Service Bulletin G.l. POLYESTER RESINS (1) Fire Resistance. Of the possible methods of improving the fire resistance of polyester resins, the use of the Aroclors has the advantage of being both effective and economical. The Aroclors recommended as fire retardants are the soft, sticky resin, Aroclor 1260, and the hard, brittle resins, Aroclors 4465 and 5460. These compounds are more highly chlorinated and less volatile than the mobile liquids, and both these properties improve their efficiency as fire retardants. Like other fire retardants for polyesters, the Aroclors are generally used in combination with antimony trioxide, itself a fire retardant. This combination is particularly effective, as the two substances are synergistic and to gether give a degree of fire resistance which is adequate for most possible uses. The Aroclor imparts self-extinguishing properties to the resin and the antimony trioxide reduces afterglow. The latter also plays the part of an inert filler, replacing a proportion of which ever of the many possible fillers is being used, and is usually included even in inherently fire resistant resins which contain chemically combined chlorine in the polyester molecule. The properties of the Aroclors as fire retard ants were evaluated in a series of laboratory tests using a general purpose polyester with a red Trade Marie. 0509379 TOWOLDMON0034674 WATER_PCB-00019143 styrene content of 35%. The catalyst used was 2% of a 60% solution of methyl ethyl ketone peroxide in dibutyl phthalate, added after the Aroclor. 2% of a 1% solution of cobalt napbthenate was used as an acceler ator. Specimens measuring 9' X i' x i' were cast in waxed moulds without reinforcement. The test method used was based on that laid down in the Ministry of Supply Aircraft Specification for unsaturated polyester resins, DTD 5537 Appendix 10. It consisted of clamping the test specimen in a support with its longitudinal axis horizontal and its trans- again failed to continue burning the material was classed as seif-extinguishing. The results obtained are shown in Table I. (2) Effect on Physical Properties. Among the special qualities of the Aroclors is the desirable plasticising effect they have on the cured resin. For general purpose poly esters a special plasticising polyester is norm ally included to increase the flexural strength ofthe naturally brittle resin. When an Aroclor is included it effects a similar improvement and thus makes the addition of a more expensive plasticising polyester unnecessary. TABLE I FIRE RETARDANCY Per cent of antimony trioxide and Aroclor Aroclor 1260 5 per cent Semi inflammable 7} per cent Semi inflammable Aroclor 4465 Aroclor 5460* Inflammable Self extinguishing 60 secs. Self extinguishing 5 secs. No test 10 per cent Self extinguishing 30 secs. Self extinguishing J secs. Self extinguishing 5 secs. 15 per cent Self extinguishing Immediate Self extinguishing Immediate Self extinguishing Immediate *21% addition of Aroclor 5460 is insufficient to make the polyester self-estinguishing. verse axis inclined at 45, and placing a bunsen burner with the tip of the flame to {' in height just in contact with the end of the specimen. At the end of 30 seconds, the flame was removed and the specimen allowed to burn. If burning did not continue, theflamewasreplaced for a further 30 seconds immediately it ceased, and if the specimen Specimens for mechanical testing were pre pared from laminates with four plies of 1} oz. woven glasscloth, giving a final thickness of approximately -/a" and a resin content of approximately 50%. Woven glasscloth was used in preference to chopped strand mat to ensure that results should be as consistent as possible, the strength of this form of 0509380 !I TOWOLDMON0034675 WATER_PCB-00019144 reinforcement varying by only 5 %, compared with the 20% variation to' be expected from chopped strand mat . The following standard methods of test were used to determine the mechanical properties of 4* x 1' bars cut from the laminates: flexural strength, ASTM D.790-49T; impact strength, falling weight, B.S.2782:1957, Part3, Method 3068, modified by the use of beam specimens on a 1' bridge support. The effect of the Aroclors on the mechanical poses of lamination. For fire-resistant surface coatings, the solid Aroclors are preferred. EPOXY RESINS Epoxy resins, like polyesters, are inflammable unless a fire-retardant additive is included, and those Aroclors which are used in poly esters are equally effective at similar con centrations in epoxies. They are completely miscible with epoxy resins, though Aroclors 4465 and 5460 dissolve more readily at 60C. TABLED MECHANICAL PROPERTIES Resin Formulation Unmodified Polyester Polyester +plasticising polyester Polyester-(-Aroclor 1260 Polyester -f*Aroclor 4465 Polyester -(-Aroclor 5460 Elastic Modulus Flexural Strength in bending Impact Strength (p.s.i.) (p.s.i. x 10-*) (ft. lb.) 47,210 219 1-73 10% 20% 43,310 39,930 200 156 1-64 1-24 10% 20% 45,600 33,880 20-9 16-9 1-33 204 10% 20% 40,740 33,390 219 129 1-41 2-48 10% 20% 37,400 35,890 170 15-5 1-85 3-06 properties of polyester resins is shown in Table II. It will be seen that at a concentration of 10% (enough for purposes of fire-retardance) none of the Aroclors reduced the flexural strength of the cured resin signifi cantly, and that their effect was comparable with that of a plasticising polyester. At 20% addition, the impact strength of the laminate is unproved. Of the three, Aroclor 1260 reduces the flexural strength less than the solid Aroclors, and is recommended for pur- Some diminution of the characteristic mech anical properties ofepoxies must be expected, though careful formulation will enable the manufacturer to strike a balance between fire resistance and strength for applications where the former property is essential. Antimony trioxide is included at the same concentration as the Aroclor since the two together are more effective than Aroclor alone. The same laboratory test methods were em ployed as for polyesters, using a liquid epoxy 0509381 TOWOLDMON0034676 WATER_PCB-00019145 resin (Shell Epikote 834) cured with 8% dicthylcnetriamine, added after the epoxy resin, antimony trioxide and Aroclor were mixed. Specimens were prepared in waxed moulds 9' x i' x 1' and the results obtained are shown in Table III. ......... If Aroclors are spilled on the skin, it should be washed with soap and water. If accidental burns occur from contact with hot Aroclors,the burn should be treated in the same way as an ordinary burn. Aroclor adhering to the burned area should be removed carefully by TABLEm Per cent addition of Aroclor and antimony trioxide 5 per cent 7} per cent Aroclor 1242 Inflammable ~ No test Aroclor 1260 Inflammable Semi inflammable Aroclor 4465 Inflammable Semi inflammable Aroclor 5460 >- Inflammable : -- --- Self extinguishing - 40 secs. *" \ 10 per cent IS per cent Inflammable Self- 30 secs. ~ Self extinguishing 30 secs. Self extinguishing Immediate "Self- ------------- Self- -- extinguishing extinguishing 20 secs. Immediate Self extinguishing 20 secs. _ Self extinguishing Immediate HANDLING AND TOXICITY J repeated washing with soap and water, or a The Aroclors are non-oxidising and non- vegetable oil may be used. Experimental work xorrosive and they are-not-hydrolysed-by ------ on-animals-indicates-that the maximum safe water, alkalis or acids. At ordinary tempera concentration of vapours in workrooms is in tures they have not presented industrial toxi the range of 0-5 to 1-0 milligrams per cubic cological problems, but they should never metre of air, and where vapours may be en theless be handled with care and should not countered, local exhaust ventilation together be allowed to come into contact with the skin, with general workroom exhaust is necessary. through which they are absorbed. 6 0509384 TOWOLDMON0034677 WATER_PCB-00019146 Every effort has been made to ensure that the information in this publication is reliable, but as the conditions under which it may be applied are beyond our control, we cannot accept responsibility for any results of its use. Forme No. P.B.649 El 6001. Published by Monsanto Chemicals limited and printed by The Chiswick Press, London, N.U 0509383 "I TOWOLDMON0034678 WATER_PCB-00019147