Document ZJoLRQvRXOpM3MEZ3GyKRmaD0
Monsanto
E
su8JECr ;
HEF CRENCf
:
TO :
M. E. Gibbs - W1A January 16, 1976 H2S from MCS-1238
Decomposition
D. Wood - B2SD
ct- W. C. Hammann - T3A R. H. Munch - TIB
J./R
Ralph Munch has run several experiments on MCS-1238 decom position. One type of experiment involved decomposition in a sealed glass tube; the second, decomposition of a capacitor. In the first case the MCS-1238 was taken to 250C. Decomposition products included water, H2S and polysulfones. No quantitative breakdown composition was measured. However, if all the sulfur were converted to H2S, one could make the following calculation:
Assume - 1 oz in capacitor and 10' x 10' x 10' room
(28.3 gm 1238) (0.234 2E-g_,
^ g|| - 0.870 gm 2S
1000 ft3 359 ft^/lb mol = 2.79 lb mol air = 1260 gmol air
or 36,600 gm air
ppm H2S in air (by wt) =
x 106 = 23.8 ppm
An estimate of sulfur as H2S to polysulfones is about 1/10 in the experiment resulting in an estimated ppm of H_S in air in our previous calculation of 23.8/10 =2.38 ppm.
In case two when an actual capacitor was broken down, no H_S was detected. The difference between the two cases (sealed glass and actual capacitor) is the type of atmosphere exist ing during breakdown. In the case of the sealed glass, there was a reducing atmosphere, i.e., lack of oxygen; conse quently, some H2S was formed. In the case of the actual capacitor breakdown under ambient conditions, the presence of oxygen resulted in SC>2 formation instead.
Our conclusion is that H2S formation will not be a problem.
M. E. Gibbs : kl DSW 185362
STLCOPCB4051608
DSW 185363
STLCOPCB4051609