Document ZJjJ7j15qz4EDbpmaZXx921L0
1 COATINGS AS BARRIERS TO PREVENT POLYCHLORINATED BIPHENYL CONTAMINATION OF lULAGt:1'2
2
L. B. Willett, Department of Dairy Science
3 Ohio Agricultural Research and
Development Center, Wooster 44691 4
5 ABSTRACT
6 In past years polychlorinated biphenyls (PCB's) were incorporated
7 ir.t.o a coating material used on the inside of many concrete silos. These
8 residues subsequently diffuse into silages and ultimately pass into food
9 products produced by livestock that consume the PCB contaminated silage. 10 Twelve coating materials were evaluated to determine if they would form a
11 harrier to PCB residues. Coating materials were evaluated by coating PCB
12 ccnti'Mine.ted stave blocks, on test sections in a contaminated silo and on
13 dairy farm silos that were contaminated. All coatings were not evaluated
14 at all the test locations.
15 vri.cn PCI) ecni-.mi.ral.cd surfaces were treated with various barrier coat-
16 is and closed to silage, 9 of the 12 coatings significantly (P<.05) re1/ -.d the concentration of Aroclor 1254 in silage compared to silage adj.i-
18
to '. nf>.ol
faces, significant differences in the effectiveness of
,7 : `ivj i. lerials as barriers were aj.ro noted. Those coatings that v/ore
/0 carried by water or a solvent in which Aroclor 1254 i not readily r.oJn* *0,
21 . ui .-r.i'.ong the most effective coatings. Coating materials with a base coat
22 dcJifgM.d to seal the surface prior to application of the surface coating
73 ~
`` * Approved as Journal Article no. |S77^ Ohio Agricultural Research
74 <id IV.-volopiaont Center, Wooster 44691.
25 * Cin.po\t'.d in part by USUA-ARS Cooperative Agreement no. 12-14-1001- 234.
0 -U*64 HONS
i -2-
! \ wore more effective than two applications of a single formulation, llydrau2 lie cement with an acrylic bonder and water-carried epoxy effectively re-
i 3 ducod the PCD residues in silage from contaminated dai>y farm silos. The 4 resulting concentrations of PCB in the milk from cc s d these silages
5 v.Mrc below the Food and Drug Administration "temporary tolerance" level.
6 JbYKODUCYlON
7 Many silos in the Eastern half of the United States have been treated
B with a coating material that contains polychlorinated biphenyl (PCB) resi-
9 duo9. These residues appear in the silage as a result of di^bdged chips
jq from the contaminated coating and/or the PCB's from the coating being dis-
II solved by the silage juices (14). This contamination process has continued
j i -?ny years (more than 16 years observed) after the coating was <pplud
U . ..J I'.ig after all visible traces of coating were gone (10).
14 coating responsible for most; if not all the PCB contaminated
15 silos * as cvJ.Vd
Cumar wn3 formulated in 1541 and was used by
16 several silo companies until 19*0. This material
ned a mixture of
iy ect.'.r.irono-i.ndene rosins, a chloriiubod rubber, clay, the JC'.'J JUoolor li-1
;g . (r. i.vi.uto Industrial Chemical Co.,St. Louis, Mo. 63166), the polychlori-
j :.atod torphcnyl (PCY) Arodor 5460 (Monsanto) and cr.rrior solvents. Simi-
j ^.i CoMPUlatio'iS b/.vo boon ahuun ho provide excellent protection of concrete
> r.
(17). Whereas tho /'mdors were not specifically manufactured for
yf inoo*poxation into coatings (9), their xdasticixfng properties nude their
yg !, n 0v.intagi.ous (6, 11). The Aroclors comprised about 42% of the cu.ed
24 ,
%vt,. i.,r
-ing ?:i lo
`ng called "Cmiur should not U)
95 _-.if uf.rd v. th
13 e n-V-GA /.*: an h h ban * ho same name.
HONS 042865
-3-
\ Dii.wr coating.
*'
2 Consumption of silage from a PCB contaminated silo, by dairy cattle,
J lOfults in tbo deposition of PCB residues in the body adipose tissues and
4 secretion into milk via the fat (4, 6, 7). PCB residues in milk are now
$ considered a chemical adulterant, therefore, the Food and Drug Administra-
6 Mf.n in 1970 recommended an "actionable level" for milk at 5 ppm on a fat
7 lasis (8). A "temporary tolerance" of 2.5 ppm was established in 1973 (2).
0 The dairyman that has u PCB contaminated silo is confronted with a two-
9 fold economic harai.ds lbst income from unmarketable miJ.k and either elfmi-
10 nation of the residue from the silo structure or lost use of the silo,
)) Therefore, a research effort was undertaken to evaluate coating materials
12 -aid systems of application that might bo used as a barrier preventing fur-
13 ther contamination of the silage with PCB's. The principle objoctive was
)4 to offer tho dairyman a low cost alternative to the replacement of the silo
15 >:lMucturo. A preliminary report h.n been made (19).
16 l.V.TUODS AND MATEKIAJ.S
17 The coating materials were evaluated on PCB contaminated stave blocks,
j i -nt sections in a contaminated silo, and applied to existing sil03 on
12 . ;(;crn Ohio dairy farms. Twelvo coatings wore evaluated, however,
) 1 I. mi .,ot iuc1 Vd in nil of tho trials.
-.Mob domomitrated
y]
t.t,vr>i>*go >*: v.ro an 3noifo:Uvo barrier to Vho PCB rnoJdnoo wore
22 oJimino.tcd from tuboo^ucnL trials. Kow costings, with similar ptop,.iti.es
23 .*' coatings that formed good barriers, v;cre incorporated into anhse.quont
n ' l''<" >5
*; 1 ^ i'ho co.i.nyj tcri.ils, Lhotr principle u. '.'i/m
MOMS 042866
-4-
1 t v.d location of testing are shown in Table 1. The coatings that wove evalu-
2 nted in thorn studies, with the exception of VII and XIII, were selected
3 on the basis of properties which were hypothesised to form an adequate biir4 rier to PCB residues and resist the corrosive action of silage juices.
5 w<.flo hypotheses were based on the formulation of the coatings snd their
6 performance when used in other applications. All were either coswrciAlIy
7 available or currently under development for application to silos. Coatings
8 VII *nd XIII did not contain the properties thought to he necessary for a
9 good barrier to i'CB's, Lut since thc.*;e had been rc-commundod for use cn farm
10. tiiloo they were included In the trials. All coatings were applied to the
11 i TMt rurfaces to two coats, howover, with coatings I, IV,V, and IX each eppli-
13 I
iv.tl a different formulation. Kith these materials, the first coat
ij 'mo Collated for penetration and sealing of the surface while the second
14 if pilea Lion vas to provide the desired surface. Coating XI was the combi-
15 nation of a
coat of an org'/po rolvent-ono ft d v::y nd a . r.;o
16 e-pplicalJon of a \.*t.*r-caix.ied opoxy.
17 Two cur.nr-Aroclor coatings were used for .tho slave block trials. Jn
j.j ' trial 1 the finished comer coating contained 5% Arcelor 1254. Tor
? 1-...k st.ial 2 f.omo of tho actual Cvwmr ello coating vac obtained. This
g d coating contained u*>out 3PA Aroclor 1254.
;>1
!\3o
jiool&lpns. A sUo#3.^5 x 15.4 m that van built and coated
22 with r.n Aroclor 1254 containing coating in 1954,was ucod. Rock fill, l:o a
23 <1>x>th of l;22 m was placed in tho bottom to p"'\. ut b'tdi. franco C..0.1 Vcn
24 rostduos that i.My h-vo neev mtiW od in tho dirt i"1
The silo was then
25 divided L to S';von 1.22 .2,44 m t ucciJ/.-us which '.ere separated by
q486? MQNS
-5-
t-'lG. 1
y Masonite dividers (Fig. X). Chips of Masonite analyzed for PCD residues were
2 found to contain .012 ppm, Sinco this concentration is nearly tho came as
3 the lowest levels found in silage, they would not significantly influence con-
4 centrations in the silage. The test sections, with the exception of a con-
5 fcrol, wore wiro brushed to preparo a sound surfaco for coating appliestion.
^ Costings were applied at random to five sections. Tho test coatings wore
I used to seal tho junctions between the Masonite and the silo wall.
3 The silo v;as filled three tin;os co that after each filling tho rattled
9 :;ilago level was oaon with tho lep of the sections. Two fillings wm:o c-'op-
jq ped corn and one a chopped grass-logvme mixture. Sections were vertically
II T.vplod four months after each filling at 0, 60, 120, 180 and 240 cm from
p : a hnso and horizontally at 0, 15, 20, 60, and 90 cm Trom the wall.
13 Sir.v/5 block trials. Two trials were conducted on concrete silo stave
II hVcks. In ihcuo trials the stave blocks (30 x 70 cm) were treated on eno
U side with a oui*vv-va-.clor wonting,
the cntJ.'o Mock was rccoot. 1 vith
1^ the barrier coatings. The block; used in trial i nono very porous and 'he
p f.-unnr coating contained 5% Aroclor 1254, wheiouu the blocks in trial 2 voro
13 emooth surfaced end treated with 32* Aroclor 3254. Untreated blocks and
c*.c ?r-Aroclor blocks wore maintained as controls. 17 ' }j The blocks w-ro plcc\ m rud and at one stdo of polyuthylc.no
I'.'ft,2 .1 drums which vote then riP-.r.l with chopped whole corn plant and
' c-.al-/I, After standing for four months, they wore e. nplod every 25 cm
93 .Mnug the block u'td
0, 25 tnd 45 cm from the block.
9^
Dairy <* .> -llo**. Two sPou < r>:o on Mort'-r
'.i Ohio <!.**/ *' i,
./ i which hi > 'tv i '<> ho Pr;t>
Ivl, voro :.! :
Cr field I., s;U of
HONS o<,286a
-G-
1 two coating materials. Bawdies of !-')o wall scrapings, silage and milk from
2 the bulk tanks wore analyzed to verify the existence of it'B residues.
3 The first silo was built in 195? and coated with tho TCB containing
4 Cumor at that time. In 1972, this silo was cleaned by wire brush prior to
5 application of two coats of hydraulic cement plus an acrylic bonder (coating
$ VIII). This silo was subsequently filled once with a chopped grasG-l<'vt:<oc
7 mixture and then once with chopped corn. The second silo was built in 1954
3 and treated with a I'CB containing coating. In 1003 the pit and lower 2,44 m
9 of this silo ware treated with a fuivuryl alcohol rc6in coating (t-vat'".g X.) .
10 In 1972, this silo was cleaned with high pressure water (51 kg/sq cm) nd
I) coated from the base of the pit to 11.3 m above ground level with water-
12 curried epoxy (coating VI). The silo was filled once with chopped lcgi'ocs
j ill after emptying was refilled with corn silage.
SHngo rcmples were collected from the farm silos at least biweekly,
lioro fj\vj' it :;. 't pllng occurred /! ;n tho doiry.-ir n h- d to > nter tho Jlo to
^ adjust tho w:cl. ib:nl unle-cdcvs*
h compJ.o
tod .> a cow or.ito. of
]7 cil^ge collected adjacent to the v.v.l.l from tho north, >outh, cast and woct
,J s'v^s of the silo.
9 KV.t.r;ction pf si lego. All solvents used to extract silage r->npl.s
i <s / ivlyi h t\l ..x agent g-.vdo. Thr*::o wero glass oVrtillod bo : o
yy vrkjl a volume equivalent to tho
used for extraction would v'old
^2 i.o ink**. r..i.lnj pr.cVs when injected in', o '.ho gas \l<*.id chromatograph ("i t;)
>3 after to.lug '<'d;uc.d lo 1 ml and 5 }ll v/nro injected.
2^
fill-go samples ...`re w.'it.V.
13./ chopped until i*o l -.'-; : t p l ton
y vr re v.bont 1 i.<\ in .iJze. Yv.'.nty-five g
o i l ,\ . vv-i'.'icJ with ?CQ i'l
04i869
kons
-7-
1 ncetcno by mechanical shaking for 15 h. The particulate matter was thrn
2 separated by filtering through Whatman No. 1 filter paper {prewashed with 3 Water, methanol and acetone) or glass wool. The acetone extract was i.iVcn
4 up in 500 ml of 2% Na^SO^ and vigorously extracted with 200 then lr0 rl 5 petroleum ether (PE) (boiling range 30 to 60 c). The aqueous phase was
6 discarded and the M2 washed with 100 ml of 2% NaliCOj. The PE was conccn7 trated to about 10 ml on a rotary evaporator.
0 Column chromatograph/. Organic solvent extracts can be fr^ed from 9 interfering pigments (13) and many pesticides by floriuil (32) and/or rUlca
f;ol columns (1, 1G). Columns to clean the jFB extracts were prepared by
It placing 6.0 cm (7.5 g) of activated florisil (Kensington, 6S0 C activation, 12 'VI00 mesh) in the bottom of a 23 mm column fitted with glass wool in i ne
13 *
On top of this was placed 14,0 cm (26 g) of silica gel (Nathcron,
14 <\ ls i . .n & noil, gredo 023) and 2.5 cm (12 g) of anhydrous NajSO^. Oo3'\>n
15 packing r.Titortols :vo stored in r'n oven at 110 C w-ivll rued. '<'!n pi 15 columns v.vro prowashed with 100 nl of PE, the oxi/vets vc-.e applied and
d
\j they were eluted with 250 ml of 'ft V r .-.no in PE. The volume of the column
;j -ili.rtcs was reduced in vacuo oh the rotary evaporator (42 c) in propafor GI.C analysis. Care was ti-ken to avoid rout .v.t.ion ot the
, ;i*plo by rnTlux doting rotary evi^.o) ..! ion. '/I Selected o;;f.ox!:s were f;c;or.i > w.d
*2 wUli nJcohollo KOII (2.5% w/v) and extracted with H2SO4 (16 normal) by i ho ^3 I'.othod described by ronsanto 00) . ad modified as f:oW.--.:s. ; nnl w. u 24 u;;od to praparo the alcoholic avoij >. nd I'E was ua- d foe rJ.-iaoHoii*. i!\e 25 : ii'.ctrd extracts were refluxed for 45 min in 25 ml of M.ohnli.c KOIl than
HONS o<*i8?o
-8-
1 extracted 2 times with 25 ml of PE. The combined extracts were then ex-
2 traded with 25 ml of H2^4* The PE extracts were rechromatographed as pre3 vtously described. 4 Gas chromatjpgraphy. An F&M model 402 GLC with a 63Ni detector was used
5 for all analyses. A 2.44 m glass column of 4% DC-200 and 61 QF-l (ltl) on 4 Gas-Chrom Q (80/100 mesh) was used with Argon-Mothane (95i5) as carrier and
7 purge. Running conditions were* flash heater 230 C, column oven 210 c, 9 detector 300 C and gas flow 40 to 50 ml/mi n. All samples were diluted so
g that they were detected within: one linear attenuation range of the dctoclor. 10 Quantitations. Quantiatlon of the chromatograms was based on total FIG. 2 j] area under peak F through peak M (Fig. 2). Area was determined by Disc inte-
12 gj-ator. This quantitation method was used to eliminate the influence of an
13 unidentified contaminant with a short retention time* which appeared in some
14 nil age samples.
1j Corrections for method loss.\:o/.*o bused on the extraction of silage to
19 which known quantities of Aroclor 3254 were r.Oi'od. These standards ranged
17 from 0 to 2 ppm. Recoveries did not vary significantly among the various
19 types of silage.
19 Dry matter doterm* nation. The water content of the silages wero vari-
20 - Mo, therefore, the concentrations of Aroclor were expressed on a dry 2] matter basis. Silage dry matters were determined by weight loss of samples
22 oven dried for 48 h at 110 C. 23 Data Analyses. The data from the three silo trials were analysed by
24 I.oast-Squares Analysis of Variance (LSANOV) as a split-split plot model. 25 The variables of this model were the Aroclor levels in silage as Influenced
HONS 04,28 71
-91 by the fivo coat.trig treatments plus the untreated coni col unction; the hori 2 zontal and vertical sample collection positions* and .he three silo fillings. 3 The fCB values in the silage were highly variable among the various sampling 4 locations. Therefore, the data was transformed to the hog (ppm Aroclor) + 1 5 fvior to analysis. Similar LSANOV analyses were conducted for the \.v>o Meek 6 trials without transformation of the data. 7 Hartley's Sequential Range Test (15) was used to test, for significant 8 differences among treatment means. 9 fdfcWfS AND DISCUSSION 10 Relative peak areas for standard Aroclor 1254 were cseentially the sn.ne 11 .'U the Aroclor extracted from silage. Typical CLC tracings of silage ex '1C. 3 12 tracted and standard Aroclor are shown in Fig. 3. Results indicated that U 'ho microorganisms or juices in the silage did not alter or selectively exU r.act the vcocii.v rovpor.onts. These findings are confix.ned fcy the vo`k of 15 Fries (6) end Skrentny ot al. (14). Since there .\;pr;,r'd to bo no pfproci16 . bio alteration of the /t.oe.lor by the silage, and saponification plus acid 17 faction did not alter tho relationship betvioen the major poakn, tho 18 total arc-a under peak F through peak M was considered a valid quantitation i? .thod. .-0 /i.tcmpts to detect t.ho Fcf'a that v/oro al.ro a cc-^wi.ont of the O nr 21 r;ilo coating wore not made. Even 1 bough they v;r:re prolvihly extracted by 72 tl.o prneoduros that wore ynod, the J'CT's were not eluted at the maximum 23 la . p'-/.M.Ui.ofl of tho liquid pho:;o of tho GbC column (5). 24 Tho average ppm of Aroclor 1254 in silage from I he th> ,e silo I rials 75 and two block trials are shown in Fig. 3, F.?tch b>r of the histograms re-
mqns 042872
-10 1 preronls the average Aroclor 3 254 concentration of all rumples analyzed re-
2 presenting all sampling locations. The comparisons of significant differ-
TABLE
3 encos among means are shown in Table 2. * Generally speaking, all of the coatings that were hypothesized Co form 5 * nii:i:s to PCB residues did so when evaluated on the silo test. sections
6 and/or stave blocks. The two commercial coatings that did not have propor-
7 tics predicted to be necessary for a good PCB barrier were indeed ineffee**
8 tivo when tested. The LSANOV for the silo and block trials indicated that
9 the concentration of Aroclor 1254 In the silage was significantly (P<.01) 10 affected by coating treatments.
11 r,)ic coatings applied to the silo sections greatly reduced the PCB con-
12 ofntration when compared to the untreated control section, and significant
13 d\fTerences were observed between the individual coatings (Table 2). All 14 of ;.ho coatings adhered well to the silo wall. With the exception of the
15 water-carried epoxy in coating XI, coverage was good. This water*carried
16 ipoxy did not provide desirable coverage over the thinly
rolvcot-
17 carried epoxy. The thickness of cov:.tJ.nys I, XT, and V was about Lho uv'me 18 ; \ ranged from .01 to .09 cm. Tho hydraulic cement material (vi7.D pro-
19 . i*3*id a very thick coating ranging between .35 and . 72 cm. A film thlck 0 could not Lo determined Tor coating XI.
2),, s results of tho silo trials (rig. 3) suggested that tho solvent used to
22 o.ny tho coating materials may influence effectiveness of the coating. I 73 T .odor 12'>4 has been shown to be readily dissolved in tho methyl isobutyl
74 ketone (MlhK), ccllosolve and xylene which are found in coatings II, V, ond 25 XI (9>. The Aroclor has low solubility in isopropanol used in coating I
HONS 042373
-111 .id Is inrolublo in tho water used to rArry coal: \ ng VHI. Tn contrast, ^ coalings IV, V and XI with M1BK, collorolvo and xylino re-poolivoly, r- iO 3 the most effective barriers when evaluated on tho stave Mwkd {i'1;. A 3). 3 The coatings Maintained their relative effc-ctivt.-ncihj throughout the 6 throe silo trials. There were no significant differences (P>.05) between 7 the three silages tooted, indicating that different typos' of silage had no 8 effect on tho levels of Aroclor in silr.go nor did the harriers become less 9 effective with continued usage, 10 Vho levels of Aroclor 1254 in tho silages from block trial 1 vcrQ ton11 'd.r'.bly lover than in either block trial 2 or in the silo (Fig. 3). This 12 . - cbuhly resulted from the lower concentration of Aroclor 1254 in tho cvnar 13 NK'i-.g and porous surfaces of the blocks of trial 1. Tho porous surface 14 1by...d tho cui.ar-Aroclor to penetrate, thus reducing tho .mount of Ayncior 15 that was in close contact with tho barrier coating and silage. 16 This experiment indicated that a coating that contains a solvent In \) ' hioh Aroclor is v^ry soluble (9) should not be m;od. Coating VII c-.nta'n13 od k-.'rosvnO which resulted in significantly greater contamination of tho 19 r.n. -.'jO t han did tho fmt.iar-Aroclor control, /0 'il.c si ago of two- co: pontnt coating systems v..n : hov n <n tho ht i.k 21 Ir lals. Tn Mu-so studies a two-component coating system utilized a nvlii'bd 22 foui-ul.ition to servo as a scaling bnr;o coat. Then tho second component of >3 -M.iilor material formed the coating surface. Coatings I, IV, V and IX '.\'o 24 all two-component systems. These materials, with tho exception of coating 25 I, \;i'o .morig tho iost offective in this trial (Fig. 3). Coatings II and
MONS 042874
-12-
1 XTI wore two oppl (cations of the single-component equivalents of coat ings
? IV ami IX, x cnpocl.i \ ely. The two-ec. 4`oncnt ryi-i
wore significantly (l'
3 <.05) nore effective than the single ccopoiH.at fo> mui *.1 Ion of the jiuk.q
4 material (Table 2).
5 Coating I was not an effective barrier to the bCB residues nor did it
6 form the desired smooth surface in block trial 1. The surface of the cont-
7. ing was not smooth and solid as it subsequently appeared to be on the silo
8 wall and in the second block trial. It was suspected that improper formu-
9 lalion or application was responsible. 10 In block trial 2, three water-carried systems, two dual-component sys-
11 tens and a commercial silo coating were evaluated on relatively nonporous
12 rtave blocks. Coatings I, IV, VI, VII and XII significantly (P<.05) re-
13 >V.\ced the Aroclor 1254 residue in the silages. There were no significant
14 differences among those coatings (Table 2). The commercial coating XIII
15 was not significantly different from the untreated control. This coating
15 was softened by the silage juices, and consequently did not form an adequate
1/ '.nrior to the PCB residues. 10 Coatings I, IV, VI, and XIII showed signs of physical failure when ex-
19 ..mir.od at tho end of this trial. Those coatings cracked or. blistered in.U-
20 c.-J ihg that they wro unable to l.ond to a smooth Curnr surface. This 1-\di-
21 caked that these coatings should only be used on silos that no longer have
22 a solid and intact Cvir.ar finish. 23 The Aroclor 1254 concentration of silage was significantly U'<.01) in-
24 flucnccd by the distance from the silo wall or the stave block, significant
25 (P<.01) linear and quadratic effects were also noted within the silo.
MQNS 04^875
-13-
t' H'i. 4
1 Figm-o 4 shows tho average distribution of Aroclor from the silo test acc2 Hons. Tho average from all sections was used.
3 This distribution was as expected since the mechanism by which the
4 residues migrated was probably diffusion. These results agree with those
5 of Skrontny et al. (14) with the exception that beyond 15 cm from the silo
6 walli higher levels were detected in this study. This may only reflect silo
7 and methodology differences. Also, these workers (14) did not state
8 whether Aroclor levels of silages were on a wet or dry matter basis.
9 Concentrations of Aroclor were significantly (P<.05) higher near the 10 base of the silo test sections. This may be the result of the downward 11 leaching of the silage juices. Leaching would deposit the PCB residues 12 near the base of the silo. This effect was not observed in the drum ex13 poiinonts. The drums were sealed and contained a relatively small volume 14 of silage, thus extensive leaching would not be expected. 13 Based on the results of the silo and block trials and commercial a16 vailability, hydraulic cement (VIII) and water-carried epoxy (VI) were 19 selected for use on two dairy farm silos. Both silos wore known to contain 18 sufficient PCB's to cause the residue level in tho herd milk to exceed .2 l? jpm. The histories and preparations of the silos was previously described 20 (p.jgc 5). Concentrations (ppm) of Aroclor 1254 in scraping of the silo 2J vails and in silage before and after recoating are shown in Table 3. 22 Concentrations of Aroclor were extremely high both in wall scrapings 23 and silage near the base of silo 1. Unfortunately, this silo was nearly 24 empty when located for experimentation so only limited precoating data was 25 available. The concentrations observed near the base may not be repre-
MQNS 042676
'
I ! j ! :
-141 scnlative of the entire silo as the residues may have accumulated near the 2 base, as a result of downward leaching of silage juice. However, the high 3 concentration of Aroclor residue {>.6 ppm) present in the milk produced on 4 that farm Indicated that the cows had been consuming considerable quanti5 ties of PCB. 6 The hydraulic cement coating VIII that was applied to this silo, after 7 thoroughly cleaning the walls with a wire brush, provided an effective barS rier between the contaminated silo wall and the silage (Table 3). The con9 centration of Aroclor 1254 did not reach .5 ppm during the two trials and 10 the PCB residue In milk continually declined throughout the experiment. n
After three fillings of silage there has been no indication of failure of 12 the coating. 13 The base of silo 2 had been coated by the owner with a furfuryl alco14 hoi resin coating (I) prior to the discovery of the PCB contamination. The 15 concentrations in scrapings of and silage adjacent to this recoated area 16 were considerably less than similar samples collected above the coated area 17 (Table 3). 16 The entire silo was cleaned with high pressure water (51 kg/sq cm) 19 then recoated to tho 11.3 m level with the water-carried epoxy (VI). The 30 luvols of PCB in the silage collected above the rocoatod area were high 31 (Table 3). However, the residues were significantly reduced when collected 22 adjacent to the surfaces coated with the water-carried epoxy. The high PCB 23 concentrations observed near the top of the coated area probably resulted 34 from settling of the silage and the downward leaching of the silage juice. 35 As observed with silo 1 no failure of the coating was evident after two trials.
HONS 042877
-151 GKNI'UAIj discussion 2 Tho results of those experiments with barrier coatings have domonstra9 ted that a number of coating materials will form an effective barrier to 4 prevent significant PCB contamination of silage. Two coatings Win and VI) 5 have beon shown to provide sufficient protection of the silage when used on 6 PCB contaminated silos that were in use on dairy farms. Based on the experi7 mental tests one would expect similar results could be achieved with some 8 of the other coatings that wore tested. The vinyl coatings (II# IX) and the 9 organic solvent-*carried epoxy coatings (IV,V) were shown to provide a bar10 rler to the PCB residues# but the organic solvents used as carriers may re11 duce their effectiveness as compared to the water-carried systems. Coating 12 I was effective in the silo trials# block trial 2 and remained as a bar13 rier five years after application to the base of silo 2. Coating XII was 14 a water-carried epoxy similar to VI, therefore, may form a successful bar15 rier to PCB's in a farm silo. 16 With the exception of block trial 2, all of the coatings were evalu17 ated on a rough surface. In these trials the bonding of the materials to 18 the surface was good. The poor bonding that was observed on the smooth 19 blocks in trial 2 suggests that barrier coatings may fail to provide an 20 adequate protective barrier in silos having an intact smooth Cumar coating. 21 Likewise# bonding problems should be anticipated on silos that had been wax 22 treated or wore improperly cleaned prior to recoatlng. 23 Results of these studies have indicated that PCB contaminated silos 24 can be effectively decorjpminatcd by the application of a barrier coating. 25 The cost of decontamination (labor and materials) ranges from 10 to 18% of
CINS 0428 78
161 the silo replacement cost. Thus, on silos with sound porous surfaces, re2 coating is a practical alternative to the total replacement of the silo 3 structure. 4 Careful selection of a coating material is advised. The components of 5 certain commercial coatings are not approved by the Food and Drug Adminis6 tration for use in livestock food storage containers. Likewise, use of 7 some coatings, particularly those that contain organic solvents, cannot be 6 used in certain areas as they will not meet air quality standards or occu9 patlonal health standards during application. 10 The effective life span for a barrier coating has not been determined U at this time. Continued observation of recoated silos will eventually pro12 vide this information. Some silo coatings have remained intact for as long 13 as 10 years when used to seal the inner surfaces of silos. It should be 14 emphasised that the effective life span of a barrier coating will be great,5 ly reduced if the silo surface is improperly cleaned and prepared prior to 16 recoatlng. 17 ACKNOWLEDGEMENTS 19 The author is grateful for the technical assistance provided by T. L. 19 Ayres, B. B. Beam, C. J. Brunvn, C. F. Stellwagon and S. L. Welty. 20 This research was partially supported by gifts from Action*. Plastic 21 Inc., Monsanto industrial Chemicals and Ohio Milk Producers Federation. 22" Tochnical and material support was provided by Standard Dry Wall Inc., and 23 Universal Cooperatives. 24 2$
MOMS 042879
-17t REFERENCES 7 (1) Armour, J. A., and J. A. Burke. 1970. Method for separating poly 3 chlorinated biphenyls from DDT and Its analogs. J. Ass. Offlc. Anal. 4 Chem., 53i761. 5 (2) Department of Health, Education and Welfare, Food and Drug Administration. 6 1973. Polychlorinated biphenyls. Federal Register, 38 (291:18096. 7 (3) Fries, C. F. 1972. Degradation of chlorinated hydrocarbons under S anaerobic conditions. Adv. In Chem., Ser. 111:256. 9 (4) Fries, 0. F. 1972. Polychlorinated biphenyl residues in milk of en 10 vironmentally and experimentally contaminated cows. Environ. Health 11 Perspectives, 1:55. 12 (5) Fries, G. F., and G. S. Marrow. 1972. Polychlorinated terphenyls as 13 potential contaminants of animal products. Presented at AOAC Meeting, 14 Washington, D. C. 10-10-1972. 15 (6) Fries, G. F., G. S. Marrow, Jr., and C. H. Gordon. 1971. Similarity 15 in behavior of DDE and polychlorinated biphenyl (Aroclor 1254) resi 17 dues in an environmentally contaminated herd of dairy cows. J. Dairy 18 Scl., 54:796. (Abstr.) 19 (7) Fries, G. F., G. S. Marrow, Jr., and C. H. Gordon. 1972. Similarity 20 of a polychlorinated biphenyl (Aroclor 1254) and DDE in rate of 21 elimination from cows. Bull. Environ. Contamin. Toxicol., 7:252. 22 (B) Kolbye, A. C. Jr. 1972. Food exposures to polychlorinated biphenyls. 73 Environ. Health Perspectives, 1:85. 24 (9) Monsanto, (Undated Report). Aroclor Plasticizers, Monsanto Industrial 25 Chemical Co. Tech. Bull. 0/PL-306A.
MONS 042880
101 (10) Monsanto Industrial Chemical Co. 1971. Monsanto Methodology for 3 Aroclor, Analytical Chemistry Method, 71-35. 3 (11) Nisbet, 1. C. T., aid A. F, Sarofim. 1972. Rates and routes of trans 4 port of PCB's in the environment. Environ. Health Perspectives, 1:21. 5 (12) Reynolds, L. M. 1969. Polychlorobiphenyls (PCB's) and their inter ference with pesticide residue analysis. Bull. Environ. Contamin. 7 Toxicol., 4:128. e in) Rote, J. W., and P. G. Murphy. 1971. a method for the quantitation of polychlorinated biphenyl (PCB) isomers. Bull. Environ. Contamin. 10 Toxicol., 6:377 . 11 (14) Skrentny, R. F., R. W. Hemken, and H. W. Dorough. 1971. Silo seal 13 ants as a source of polychlorinated biphenyl (PCB) contamination of 13 animal feed. Bull. Environ. Contamin. Toxicol., 6:409. 14 (15) Snedecor, G. W. 1956. Statistical Methods. Sth Ed. Iowa State Univ. 15 Press, Ames. p. 253. 15 (16) Snyder, D., and R. Reinert. 1971. Rapid separation of polychlorinated 17 biphenyls from DDT and its analogues on silica gel. Bull. Environ. 18 Contamin. Toxicol., 6:365. 19 (17) Sproul, J. R. 1941* Acid-resistant concrete coatings. Ag. Eng., 22i 90 209. 21 (16) Willett, L. B. 1973. Docs your silo contain PCD residues? Hoard's 22 Dairyman, 110:610. 23 (19) Willett, L. B., and H. R. Conrad. 1973. Coatings as protective barriers 34 to polychlorinated biphenyl residues in contaminated silos. J. Dairy 35 Sci., 56:669. (Abstr.)
mons 042881
TAMF 1. The identification, principle components, principle solvents and test locations of the barrier coatings tested.
Coating Numeral
Coating ____ Type_____
Principle Component*?
Principle Solvent?
inhere .Tested ~ Farm
Silo Block Silo
Name
I
Furfuryl1
Furfuryl
Isopropanol
x
X
2 Silenzcrete
alcohol resin
II
Vinyl
Vinyl resin
MIBK7
XX
111
Epoxy
Epoxy resin
Xylene
X
IV
Epoxy1
Epoxy resin
Xylene
X
V
Epoxy1
Epoxy resin
Cellosolve X X
Monolite E* poxy2 2 Epoxy 4 800-909
VI
Water epoxy
Epoxy resin
Water
XX
009*
VII
Thermoplastic
Alkyl aeromatic
Kerosene
X
Type"0"6
hydrocarbon
hydrocarbon
VIII IX
Hydraulic cement
Vinyl1
Cement + acrylic
Vinyl resin
Water MJBK7
X XX X
Thoroseal9 Monolite7
X
CONTROL
Cumar-Aroclor
Mineral
spirits or
Xylol
XX
XI1
xjix
Epoxy + Water epoxy
Epoxy filler
Phenolio resin
Epoxy resin
Epoxy resin Amherol
Xylene Water
Water
Xeopropanol Methanol
X
X X
Epoxy2' 3 Watorpoxy Block filler'
.4C Sealer6
1 Two component coating system 2 Universal Cooperatives, Alliance, Ohio
3 General Hills Chemicals Co., Minneapolis, Minnesota
4 Action Plastic, Inc., Charlotte, Michigan * Standard Dry Wall, Inc., Miami, Florida
* Whllleker Corp., Wooster, Ohio 7 Methyl Isobutyl Xetone
A
The use of trade names is only to Identify the products used. The use of trade names is not an endorsement of the products used nor meant to discriminate against similar products not used.
9 As stated by the manufacturer.
TAPI.E 2. The comparison of differences in mean concentrations of Aroclor 1254 in silages
from the barrier coating trials. Significant differences vere determined by Hartley's
Sequential RangeTeet.__ ____ ___ ___ ___ ____
COATING NUMERAL
Coating
Numeral
Trial
X
II III IV V
VI VII VIII IX X
XI xn xii:
Silo 1 Block X
Block 2
< <
>*> nsc > > >
<
ns ns
< << > > ns ns < ns
<
Silo
>
XX Block 1 <
Block 2
ns ns < ns < ns ns > < > > <
Silo in Block 1 ns >
Block 2
> > > < > > ns
Silo
XV
Block X <
ns <
Block 2 ns
ns < ns
<
ns ns < ns <
ns <
Silo
> ns
V
Block X <
ns <
ns
Block 2
> ns < ns < < > ><
Silo
VI
Block 1 < < <
>>
Block 2 ns
ns
< > >< ns <
ns <
VIX VIII
Silo Block 1 > > >
Block 2
>>>
> >>
Silo Block 1
> <
ns <<
Block 2 ns
<
ns <
<
<
ns ns
<< ns <
< ns
<
silo
XX
Block 1 < < <
ns <
<
<
ns
Block 2
<
Silo
>>
>
>
X Block 1 ns > ns > > > < > >
Block 2 >
>>
> >
ns
Silo
> ns
XI Block 1
Block 2
silo XIX Block 1
Block 2 ns
ns ns ns
><
HONS 042883
ns <
<
XIIX
_____
Silo Block 1 Block 2
> _... ____
>
-_ > ____
>
___ ns --
FOOTNOTES FOR TABLE 2 a Coaling on vertical axis is significantly more effective than (P<.05) coating on horizontal axis. k Coating on vertical axis is significantly less effective than (P<;05) coating on horizontal axis. c Coating effectiveness is not significantly (P>.05) different.
MQNS 042884
TA3LE 3. Level of PCB (pfm Aroclox 12b4) in silage and silo wall surfaces collected before and after recoating.
Level silage collected
(m)
13.7 15. ? 10-7 10.1
9.1 6.2 7.6 6.1 5.2 4.6 3.7 .3.1 2.1 1.5 0.3 0.0 -0.6
Scrapings before recoating
(PE*>
20155.00
Silo la Silage before recosting
(ppm)
103. OO"3 7131.88
Silage after reCCAtlrig
Trial 1
Trial 2
(pp>
(ppo)
0.013
0.06
0.013
o.os
0.08 0.27
0.38 0.42 0.24
0.29
0.07 0.02 0.07 0.08 0.10 0.11 0.16 0.10 0.11 0.07
Scrapings before recoating
(ppm)
314.02 175.37 705.27 --
4.90 ' 3.60
Silo 2b Silage before recoating
(ppm)
5.11 8.04
0.99 0.03
Silage after recoatinq
Trial 1
Trial 2
(ppm)
(ppm)
20.68 58.98 28.80
1.91 0.85
1.06 1.00
13.43 18.23
1.31 0.69 0.40 0.62 0.62
0.50
0.86 0.61 0.35
0.98 0.86 0.48
0.48 1.56
1.19
X to
Q * N CD CD
* Silo was coated with hydraulic cement with an acrylic bonder (coating 1).
h silo was coated with water-carried epoxy from the base of the pit to 11,3 m above the ground (coating VI).
c Sampled adjacent to the silo wall.
^ This sample was a blend, not adjacent to the silo wall.
FIG. 1. Dividers made of Masonite were used to separate the coating test sections in a PCB contaminated silo. The test coatings were used to coal the junctions between the Masonite and the silo wall.
HONS 042886
9 9 7 * 0 SNOW
ri'j. 2. Typica. chromatograms of standard Aroc'or .ITAd /w and Arocior 125d extracted from silage (A). Quantitations were b. >ed on the total areas of pea^s ihrctgh
14
1 SilO
10p
B
6
4
2 0
i B B -Djfl
x v xi n vm i
2 04f
BLOCK TRIAL I
i BBInnnn
V|| ' S' X VI It V IV IX VIII
FIG. 3. Average concentrations (ppm) of Aroclor 1254 In silage from the various barrier coatings test locations. Each bar of the histograms represents the average from all sampling locations. The X Is the un treated control section in the silo and the Aroclor-cumar coatings In the block trials.
HONS 0*2888
9
cs r
a
O
4
V
6-
O s'-.'i
<
V. o
ft.
r.
j! jl.
i" i i
l'
o 30 60 90 no
CM . .?OM 5110 WALL
r <;. <J. <?> -t ..\\ f..vi4.*ivj
*, V\.
],or<
>1 r.
ib*;ticr of .* tr' or
?-;h h*r
t.:.o Mi-i.tfj-rAir. r v;.r - ''.'`is the
i.m/..'ol factions.
in tV.-j
MONS 042889