HYDROUS CALCIUM SILICATES
f' 'jp*0'
/
PART V
;
Physical and Chemical Properties ______ of Kaylo Products
*
> ,}"
4
if
Sing (2) H--r Buroh Sex<&4 - s- s 7
aylcr
r. P'.
Jarjin - Collir-.--
Mr, J. R. HacRstt
General Research (2) ---- "
PLAIIMTIFF'S EXHIBIT
wy-ooo/z^
01 102 0743
HYDROUS CALCIUM SILICATES
FOREWARD
The science and technology of the hydrous calcium silicates were not advanced as far as desired when the broad potentialities of these products as structural and insulating materials were recognised by the Owens-Illinois Glass Company. The overall plans set-up by the Company to develop the kaylo products in cluded a relatively large project having as objective the ad vancement of the basic knowledge.
This report, in the first three parts, summarizes In some detail the results of the planned research on the chemistry of kaylo. Part I deals largely with the nature of the solids forming in the ternary system llme-sillca-water and represent* the foundation of the basic science. Part II gives the funda mental and some practical information on xonotlite and lepisil kaylos, products which originated in the basic studies described in Part I. Part III, also based on the first part, gives the chemistry of the presently produced kaylo products and describes the important effect of alumina not previously recognized in these solids.
parts IV and V include discussions on materials and processes, and physical and chemical properties of kaylo, respectively. The subject matter of these two parts was not amenable to detailed description because changes are being made currently in both formulations and processes. Alos currently, some of the test :~3thods for determining the properties of kaylo products are :eing revised to keep pace with other developments. It was for `his reason that this report was prepared in five separate parts, >ach of which may be amended or rewritten without calling for *'9vision in the others*
01 102 0741
3!ABLE OF CONTENTS
I. INTRODUCTION II. DENSITY III. STRENGTHS
1. Modulus of Rupture in Bending 2. Compressive Strength IV. HANDIEABILITY 7. THERMAL CONDUCTIVITY VI. VOLUME STABILITY AT ELEVATEDTEMPERATURES VII. PERMEABILITY TO GASES VIII. DURABILITY IN C03 AND S08 IX. DURABILITY IN FREEZING ANDTHAWING X. FIRE RESISTANCE XI. CORROSIVENESS XII. OTHER PROPERTIES OF KAYLO
Page 1 2
3 4 5 7 11 14 17 19 20 21 22
01 102 0745
I. INTRODUCTION
Description of kaylo products in sales literature centers in large part around the terms: light density, high strength, low thermal conductivity, volume stability, incombustibility and others. These terms denote properties responsible for the position kaylo has gained in wide markets as an accepted new structural and insulating material. This portion of the report defines the properties and the methods of measuring them, and the units in which they are expressed. Considerations are also given to the implications these pro perties have on the usefulness of the kaylo pi'oducts.
-1-
t
f1 ?
01 102 0740
II. DENSITY
Density simply means the weight of a solid per unit of volume. It is understood in using the term density in connection with kaylo that apparent density is implied. The density of the constituent solid parts of kaylo, approximately 150 pof, is many times greater than of the overall density of the highly porous kaylo products. The density is obtained by measuring the dimensions of a trimmed sample, weighing it and computing the weight in pounds per cubic foot. The sample is weighed while still hot after being oven dried at 300?, generally overnight.a
Kaylo products are currently made in two densities, nominally 10-11 and 20-22 pcf. Density indirectly expresses the thermal conductivity, and the lighter the weight the better is the heat insulation. Strength and other factors, particularly of processing, established the basis for the choice of the given densities. Strength is less important for products of low densities used primarily as heat insulation than for the 20 pof products, except from the standpoint of breakage losses.
a Details of tests and limitation are given in Company's specifications.
-2-
01 102 0747
in. strengths
1. Modulus of Rupture in Bending
The strength most descriptive of this property of kaylo is the modulus of rupture in bending, commonly referred to as flexural or bending strength. The modulus of rupture in bending is the computed ultimate strength, and is defined as the fictitious tensile (or compressive) stress in the extreme fiber of a teem computed by the flexure equation,
S * Mc/l
where
S, is the fiber stress,
M, the bending moment,
c, l-d (depth of beam),
and I, the moment of inertia.
For a square or rectangular cross section the equation reduces to the following form, for single point loading at midspan,
where
57, is the total load at failure.
1, the distance between supports.
b, the width,
d, the depth.
Obviously, the kaylo products loaded as a beam in service such as the roof tile must carry a total load at midspan considerably smaller than that represented by the total load at failure, Vf in the above equation. In practice the tensile stress developed by kaylo without reinforcement is insufficient to carry the ultimate potential load, allowance being made for an appropriate factor of safety. For this reason roof tile is reinforced with a wire basket located approximately l/2 of an inch from the bottom side of the tile as placed in the roof. The modulus of rupture of the non-reinforced kaylo is not of itself a criteria of the strength of the roof tile. Present specification is based on the ultimate load applied to a full size slab. With a 34 inch span between supports,with the load applied at midspa^ the reinforcement taking the load is in Tension. The specified minimum ultimate load is 900 pounds. This corresponds to an overall fiber stress of 355 psi for roof tile having a thickness of 2-5/8 inches. The specifications also require that the modulus of rupture of non-reinforced kaylo of the roof tile shall be 150 psi or higher. This value is obtained by loading the roof tile in inverted position, the wire basket being in the top position. The same tile is then turned over and tested for the ultimate load. This double use of a tile for test purposes is possible because structurally the face containing the reinforcement is not damaged during the first loading. The failure occurs in tension. The modulus cf the kaylo itself
0- 01 102 0748
la a roof tile might appear to be a superfluous result, but in practice it genres as a check on the quality of the kaylo.
The modulus of rupture of the core material i3 obtained in the same manner as that of the roof tile during the first loading. The computed stress is a measure of the quality of the product. The minimum allowable modulus of rupture is 160 psi.
The light density ware at Sayreville is tested the same as the core material. Tests at the Berlin plant are made on specimens by 3 by 12 inches in size. The minimum allowable modulus of rupture is 35 psi. This requirement is easy to fulfill but experience has shown that a higher modulus is desirable in decreasing losses due to breakage. The present 10-11 pof density kaylo shows a modulus of 60 to 80 psi.
Standard testing machines are used for strength determination. The Sayreville plant is equipped with a 50,000 lb. Baldwin-Southwark Universal testing machine, the Berlin plant with a Scott flexure tester and the General Research Laboratory with a Tiniua Olson Universal Testing machine.
The bending strengths of kaylo-cement asbestos (KGA) laminates and others are, of course, muoh higher than of un-reinforced kaylo. The increase in strength is proportional to the strength of the surfacing material. Cement asbestos increases the modulus up to about an 800 psi fiber stress. Recent experimentation in the laboratory with the direct application of speciallyprepared Portland cement slurries to kaylo is showing promise as a method for making laminates according to a comparatively simple method. The modulus of these products ranges from 600 to 800 psi.
2. Compressive Strength
The compressive strength of kaylo does not represent the ultimate strength in compression at failure as in the case of concrete. Because of its highly porous nature kaylo undergoes an inelastic deformation at a certain load and continues to deform as the load i3 increased. The 10 pcf product shows a com pressive strength of about 150 psi at a deformation of 5 percent. For so light a material, this is a relatively high strength which is desirable during application and maintenance as workmen moving about on the kaylo do not cause any structural damage to the insulation in place.
The compressive strength of the 20 pcf material has no real physical significance in any present applications. Only a few data have been obtained and these indicate that the strength in compression is about 400 to 500 psi far small deformation of the test specimen.
01 102 0749
HA! 'DISABILITY
Kaylo, due to its very nature of being light weight, is subject to abuse in handling which a heavier material v/ould be spared. Because of this the susceptibility to loss by breakage at the plant, during transit and installation requires evaluation by tests -which would measure the quality of the ware in this respect. The resistance to breakage is not easily measured or expressed as n. number of factors are involved. The modulus of rupture gives a rough indication of potential losses due to fracturing of full sise specimens, but is not a measure of resistance to chippage. Brittleness is an important factor in chippage and that is me.3urabie in terms of resistance to shear and impact stresses. Mechanical abrasion is another potential cause of loss of wear and can be evaluated in abrasion tests.
The term hacdleability hms been introduced by ASTM Committee G-16 Sub committee S-l for designating the resistance to breakage of such materials aa kaylo. As indicated by the preceding paragraph, the number of factors involved does not permit the derivation of any simple definition. The definitions pro posed by the sub-group for handleability and some comments are as follows*
1. Handlaability is that group of physical properties of a block of pre formed insulation, 'sheroin each property is expressed as a numerical value, which can be used aa a measure for evaluating the block's ability to withstand the rigors of reasonable mechanical stresses upon it without suffering undue damage. These stresses may be encountered by the dry block in the manufacturer's finishing processes, in transferring the individual blocks, in shipping the cartons of blocks, in applying the block to the job and in its ultimate service on the job. They may consist ofj static flexural stresses* com pressive stresses; impact stresses and abrasive stresses.
2. The handlability of an insulation block (or pipe covering) might be understood to be the ass and effectiveness with which it can be transported, manipulated sad applied to a job with a minimum of breakage and labor.
3. Handleability is that property of a material which enables it to be shipped and installed without undue breakage -when handled with ordinary roughness.
t. H&ndleabiiity ia defined as the measure (or index) of that combination of physical characteristics which enables the preformed insulation to be handled without excessive damage .due to breaking, cracking, crushing or other S'cmctural failure, under the conditions of normal severity of loading or stress to which it will be subject as a result of handling before and during i ns ta'11 atio n.
j. Handleability of preformed thermal insulation blocks is the ability of the material to be processed, packed, shipped, stored, transferred to job cits, shaped where necessary and installed with a minimum of breakage or other donate* it i.3 a combination of strength, resiliency, hardness and abrasion resistance and is affected by density and unit dimensions.
-5-
01 102 0750
' Comments -
It seems improbable that an index value obtained by slimming or multiplying factor.* assigned to the test results of individual measurements of various properties such as outlined in the definition above will give a quantitative figure indicating handleability. A single poor factor - such as poor resilience - with other factors good- could result in poor handleability example; long, narrow, thin glass plates.
Low strength and hardness, but good abrasion resistance and excellent resiliency could produce a very handloable product - example* rubber mats.
ilith equal resiliency, strength, hardness and abrasion resistance, long, narrow, flat sheets could not be handled as well as shorter, wider, thicker sheets. All other factors being equal, high-density products will be harder to handle than low-density products.
Of interest in connection with handleability are hardness and abrasion
tests described in Navy Department specifications for Thermal Block Insulation
No, 32-I-3, Dec, 1, 1943. The hardness test consists in the measurement of
the penetration, of a 1/8 inch diameter ball point under a load of 1 kg into
the material mounted in a commercial apparatus called a plaatometsr. The
maximum all rwable penetrations are 1.13, 0.95 and 0.75 mm. for densities of
ib O.-r } 23, 27
Kaylo of 11 psf density showed a penetration of 1.00 nn. which
well -within allowable limits of the test.
The abrasion test involves the determination of material abraded from twelve 1-inch cube specimens by twenty four 3/4-inch oak tubes during 10and SO-minute periods of tumbling in a special machine built for this purpose. The percentage by weight of the cubes dusted or broken off during this period is obtained. The maximum loss in -weights for 15 pcf density ware were 40 and 70 percent for the 10- and 20-minute tests. Light density kaylo showed a loss cf only 17 to 13 percent at the end of the 20-minute test, which is well within the allowable limits.
kaylo insulation block containing a fracture is still usable providing
the pieces do not separate at the point of fracture. Long-fiber asbestos impart.3 the desired hinging strength discussed in another part of the report concerned with properties of asbestos.
01 102 07
RMAL GG:;DuCTIV:IY
is a well-known fact that heat may he transferred between two surfaces at different temperatures by adiation, convection and conduction. A heat insulation material for highest efficiency hould offer resistance tc heat flow by each type of transfer. The nrooortionate amount of total heat transferred by any one of these type depends on a number of factors. Flow by radiation increases as the fourth power of the absolute temperatures. Air is a very poor conductor of heat and, if immobile, so that heat is not trans
Cerred by convection, it is a good insulator.
Kaylo contains pores of exceedingly small sizes and this very fact accounts for small radiation&l losses. Although kaylo is a continuous-air type insulator the resistance to air flow is relatively high and heat loss by convection is relatively 3ml 1. The heat is transferred primarily by conduction at the relatively email temperature differences as would obtain for roof tile or KCA panel in service. At high temperatures, the heat losses by radiation are of course greater, and convection losses may also be significant, especially for thin insulation application.
Thermal conductivity of a substance is defined as the amount of heat that will flow in unit time between opposite faces of unit area and ur.it thickness having a temperature difference of 1 degree. In the English system the unit for thermal conductivity, designated as X, is B.t.u./hour/s^. ft./F/inch of thickness. is expressed in many units. Seven of the more common ones are as follows;
ITo.
Unit
Used 3y
1. Joules, sec*'1, era*, CTx,eia Elsctr. Eng . & ICT
2. Gm cal. sea"1, cm"2,"C"1,cm Physicists
3.
hr"1,
11 Foreign Engineers
4.
3tu, hr''x, ft", F-r, in.
Mech. A Refrig. Eng.
5.
3tu, hr"'x, ffa. CF"1, ft.
Chem. Eng.
0,
Biu, hr" in."3, "I"1, in.
-
7^
'ttB.ij C%> 3 i 5
v/ ^-3 jji
Ales system
It will be noted that unit No. 4 in this table is used in kaylo technology'-. For facilitating conve rsion from one unit to another this following table is presented
Joules, jec,"3-
cnra c> ~~ cm.
3S0 j cm, "3
**> cal.
?-* v -* 1
C,"l 7s
ij tAl *
hr,'"3, i.ojO- , -2 F,~1 in.
--j j
hr,"1 V,4'.-.. -2
..
*F,"* ft.
Btu, hr,"1 in,-3
!? -X
in.
batts m"a G,J*1 m.
1.000
4.135 0
0.00144 0.0173 0.208 0.0100
0.235 1.000
0.00273 0,000345 0.00414 O.O497 0.00239
y y> -i A O .t.
360 1.000 0.124
1.49 17.9
0.861
693 2S03
3.06 1.000 12.0 144 6.93
"Unit used in kaylo publication. rr
57.7 242
0.672 0.0833 1.000 12.0 0.577
4.61 20.2
0.0560
C.00695 0.C835 1.000 0.0481
100 419
1.16
0.144 1.72 20.8 1.000
01 102 07
sibtjq^ux 9uxq.T3insui JO 80UBq.onpuoo q.B9M 3uxJns-8aui jcoj ^uarndynbo 3ut.i-p.r3n2 jo sq-red x'sdioui-1^ J 3niAra.ia
X -j[ a-inSx^ *Utd P9/0O0 -J9JDM
///////"//// ' 'B/c/U/DQ /C 92.
///s//Z '/*>>////> // 9/du/og js9J_ V//S///////
01 102 0753
Use of .'able,
d! '
--e { fao^o -
-i insulating cats a' .1 - i j. foreign manufacturer is
given '3 0.041 lg.>l. 'hr ./4n.3/o0/ia. .o c,, - - - ihis value to other units,
run :1c vn the
' ..dad, Xg.C&l, hr,"1 *i3 ' O,""3- m, until the value of
1.CC0 .s foi' -' -in -.ove horizontally to ' o column headed by the desired
unit fund r;'
:,e original X faocor by ha factor found. Thus a K factor
of 0.C41 }.
-/"O/e is equal to 0. 41 x 3.GQ .330 3tu/hr/fta/s?/in.
fie c.-.-thoas .f list for determining the K factor are not as precise or
t3hly sta.-,.. u u;. r-d. aa would to desired, fany factors are involved in the
design of -.-st squipment. The guarded-plate method is generally acoepted as
the moat orr-cise and has been standardized by the American Society for Testing
Materials, ft is described in ASTM specifications C177-45. Although this
method is
od currently in our laboratory (its adoption being delayed by
obtaining
' vt input heater units) it will become the standard method.
4 ooaparati
.thod embodying most of the principles of the standard test
method is bo
ised. The equipment is cheeked against either kaylo or cork
t-oeoimeas of :-n X factor and the factor so obtained is then applied in
;.-ioutati .'r. . 9 K factor of the test specimen.
TVe p -v.ic.t- ie of the guarded-plate method is the measurement of the amount :* a: it t. -un-r.i tted through a sample of known area sad thickness, and the temperature ifforou .I.. ' tween the hot end cold sides. The heat-input unit is placed between ir. 3;ecisens of a given kind and size. The important factor to control .? the po :s .. . j movement of heat laterally from the heater. Such heat obviously
Id -,o e vansnitted through the test samples. The corrective against this iff . .".'.v' c the use of a guard ring heater placed around the heat-input unic -id ?i-sd -vlh the material under test. This ring heater is built in the
inner '-i of the came' materials as the heat-input unit. In use, it :.s ; . : ained ;-.t Identically the same temperature aa the input heater by a
M-ats c ctrol and heater system. The control of temperature is affected .n electrical controller activated by a multi-junotion thermocouple, equal "her of junctions being placed in contact with the guard ring heater and the . .V.-'o ai heater. Only the guard ring heater is in circuit with the controller. ? % vc input into cue principal heater, which of course, equals the heat : ;af :rred through the test specimens after equilibrium conditions are v-tain-'d, is 'vacured with a wattmeter.
'"-.3 gensi-\.L arrangement of the guard ring, principal heater, samples, ; c . rcrnal plates maintained -at constant temperature ia illustrated by --.c u -out section in Figure V. 1. This cut shows the method of using watov at
t temperature flowing through the steel plates comprising the cuts! 'c !. .g of the js. -.ole. This method of maintaining constant temperature oi n.c .d 3id is suitable, of course, for temperatures in the range between 32 rd *F. ft :: 2: irafures bslow 3T: or above 212F other methods are 'used. . u vat f v .r.-?ratnj'8 the outside plates may be maintained at a selected s . .ire by vlrctrio 'caters in conjunction with a suitable controller. r;v ethod generally used is that of increasing the thickness of the . ;i. : on the cold side , ' he water coil plate forming the outside su.rfe.co
-i v .posits set of -.psoimeas.
I he ` .'tnosi'aov'.re of the cola end hot sides are measured v/ith thermocouples hi electrical input is measured with a wattmeter. These and other data -..pairod for the determination of the X factor are.-
~8~
01 102 0754
1 = thickness of the sample ia inches.
A m area of sample through which th9 heat flows in square feet.
fc3 average temperature of warmer -surface in F.
average temperature of cooler surface in F.
q corrected watt input to heater x 3.412 in Btu/W.
The aquation for computing the K factor is*
X - ql_________ Btu, hr"1, ft"a, in"1,0?"1 A(t3 - t'x)
The overall coefficient of heat transmittance, air to air temperatures, is designated U. It is the measured factor for built-up wall sections. The heat may be transmitted by conduction, convection, and radiation in a wall and therefore the factor IT is used correctly only if this condition obtains. The factor C ia the coefficient of thermal conductance computed for the sur face temperature of the unit under test. Strictly speaking, the factor U for air to air temperature is correct for expressing the heat conductance through a Trail or roof exposed to the sky. The outside surface temperature in winter of a built-up wall or roof will be 1 to 2F lower than the air due to heat lost by radiation to the sky. Therefore, the factor U as determined in the laboratory, by a method to be described, would be somewhat in error if used in computations for the stated service conditions. The factor U is obtained using the guarded box method in which a wall is mounted as a partition in a constant temperature room and an area in the middle region on one 3ide is covered with a box containing heaters in circuit with a wattmeter. The air immediately outside the* heater box is maintained at exactly the same tem perature as within the box. The air on the cooler side is maintained at a fixed and constant temperature. Baffles are inserted between the heaters -and the test wall as a precaution against radiation from the heaters. The overall air-to-air coefficient of heat transmittance, IT, con be computed from the equation,
Watts x 3.412 Btu, hr"", ft"!VF~1 (t~- ^x) ~ Area
The preceding discussions and formula for calculating the factors apply to parallel flat surfaces. In computations involving curved surfaces such as pice covering it is required that the proper effective area is known. In a cylindrical shell the area across which heat is flowing becomes greater as the thickness is increased. This area can be computed from a formula obtained by calculus. This formula iz:
A * 2 (r3 - r^2, in i r'c7r"i)
(per unit length)
where A is the log mean area, ro, the out3ids diameter,
and the inside diameter.
-9.
01 102 075E>
\.r 1 xc-sv z-'at'i? and relatively small -rhicknees value, the arithmetic sear. -.a (rfe - rjJ/2 nay is used. Consider able error is made, however, using *he -u".'nsaetiw Year, area when the ratio of ??j?x 13 Iss'S*
tap re se ntativa values of X are given in Table V. 1. for regular plant kayio uid -to not lite slabs made in the pilot plant.
The ykij^cm of heat diffusivity is of interest in connection with the time requirements for heating or cooling and also for explaining why hot kayio nay be handled rithout causing burns. Thermal diffusivity expresses the rate at which ,n_ insulating material is heated or cooled. Computations of time required to heat a furnace, for example, to some desired temperature are based on the thermal conductivity, heat capacity and density of the insulation material. The thermal diffusivity is expressed as l/cd where X is the con
ductivity factor, c the specific heat, and d the density. 'The lower the value of X/cd, the longer is the time required to heat to a specific temperature, or conversely, uo cool.
It is ,;f : Tteresi to reproduce an example from iViIkes1 book on "Heat Inflation ' (p. 133-134) comparing 3 insulation materials set up as walls of orsns of -- tual factor (.042). nemely, 4 inches of 85 percent magnesia block, 4 irr: :.vs f glass wool, and 4 inches of crumpled aluminum foil. At a constant tec?emature of 500"? all three ovens lose the same amount of heat per unit of lime. I a '-h Ls computation it is first required to compute the heat input to olsTuro 'he tempo ratin' of the insulation. This is simply the product of average Minimum temperature, specific heat and density. These data are given ,.n t.j following tablej
ou_ abion
d, (Bulk)
3tu/ft'3
ISagn osia Class wool Al. foil
0.234 .234 .24
15 3 0.13
1233 204 13
CV> :,..rt step is the computation of the ratios of heat requirements and these f.r " 1 11.03 for the aluminum foil: glass wool- magnesia. This ratio also ;-- ni 3 the relative tines to he at the oven since the U factor is the some for .-.11 three ( ,C42) .
'he same result is obtained by substituting in the formula, x/ed, for heat
if.;: ; Lvity. The values for heat diffusivitiss are 0.0099 , 0.060 and 0.92 .t-yh .. for the magnesia, glass ?/ool and aluminum foil, respectively.
incc the time required for heating or cooling is inversely proportional 'o f - diffusivity, it follows that the larger the thermal diffusivity the , v:-rthe time required to offset the change in temperature. The ratios 1 scr;-'u: the X/od values are 1*15:93 for magnesia block; glass wools aluminum >il. This means that the magnesia block will take 93 times as long as the aiunirun to heat up to a steady stats.
-10-
01 102 0750
<jl. STABILITY YLE-TAirD TS!.:?1IRAT1JEBS
A high degree oi* volume stability of light density insulation block and pipe covering is desirable fer certain installations at elevated temperatures. Tavy Department Specifications 32i-8d Aug. 2, 1948 ior pips insulation require chat linear shrinkage of pipe covering shall not exceed 2.0 percent for com pounded insulation of 18 and 15 pof density at temperatures of 750 and 1000*F, respectively. Xaylo easily meets these specifications, showing shrinkages of 0.3 and O.S percent (or less) at the stated temperatures. In practice this shrinkage is somewhat too high, ns the kaylo pipe covering exposed to high temperatures on the hot side (500-900?) undergoes a shrinkage while the out side surface at a markedly lower temperature does not. The insulation tends to warp and if restrained from movement, as it generally is in service, it may undergo cracking. These cracks in no way impair the thermal efficiency but ere a cause of loss in oil refineries where the pipe insulation is removed periodically for inspection of the pipes. In the stripping operations and subsequent re-application of the erne ware, some pieces break in two and are discarded.
The drying shrinkage of the gel-like hydrous calcium silicates may be eliminated in large part by previous drying at elevated temperature, the gelliko solid becoming partially irreversible. This treatment preshrinks the insulation but is a costly operation. A considerable amount of work on formulations and processing has been carried out with the objective of preventing the drying shrinkage without increasing the cost or altering the present processes. Some interesting results have been obtained, occasionally certain products showing D,o shrinkage-cracking. These results are not always -oadily duplicated. Among other observations holding promise were those using CaGL-, ?.s an Additive. Addition of this salt to regular plant slurry produced in on experimental autoclave was effective. However, duplicate products mads in the plant did not perform satisfactorily, the specimens showing about the same degree of cracking as those without treatment. It appears that our operations are on a borderline and the products obtained it certain stages of the reaction or under different initial processing may vary due be r,light unknown alterations in the process,
.hcr.otiits kaylo would perform satisfactorily as a pipe insulation, but the slurries our. be handled only with difficulty in present equipment, konotlite-lepicil combinations relatively low in iopieil -should prove satis factory also and possibly, if made from cement formulation, present process equipment would be suitable.
t-u method of test for evaluating the drying shrinkage of kaylo may be one of three used to date. The exposure of a full section of pipe insulation on a pipe heated to the temperature of service is the most direct. Cracking, if it is to develop, will be evident in one day or less. Another method per mit ting the simultaneous testing of a number ox* specimen, cut from slabs or pipe insulations, is heat seeking overnight of previously-measured specimens at a selected temperature. The length can be measured to a sufficient degree of accuracy using micrometer calipers and specimens about 10 to 15 inches long. The allowable shrinkage will have to be predetermined and data are now being gathered which will give the maximum permissible shrinkage. The third method involves xhs use of a furnace designed for measuring thermal coefficient
,, n.
01 102 0757
Ranges in shrinkage of different types of plant and laboratory kaylo upon heating.
01 iaa
Linear change? oT 10 pcf Berlin and 14 and 45 pcf xonotlite kaylo during heating and cooling.
it & 'i
01 102 0759
L ./n m a r cficrnpm
'? -jV" ;
. . .rt
i` aC I
,e. i .' .mo-3 ;;;.r a
` .j '. is a" * ly r?. r; . .1 sv i..i A/
0^ ".bt ...
brinkage. day apT3ears ,, each temper;
' ,K is netnod permits the rictsr-
08 . .. . data giving the ,,-o-ation
-^-'T. .ar^s several 'days for com-
; .
"or the attainment of
1 . V'"C".. . - c .' tests on f ar lin ; xonotl
kaylos obtained with the
arm? - 00c* *. i . ir.. quinraont are pren ted in gure V. 2. The xonotlits
.ylo oontai *e 6 ; c. ent oluysotile ... icastoo. : he individual points of the
curre ia Pi grr 7. : were obtained af:- r heat making periods of approximately
ahr. ."-hour -.-at:* Shortly ufter the micromotor dial indicated no .further
lin. sir oiia- -o at -i given temperature for about Vi-15 minutes the temperature
was lnoree.-i.-A (or ijcuauseri in returning to room temperature). This procedure
was .apeated a-'-. ;v5h ^amperaturs.
-giro - . shows that the 10 pof Berlin kaylo started to shrink
vr ; . temperatures above 400F. The shrinkages of the two sen-
i - 3
,<i 1.0 percent ah about 1200 and 1300F respectively. Tins
- -->-ure vas then decreased stepwise to room temperature, i'ho linear
3" tg during cooling ia duo simply to the thermal change of eke
a -f vb. :
sr; .i . k'.-'i
'
.
lite samples c.rr-xrc-od about 0.2 percent over the temperature 1-400?, due to us thermal change alone. At about 14003F an ' age occurred u: o"u-' i_ig to about 0.5 and 1.0 percent for the 14 densities, oceu :ict-roly. This shrinkage is caused by the . 'n of xonctlite ho ro.U.astonite (Ca0*3i035. This change is . the Tfollastcnite is such dos3 not form a hydrate. After hr is u is comp late the -.voliastonite upon subsequent increase i a 'unds thermally. The linear shrinkage represents a thermal .fs found to be reversible during alternate heating and cooling.
1 by 6 inches in siae, cut from a set of 12 different
... .ulation, representing different formulations and processing
hi r neasured for shrinkage after heat soaking at temperature
/ A" .. u ' 300 to 122';?. Those products were made with 6/2 caciss of
: 'id .
induratsf. lor periods of 1 to 1 hours set 225 pal in the
lar/-<: A
<Tinier And dried at 460 to of"?' for periods of 1 to i tears,
Till -a presented, vs i band in Figure . 3. indicating etc spread in
*h> >... 1 . -..a the host art worst perform
No correlation obtained
bet a ...
;.o and any o? eve mentioned va. lab lea. Two samples induratsc.
far :r a: >.v ,-d for 1 .r represent the pi r boundary of ths ar si. in
s " 'rso pieces of A nolatieu - uv I30 the only o ns L"1 ire
.I-
.'.ck *.;*an e.tpcx rS o:a a . Toe oed up to 1230'F. :~,3
"J ' n
due-id > itc vonson . . f excellent perf cmc-ance reun'.
r
'/
.
A.--
is . i
.. -v** ' /
. .'r). . ..
i
-Pf o-/' ; h- -
: Inc id results -i - plant produced ereciiosao of
k- ions rora hea..a --a for 24 hours prior ho
o; < - no
. with a micr ..
caliper, while still hot
at 0 .
.-'her tempers.' . ` -e samples "ndorarest the
ifa, ing
i tomperatura
. 1200F. Xks transfomati0n
, . ra .3. i up bo a temper? .
2 1800''P at which point
f 01 102 0700
Insulation block may bo taste similarly as the pipe insulation. A hot box suitable Tor temperatures up to about 2500*? has been built for suoh tests. The exposure of one surfs.ce of insulation to high temperatures has caused warpage. If the hot side shrinks, as it boos for regular plant kaylo over nearly the entire temperature range, the v;arpage of the hot surface is con cave. Xonotlite kaylo, however, shows slight convex warpage of the hot surface up to temperatures of about 1200-1400*P, and at temperature higher than this the warp age becomes conca-re due to the resulting shrinkage.
If the slab is restrained from warping, the stresses due to the linear changes are relieved by cracking. In a permanent installation such cracking is not a problem, as the cracks are relatively small and shallow. Because of this the thermal efficiency of the block is not altered.
Regular kaylo insulation block warps and cracks badly when the temperature of the hot side is in excess of 1S00F. The xonotlite kaylo performed satis factorily up to about 2000-2100?, but at the latter temperature the cracks were relatively large. In one tost of 3 weeks, 'the oold-aide temperature of a 2^ inch thick 3lab of 10 pcf xonotlite remained constant at about 210? throughout the test with the hot side at 2100?. At these high temperatures the kaylo becomes relatively weak and soft.
-13-
01 102 0761
ill. ^EliKAivILlTY TO GASES
one-dry kaylo of ZO pci density consists of about 85 percent air and 15 percent 3oiids by volume - The air spaces vrlthin the solid are both extremely numerous and very small. Because the solid consists of a network of minute fibers, i-he air spaces are continuous from boundary to boundary. Flow of gases through such a solid can occur. The amount that might pass under normal operating conditions 3xclusive of high-temperature insulation would be very email. The possible passage of air through kaylo is of no particular significance sxoeDt in insulation block in service at high temperatures. The latter con ditions would lead to the transfer of a part of the heat by convection with the affect of increasing the 2 factor.
The meet undesirable feature- of the pervious nature of kaylo is that water vapor can pats into the insulation. If the passage is from the warm to the cold side is is normally the situation, the vapor condenses if the daw point is reached in the cold aide temperature. The water so oondensed aggravates the condition further as the 2 factor increases end a lower temperature zone extends farther into tne insulation going from the cold side.
fhe only preventative against condensation is the application of a vapor seal on the warm side of the insulation so that water vapor cannot enter the insulation. The effectiveness of 3uch seal is determined by a measure of the amount of water that passes into the insulation with and without the seal. A o-craplate seal is difficult to obtain.
Tamer vapor is a gas end obeys th8 laws governing the behavior of gases. 2.0 pressure exerted by a gas is dependant on the amount or concentration of
present, hater'vapor in the atmosphere contributes a small portion of the Tubal atmosphere (barometric) pressure. The amounts of water vapor in the air v-ay very over relatively broad ranges at a given temperature. At each tem;visure the air has a certain saturation value which is expressed as 100 percent telafcive h-vaibity. The amounts smaller than those of saturation are expressed or. fio relative scale as percentages of the saturation value. As the temperature l? mcr ms-i'i -lie saturation values become higher, and equal percentage relative humidi r.-.ec X two temperatures represent different amounts of water in the air. The j.L pressures are, therefore, also different. Water vapor flows from i; Ci -, :or he lower pressures and in nearly all cases ths lower temperature reprea nts due lover vapor pressure. Accordingly, vapor barriers are applied to fo face of the insulation in contact with the higher temperature to pretout mh migration of moisture.
The unit -- ip-re3sing the amount of water in 1 cubic foot of air is ths grain. T ie -:rm 3quale 7000 grains. The amount of water vapor flowing (the romoanoa) v,*re-t y. a barrier 5.3 expressed as the number of grains of water per unit time per --lit area under a unit vapor pressure differential. Different units are rseu uni in comparing the results from different sources it is neon33ary to be certain of The unit used. The unit "perm" (abbreviated form of permeance) Vis boor? adoptsd by some writers and it means the flow of one
grain of water va-.;or per hour per square foot under ft pressure differential
of one inch of mercury.
-14-
01 102 0762
Til permeance of a material is measured by using it as a barrier between two chambers at different water vapor pressures. These ohambers generally sure also maintained at different temperatures, the more humid side being at the ...-/ter temperature. The simplest equipment consists of two air-tight compart ments separated by a wall with provisions for holding the test specimen sealed in suah manner as to prevent leakage around the edges. One compartment (on the humid si is) is provided with an atmosphere of constant humidity such as that obtaining over s. saturated solution of UaCl. This chamber may also be provided with a fun for circulating the air to facilitate the maintenance of the desired humidity. The temperature is measured by appropriately-placed thermometers and the humidity with a psychrometar, the wet bulb thermometer being placed in the air stream of the fan. The air on the dry side in the other chamber, if the temperature la above the freezing point of water, is maintained at low humidity Approaching aero by the use of a desiccant such as anhydrone. The desiccant also serves sis the collector of the water vapor passing through the specimen. The diffarence in weight of the desiccant before and after test gives the amount of -vator vapor that passed through the sample.
At temperatures below freezing the water vapor freezes on the walls of the sealed refrigeration unit. The ice carefully collected and weighed represents the amount of water passing through the sample under test.
r.'.o ibove-dsscribed equipment can be made up for different size specimens. Two models -vere used in the General Research Laboratories, one designed for > ' inch specimens and the other for full size roof tile. Data obtained on a r.r:f tile at the Engineering Experiment Station, Pennsylvania State College,
ra , _ on In a report by E. R. ^ueer covering the period of Maroh 1, 1949 to August 11, 1950.
Ein';la laboratory methods are also available for measuring the permeance nd one :f 't.3S9 known as the water or wet-cup method has been proposed as a -...C'vbivo .'.5111 standard (ASTM designation D697-42T (1946)). In this method he .'-a.rrpie is sealed in a small gla3s cylinder one inch above the level of e-i': >i' .1 usd in the bottom of the assembly. This unit is placed in a oonat-scrt-hum!dity chamber and weighed periodically. After the water loss attains i ;ucctaTt rate, the test is continued until an amount of water is lost that
,-33u;r'?le to a desired degree of accuraoy. The time required for attaining u :.a a n.udy condition will vary with the permeance of the material.
':: er relatively simple method known as the dry-cup method has been used In ' -norsi dosearoh Laboratories. In this method the specimen is sealed in a :33 tube or cylinder just above the top of anhydrone which is also sealed i : u assembly. The unit is placed into a chamber of high constant humidity
-;ain in '-eight, similar*ly as the loss in weight with the wet-cup method, u j-j 3. -.casure of the permeance of the test sample.
*'hj simple. ' To oratory methods give results subject to errors arising from ;s .recAn-ie if *.ir films at the surface of the specimens having the effect of '.ocreasing the irmeance. Forced circulation of the atmosphere above the samp :-e ij roquired ;o eliminate this difficulty and data reported on dry-cup and >ot--c:.p .oiermi-v.vbior.s ran for tests with si ch convection of air.
01 102 0763
Inasmuch as permeance decreases with increase in thickness, it is required that in presenting the data the effect of thickness he indicated. This is done by designating the exponent of the thickness. For products of definite thickness such as roof tile or KCA board, the permeance is expressed for the fixed thioknes On she other hand, it has been found that permeance increases linearly with increase in the pressure differential, the straight line passing through the origin.
In Table V. 2. are given representative data obtained on roof tile, KCA board and xonotlite kaylo by the dry-cup and wet-cup methods. In comparing the xonotlite kaylo with the Sayreville core material tested at Penn State College it is seen that the permeanoe of the xonotlite is double that of the core material at comparable densities for a thioknesa of 1 inch. As one would expeot, the permeanoe can be deoreased markedly by a vapor barrier (Harrington GIO rubber). The wet-oup method leads to a higher value of permeance (14.2 perms) than the dry-oup (12.2 perms) method in the text on roof tile.
One of the errors of tests on specimens of a single thickness is that of the combined resistance of the air paths on the two sides of the specimens.
(VIt has been found that a plot of the reciprocal of the values of permeance permeance) against the thickness, this property being designated as the resistivity, gave a straight line. Such a line did not intersect the origin of the chart, a small resistance value being indicated at zero thickness. Accordingly in evaluating the permeance of kaylo products the surface resistance (at theoretical zero thickness of speoimen) has to be evaluated by measurements on a number of specimens of different thicknesses. Thenesulting plot of l/p^meance, having the unit of fta/)ir/inch Hg/grain, against the thickness and extrapolation to zero thiokness gives the surface resistance.
The passage of water vapor into kaylo is of interest if the temperature conditions and humidities are of such values that the moisture condenses in the kaylo. For installations where 3uoh conditions may arise, the desirability of sealing the warm side against passage of vapor 1b indicated.
The permeance of air through core material was determined. The results voro jomputed as air rates for different pressure differentials and are as .follows For x thickness of 2,61 inches*
P, inches Hg
Air rate/in.a/min./ft.a
1 1.8
3 6.S
5 11.0
The porr.oar.ee a computed to be 38.5 gr. of air/kr/ft^/inch Hg for 2.61 inches of ihiohr.ass. The comparable permeance of water vapor for the same conditions <0.3 5.2 gr.
01 102 0764