Document V3qK9om4O2ZynQDQ5XYwexBj8
TOWOLDMONOQ38557
TOWOLDMONOQ38558
^fic/iewo/td
This booklet is prepared for the purpose of setting forth the essential characteristics of certain plasticizers and resins made bv Monsanto Chemical Company. On account of the diversity of basic raw materials used as plastics and the almost unlimited uses of the finished articles, it is obvious that there is not likely to be a uni versal plasticizer. A knowledge of the properties imparted by each of several plasticizers, however, gives a working basis for selecting the right one for any par ticular purpose or making the correct combinations. We believe that the data and suggestions presented here will enable the manufacturer of articles requiring these products to make a proper selection with a mini mum of time and testing.
:* Ubl^l
TOWOLDMONOQ38559
General...............
Page ..................................... ................ 5
Suggested Uses for Plasticizers.........................
.. 6-9
The Phogphateg......
.........................
Tricresyl Phosphate
...............
Specific Gravity (Graph)....
.........
Vapor Pressure (Graph)............................
Triphenyl Phosphate....
10-13
10-12 ....... 29
..... 30 12-13
The Santicizers............
.......................
14-22
Santicizer 3 Santicizer 8 ..........
...........................
14 13-16
Softening Effect on Shellac of Santicizers
8 and 9 (Graph)
.......................
Santicizer 9
............
Santicizer 10
....................
Santicizer E-15
...................
Santicizer B-16 .
16 17 18 18-19 20-21
Santicizer M-17......
21-22
Vapor Pressure-Phthalyl decollates (Graph) 31
General Data....
Flash Points (Chari).. Viscosites and Pour Points (Chart) . Solubility of Liquid Plasticizers (Chart) Solubility of Solid Plasticizers (Chart) . Solubility of Waxes and Resins (Chart) . Suggested Plasticizer Applications (Chart) Table of Characteristics .
The Santolites General Properties Santolite MS . Santolite MS-Butyl Acetate Santolite MHP................... Santolite K....... Santolite K-5 ................. Solubility (Chart)..... Table of Characteristics (Chart)
Par
^ % 37 3K 3't UMI C-G
It-111 tt-l*>
U t-- If*
t< 16-17
t. IK 13
The Phthalates....
Dimethvl Phthalate..................... Specific Gravity (Graph)
Diethyl Phthalate .....
Dibutvl Phthalate Specific Gravity (Graph)... Vapor Pressure-Phthalates (Graph) .
Diphenyl Phthalate
.
Hii-40
Ortbo-Nitrobiphenyl Vapor Pressure (Graph)............ .......................
23-26 23 32
....21 ) .33 31 26
.26-27
27-23 .33
The Aroclors .
16-'>'i
General Properties
I'1
Physical Properties (Chart) .
Chlorine Content of Pure Compounds (("hart)
Specific Volume of Aroclor 1248 (Graph)
Compatibilities with Plastics
32
Solubilities (Chart)............
3
Lacquer Composition Diagrams
.'>t-V>
Vapor Pressures (Graph)..
36
Suggested Uses.........
37-3'*
Densitv of Aroclor 1248 (Graph)
4 06U A22
TOWOLDMONOQ38560
General
( >IIuI<m` dcri\ <iti \ e. and practically all resins, both s\ ntlutie ami natural. haye a brittleness which increases will) ape1. To counteract this characteristic, as well as to give workability and flexibility, and to overcome shrinking which causes cracking and shattering, plas ticizers arc added.
Plasticizers came into particular prominence with the development of pyroxylin and the subsequent growth of the lacquer and molded synthetic products indus tries. Camphor was the first satisfactory plasticizer, and it was its use with nitrocellulose that made cellu loid and molded pyroxylin articles possible. On account of the fire hazard involved in the use of articles made of nitrocellulose, a fire retarder was necessary, and Trieresyl Phosphate came to play that role. In spite of numberless attempts to produce other compounds for the purpose, Trieres\l Phosphate still retains its place, although with improvements in nitrocellulose stabiliza tion it is not as essential in most compositions as lorinerh.
Alter the \\ orld \\ ar, the availability of large stocks of butv 1 alcohol and a process for making phthalic anhy dride cheaply, opened the way for Dibutyl Phthalate as a component of the new nitrorellulose lacquers just becoming so important. The combination of Trioresyl I'hosphate ami Dibutyl Phthalate was quite satisfac tory until a host of new molding and coating materials, composed largely of synthetic resins, were developed a"d requirements became much more exacting. These ''impositions required new plasticizers, or to be more 1 'll,, t. properties not imparted by the older plasticizers, hstrcinc light stability, water resistance, grease resistai"e, non-toxicity, greater compatibility with special r,'Miis, gloss, smoothness of working, flexibility at low ''mperatures. non-softening at high temperatures, stabilit\ toward acids and alkalies, and numerous other
properties were demanded. Cellulose acetate came actively into the plastic field and required entirely new plasticizers because, while most of the compounds pro posed were compatible with nitrocellulose, very few were sufficiently so with acetate. Thus, for Tricresyl Phosphate, which is not at all compatible with acetate, must be substituted Triphenvl Phosphate which has good compatibility. Dibutyl Phthalate is not com patible in amounts sufficient to give the desired proper ties, and therefore Dimethyl Phthalate and Diethvl Phthalate, in spite of relatively high evaporation rate*, were used.
Plasticizers are required to impart such a multiplicity of properties that it is not reasonable to expect any one of them to do everything. We often recommend that mixtures of several plasticizers be used, selecting the components of the mixture on the basis of the physical and chemical properties of each plasticizer. But this means one can frequently make use of the excellent properties of a relatively incompatible plasticizer, which by itself would be unusable.
Monsanto Chemical Company is prepared to supply a line of plasticizers covering most of the essential require ments. Standard products of proven value have been selected and additional ones developed to fit those requirements not fulfilled bv the older materials. In all those products the usual high standard of quality of Monsanto products is maintained.
The requirements for resins are as exacting as for plasticizers. Two important factors in many specialty combinations are compatibility with cellulose acetate and lack of color. The Santolite resins possess both these features, as well as manv others which make them outstanding in the resin field.
. Obi'll
TOWOLDMONOQ38561
Suggested Uses for Plasticizers
Acrylic Type Resins
Dibutyl Phtbalate and Santicizer B-16 are recom mended. The solid plasticizers produce less softening effect but also less flexibility.
Alkyd Resins
Santicizers B-16, -15 and M-17 are recommended as plasticizers in amounts of from 5% to 40% of the resin. Tricresyl Phosphate and Dibutyl Phthalate may also be used. Ortho-Nitrobiphenyl may be used in alkyd resin varnishes in amounts up to 10% without effect upon the drying time. The Santolites are of value for increasing moisture resistance and compatibility in lacquers. The Aroclors are compatible with alkyd resins and can be used in conjunction with them for lacquers, varnishes and enamels.
Benzyl Cellulose
Diphenyl Phthalate is recommended. Santicizers B-16 and E-15 and Tricresyl Phosphate are also excellent for many purposes. 25 PHR* are sufficient for normal purposes.
The Aroclors are compatible and aid alkali resistance and reduce moisture and gas permeability. The liquid and soft resinous Aroclors give greatest flexibility.
Cellulose Acetate
Dimethyl Phthalate, Diethyl Phthalate, Ortho-Nitrobiphcnyl, Triphenyl Phosphate, Santicizers 3, 8, 10, M-17, E-15 and, for some types of acetate, B-16, are all of value.
Dimethyl Phthalate and Diethyl Phthalate produce great flexibility and are relatively cheap. A rather high evaporation rate and poor moisture resistance are the chief defects.
*P1IR = parts per 100 parts resin.
*
Ortbo-Nitrobiphenyl is very compatible and give* cle*r workable compositions of good flexibility.
Triphenyl Phosphate provides non-flammability (ftm. with 20 parts per 100 of acetate will not support com. bustion) and produces firm, flexible films of high tensile strength.
Santicizer 8 produces tough, flexible compositions of high gloss and smooth working properties. It* fight stability is better than Triphenyl Phosphate but not equal to the phthalate derivatives.
Santicizers M-17 and E-15 give products of high qualm as regards all characteristics. They do not affect th> burning rate. These plasticizers are recommended over most other compounds for general use. M-17 is a better solvent than E-15 for cellulose acetate.
Santicizer B-16 is not a solvent for cellulose acetate and its retentivity varies over a wide range, being greaie-i with the more highly acetylated acetates. Although not recommended for general acetate work its 1**"' bilities should not be overlooked when the me of * permanent, light-stable, water-insoluble, alkah-re-i-i ant, odorless and tasteless plasticizer is required.
The Santolites are especially valuable in cellul"1 acetate compositions, adding gloss, adhesion and 11,01 ture resistance. They should be used with pla^H'1/1 r to produce flexibility, Santolite K requiring tin I'3 amount of plasticizer. The Aroclors are of little value in cellulose acta because of their low compatibility.
Cellulose Acetobutyrate
Dibutyl Phthalate, Tricresyl Phosphate and Shu*' ^ 10, B-16, E-15 and M-17 and Ortho-Nitrolip|lfn' ^
all efficient plasticizers. Suitability will depend 1^
the intended use of the finished goods. About of plasticizer (by weight) to 100 parts of the a< et
^
rate is usually required.
6
TOWOLDMONOQ38562
IVlInloM' Aoelopropionate i/i'i' 8. -1 o. and M-17 and Ortho-Nitrobiphenyl
arr rcnmimcndcd. Triphenyl and Tricresyl Phosphates, | )il>iii \ 1 Phthalate and the Aroolors are also useful.
Chlorinated llublier
Samicizers 11*16. L-15 and M*17 have special merit. Santieizer 11*16 increases the adhesion and is usually jiudvrrcd. although Santieizer M-17 produces greater (lc\ihilih and is not affected by petroleum hydroear* I >< hi-. 1 roin 5 to 25 PI IK arc suggested although more 'an In used, the retentivit) of Santieizer M-17 being altnufi 200 PHK in chlorinated rubber.
I lie Aroclors -both liquid and solid--are valuable for pi' ing a 'vide range of properties between flexibility and liauhios. Aroelor 1260 is recommended for flexibility and toiiglmess combined with water and alkali resistan'1. I sually from 20 to 50 parts of Aroelor to 100 ['an,, of chlorinated rubber are required. The Aroclors ar< ojiccially useful where alkali resistance is desired.
Natural llestns
DAMAR--Diphenyl Phthalate in amounts from 5 to 25 parts per 100 of damar is recommended.
KAURI--Santieizer B-16 and Dibutvl Phthalate are suggested.
MANILA--Santieizer K-15 and Dibutyl Phthalate are suggested.
ROSIN - -Tricresyl Phosphate. Santieizer 11-16 and the Aroclors are suggested.
SHELLAC--SanticizersS, 9 and 13*16are recommended. Santieizer 8 produces great flexibility but softens the shellac. Santieizer 9 produces harder compositions. 10 parts of Santieizer 8 per 100 of shellac produces about the same degree of softness as 30 parts of Santieizer (). Neither affects the heat curing of the shellar.
Santieizer 8 is best for mixing into melted shellar but where solutions are used. Santieizer B*16 has about the same efficiency.
*
K,|i vl Cellulose
'"Uin/er M-l, produces maximum flexibility. Amounts *d",'i ,.> PIIK produce taekv compositions. Santieizer ' '1116 and 8, Dibutyl Phthalate, Tricresyl and I ripheny | Phosphates. Ortho-Nitrobiphenvl. and 1111-
an' all of a alue.
Santolit,. resins produce flexible, tough eomposill"|i- of cM-ellcM properties.
\rt>e)ors arc very compatible and afford a means of
^'ainini; an\ desired degree of flexibility or hardness.
I Aroclors, such as 1242, produce great flexi-
^ | ,'u' bard, resinous Aroclors, such as 5460,
* ' hard compositions of unusual weathering
Qualities Tt, . ,
.
]' Ilc Aroclors are highly recommended for
fi good water resistance, gloss, alkaliu flexibility, adhesion and weathering qualities.
Neoprene
From 10% to 25% of Aroelor 1270 acts as a flame retarder when milled into Neoprene.
Nitrocellulose
Tricresyl Phosphate is recommended for fire retarding and also imparts good flexibility, permanence, tough ness and water resistance.
Dibutvl Phthalate and Santicizers 11-16, K*15 and M-17 are best for color stability, high flexibility and practi cally all properties except fire retardation. Santieizer 13-16 gives the greatest film strength and Santieizer M-17 the greatest flexibility. Dibutvl Phthalate is a low-eost, general purpose plasticizer. Santieizer 8 produces high flexibility, gloss, brilliance and smooth working qualities in lacquers. Its color
0614425
TOWOLDMONOQ38563
stability is of tin* same order as that of Tricresvl Phosphate.
Santicizer 10 and Diphenyl Phthalate impart water resistance and gloss. They produce hard compositions when used alone, so arc most frequently used in combi* nation with other plasticizers or resins to aid flexibility.
Ortho-Nitrobiphenvl produces results similar to cam phor. in molded plastics it may be used alone, or with camphor or camphor oil. In lacquers it produces hard, tough, resistant compositions and seems to aid solvent release.
The Aroelors act both as plasticizers and resins in nitrocellulose lacquers. Compatibility decreases as. the chlorine content of the Aroclor increases. Aroelors 1212, 1231, 1260 and 5142 are most suitable and aid water resistance, adhesion, gloss and reduce the burn ing rate. They reduce gas permeability and tend to eliminate "corona" effect when used in high tension cable coatings. The Aroelors yellow somewhat in ultra violet light.
The Santolite resins are valuable in all lacquers not intended for severe exposure to weathering. They are highh compatible, produce solutions of low viscosity ami impart high gloss, good flow and moisture resistance and are essentially colorless. Thev may be used with any of the plasticizers, either liquid or solid. Amounts of Santolite MHP suggested are up to a weight equal to the nitrocellulose, and the quantity of plasticizer for such mixtures will he the same as that required if the Santolite were not present. Santolite K gives more water resistance than the other Santolites and produces some flexibility of itself.
The Santolite resins, like the sulfonamide plasticizers, tend to accelerate the decomposition of nitrocellulose at elevated temperatures and so should not be employed in nitrocellulose compositions that may he heated much over 80 C.
Phenolic Resins
Santicizer M-17 and Tricresvl Phosphate give the greatest flexibility. Dibutvl Phthalate, Santicizers B-16 and E-15, and Diphenyl Phthalate may also he used. None give great flexibilitv to the completely cured (C stage) resin. Santicizer 9 in amounts of from 2( to 5^, (1 will improve the workability and curing of phenolic molding compositions. The Aroelors mav be used in special cases as lubricants or in coating com positions.
Polystyrene
Santicizers B-16 and 10. Ortho-Nitrobiphenvl and Di phenyl Phthalate are recommended. Santicizers E-15 and 9 are also suggested hut are not so generally appli cable. The Aroelors are compatible, the liquids having sotne solvent action when warm.
Polyvinyl Acetate
Mixtures of plasticizers usually give the best results. Santicizers M-17, E-15 and B-16 are recommended as liquid plasticizers. Ortho-Nitrobiphenvl. Dibutvl Phthalate and Tricresvl Phosphate are also useful. If excessive softening is to be avoided, the solid plasticizers --Santicizer 10 and Diphenyl Phthalate--are of value. The Santolites either alone or in combination with a solid or liquid plasticizer improve workability, flexi bility and adhesion. The liquid or seini-solid Aroelors give tough, flexible compositions of improved water resistance and electrical properties. The resinous Aroelors give harder, more brittle compositions.
Polyvinyl Butyral
Dibutvl Phthalate and Ortho-N'itrobiphenyl are es pecially recommended, but Santicizers 8, B-16, K-15 and M-17, Tricresvl Phosphate and the Aroelors mav also be used to obtain special properties.
06i<t42b
TOWOLDMONOQ38564
Polyvinyl Chloride
Santieizers M-17, K-15 and Ortho-.'Nitrobiphenvl are efficient plasticizers. Tricresyl Phosphate, Dibutyl Phthalate and Santieizer H-16 also have good com patibility. The Aroclors are compatible but do not produce great flexibility. Santieizer 140 produces com positions having lire resistant qualities similar to TCP but more flexible.
Polyvinyl Formal
Diethyl Phthalate, Ortho-Nitrobiphenyl and Sanlicizers 8, B-16, E-15 and M-17 are recommended. Santicizers 10 and Tricresyl and Triphenvl Phosphate are also useful.
Protein Compounds
(Soybean or Corn Protein, Casein, Glue)
Santieizers 8 and 9 are compatible with and give a temporary plasticizing action to most protein com pounds. For more permanent results we suggest a combination of Santolite resin with a plasticizer. Polyliydric alcohols (such as glycerine or ethylene glvcol)
may be used with the Santieizers and Santolites without materially increasing susceptibility to water. Addition of Santieizer 8 to glue-glycerine mixtures improves the flexibility and water resistance.
Santolite Resins
All of the plasticizers--both liquid and solid -may he used: one part of a liquid plasticizer to four parts of Santolite MHP will be verv soft. The solid plasticizers also produce a softening effect but to a lesser degree. Combinations of solid plasticizers and the Santolites make efficient plasticizers for celhilose esters and ethers and polyvinyl resins. Diphenyl Phthalate and Santicizer 10 are recommended for such combinations.
Equal parts by weight of Diphenyl Phthalate or Santicizer 10 and Santolite MHP will be liquid at ordinary temperatures. Increasing the proportion of Santolite hardens the combination.
Urea Formaldehyde Resins
Santieizer 9 improves the uniformity and workahilitv of resins of this class.
9
TOWOLDMONOQ38565
The Phosphates
Tricresyl Phosphate
Technical
^cwteunekA
55-gallon one time shippers (inch) (approx. 500 lbs.)
Tricresyl Phosphate is a practically colorless, odorless liquid weighing about 9.7 pounds per gallon. It has a high boiling point and an evaporation loss of onlv 0.2% in 100 hours at 100 C. Its viscosity increases rapidlv at temperatures below normal until at --35 C. it G a solid, transparent mass without crystalline structure.
Form ......
Clear, practically colorless. oilv liquid.
Color
API! \ 10 max.
Km* Phenols (Permanganate
Test)
A distinct purple color to
he present after 30 minutes
(10 gram sample -- 40 ec.
\ 100 KAlnOO.
Acidity (as H,P04)
0.01% max.
Specific Gravity at 25 25 C..........................1.166*0.007
Ester Value ..................................................Essentially 100%
This product is miscible with all the common solvents and thinners, and with linseed, china wood, and castor oils. Its solubility in water is less than 0.002% at 85 C. and it imparts good moisture resistance to nitrocellulose films. Being a solvent for nitrocellulose, it has a high relentivity and can be used in large proportions without danger of sweating or separation. It imparts excellent flexibility and increased amounts do not cause propor tionately as great a decrease in tensile strength as most oilier plasticizers.
Tricresyl Phosphate is the standard fire retarding plasticizer for nitrocellulose. It is compatible with most lacquer resins and gives firm, tough, flexible films of excellent weathering qualities. Although Tricres\l Phosphate has an inherent tendency to vellow in nitro cellulose lacquers when exposed to heat or light. e\erv precaution is taken in the manufacture of Tricre*vl Phosphate Monsanto to eliminate impurities \liicli might aggravate such discoloration.
Tricresyl Phosphate has a low compatibility with cellu lose acetate so when extreme fire resistance is desired in acetate compositions Triphenyl Phosphate should be used. Small amounts of Trieresvl Phosphate inav he
10
06i4A<;a
TOWOLDMONOQ38566
n-r<| cflcrtiv cI' how c\ rr. ill mixture* u itli marc com|,.ilil>l-' |ila-li'i/i'i-.
Tricrcsxl Phosphate lias good lubricating properties M ]iirii, in addition to its stability and fire resistance, make it valuable as a special lubricant, cutting oil coinjHinent. and pump seal.
Three isomers of Tricresyl Phosphate are possible-the tri-ortho--, tri-nieta--, and tri-para cresvl phos phates, and the technical grades usually contain all three isomers with the rneta- and para-derivatives pre dominating. The structural formula for the para compound is
J lie orllio compound is also a liquid: ch3 I
ch8 I
0
CH, -- CHS
-- Ov
Obviously it is possible to have ail three in a single molecule, thus--
Ch
illis isomer is a solid, melting point 77-78 C., boiling |K>int at 10 mm. 250-25S C.
1 the meta-compound the position:
CHS
ethyl group occupies the
0
CH3 I <=>
0
^ bis isomer is a liquid at n< Dial temperatures, with a foiling point at 10 mm. of 2 P.2430 C.
This matter of isomers explains whv there ma\ he minor differences in physical constants, such as specific gravity, refractive index, etc., between various produc tion lots of Tricresyl Phosphate. These variations do no t. however, in volvedifferencesin plasticizingproper ties.
The ortho isomer, which is reputed to he the toxic element in normal Tricresvl Phosphate, has been virtually eliminated from Tricresvl Phosphate Mon santo. thereby reducing toxicity dangers to a minimum and making the product more suitable for many applications.
11
TOWOLDMONOQ38567
The following table of physical and chemical properties
gives values that are accurate for the particular samples
upon which the tests were run, or are averages of a
great many samples, but are not intended to be con
sidered as the arbitrary limits for all Tricresyl Phos
phate.
.'
Triphenyl Phosphate
Empirical Formula . Molecular Weight Specific Gravity . Hefractivc Index Boiling Point
Flash Point
Crystallizing Point
Pour Point Specific Heat Solubility
Viscosity---at 3.0 C. 6.5 C. . 10.0 C.
20.0 C. 25.0 C. 30.0 C. 40.0 C. 50.0 C. Heat of Vaporization .
CnlloAP
........ 368.358
1.162 at 20720 C.
1.556 at 25 C.
235 C. at 4 nun. 295 C. at 13 mm. 420 C. at 760 mm.
235 C. (455 F.) Cleveland Open Cup
Non-crystalline solid at --35 C.
--26 C.
0.47--0.02
0.002*^ at 85 C. in water. Miscible with alt common organic solvents.
1100. centipoises 755. centipoises 460. centipoises 160. centipoises 113. centipoises
74.4 centipoises 39.2 centipoises 23.7 centipoises
21120 Cals. mol. 57 Cals. gm.
103 BTU. lb.
0 -0-- P = 0
Appearance___ ..
\\ hile Flakes
Odor...................
Very faintlv aromatic
Melting Point... .
18.5 C. min. start
Solution in Alcohol (10 gms. in 50cc.) Not more than faintlv opalescent
Permanganate Test..............Distinct purple color to be
present after 30 minutes.
Free Phenol -
0.1' \ max.
Acidity (as H3PO4)
0.003' t max.
225 lb. I.everpaks.
Triphenyl Phosphate is a white cry stalline solid inching at about 48.5 C. and boiling at 2159 C. at 11 nun. pres sure. Its evaporation rate is of the same order as Tricresvl Phosphate.
12
06l<t<t30
TOWOLDMONOQ38568
This product is soluble in the common solvents and thinners and with vegetable oils. Its solubility in water is 0.001'\ at 34 C. and 0.002rT at 54 C. and it imparts some moisture resistance to cellulose aeetate films.
Its retentivitv in cellulose acetate varies between 40 and 80 PHR depending upon the type of acetate, the method of incorporation, the conditions under which the end product is used, and the age of the end product. In most formulations the amount of Triphenvl Phosphate used is less than 4ft PHR. It imparts good flexibility and gives elear. tough compositions without tendency toward tackiness.
Triphenyl Phosphate is toxic ami should not be used in articles, such as foil, which are to come in contact with foodstuffs. Its light stability is rather poor but the rate of discoloration of Triphenvl Phosphatecellulose acetate compositions is much less than that of Irieresyl Phosphate-nitrocellulose mixtures.
One valuable property of Triphenvl Phosphate is that of fire retarding. When used alone in cellulose acetate films au amount of Triphenvl Phosphate equal to 2ft 1*11 H prod uoes films w hich will not support combustion. ^ hen other plasticizers are used with it, a greater
amount of Triphenvl Phosphate is necessary to retard the burning rate.
I riphenyl Phosphate has fair softening action upon
most synthetic rubbers and is essentially insoluble in
gasoline and mineral oils, which combination of proper
ties makes it a valuable ingredient of many synthetic
rubber formulations. The amount used is generally in
tbc range of
to 20<T bv weight.
Iripheml Phosphate mixed with Santicizer M-17 dis solves cellulose acetate when heated to temperatures above 120 C. Such mixtures, with or without the addi tion of pigments, may be used for making flexible sheets, either alone or on a filler base. The pigmented
sheets arc especially fire resistant. The addition of a small amount of one of the Santolitc resins is usually benefirial in aiding solution and increasing flexibility. As a suggestion for the relative amounts to he used. 1ft parts by weight of cellulose aeetate, 8 parts of Santi cizer M-17, 8 parts of Triphenvl Phosphate and 1.3 parts of Santolite MHP gives a very flexible product.
If a pigment or filler is to be used, it should first be ground with a portion of the plasticizer and may then be mixed directly into the hot solution.
Following are some of the chemical and phvsival proper ties of Triphenyl Phosphate--
Kinpirical Formula Molecular Weight Specific Gravity... Refractive Index Melting Point Roiling Point Flash PointSpecific Heat .
CM MU' 326.28
1.268 at 60' 2(T C. 1.330 at 60 C. 18.3
213 C. at 11 mm. 223 C.
0.30 =*=0.02
Solubility in:
Water .
o.oor; at 34 <:.
0.002r; at 51 C.
Gasoline .
2.7 grains TPP TOO ee. solvent
Jlenzene
230. grams TPP 100 cc. solvent
Fth\ 1 Alcohol
160. grams TPP TOO cc. solvent
FtlivI Acetate
.270. grams TPP 100 cc. solvent
Acetone
340. grams TPP 100 cc. solvent
Kiln lene
Dichloride
400. grams TPP 100 re. solvent
Linseed Oil (Raw) 13. grains TPP 100 ee. solvent
'Turpentine.....
36. grams TPP 100 ce. solvent
Triphenvl Phosphate imparts excellent properties, but because of its rather low compatibility with many plastics its true value will appear when it is used as one component of a plasticizer mixture.
13
061*431
TOWOLDMON0038569
The Santfcizers
(Sulfonamides, Sulfonates, Phthalyl Glycollates)
Santicizer 3
X-ethyl para toluene sulfonamide
common plastics is limited and its greatest value is obtained in conjunction with other plasticizers. When used either in such combination or as the sole plasticizer Santicizer 3 imparts high gloss, toughness and hardness. It also seems to sharpen the softening point of some thermoplastic compositions, especially the cellulose esters.
0H
/------- x 1 I
CH,-<
) " S -- N -- C,H,
0
Santicizer 3 imparts desirable properties to cellulose acetate although the compatibility is less than 30 PIIR. In addition to gloss, toughness, and hardness, it improves the flow of molding compositions.
Its compatibility with nitrocellulose is low but it does improve the film properties of coating compositions, although not recommended for outdoor exposure or temperatures above 80 C.
Appearance Odor ... Color (Melt) APHA Melting Point Acidity (as H5SCM
White Solid Slight, Characteristic
50 max. 59.0 C. min.
0.10% max.
Santicizer 3 has very limited compatibility with cellu lose acetate-propionate and cellulose acetate-butyrate.
With ethyl cellulose, Santicizer 3 is compatible only in low concentrations but it improves the gloss, tough ness and general film properties.
Santicizer 3 is not recommended for use with polyvinyl chloride or polyvinyl chloride-acetate.
Fiber Containers
Approx. 400 lbs. net
Santicizer 3 is a white, solid sulfonamide plasticizer, melting at about 60 C. Its compatibility with the
With polyvinyl formal, Santicizer 3 imparts good flow and excellent gloss although the compatibility is less than 50 PHR. For best results it should be used in combination with other plasticizers. This is a general characteristic of Santicizer 3. It maintains it6 good effects even when used in amounts of 5 to 20 PHR and in mixture with other plasticizers even though these are used in much higher proportions.
14
0619432
TOWOLDMONOQ38570
Santicizer 8
(Mlxtnre of ortho and para IV-ethyl toluene sulfonamides)
CH,
0H II I S-N-CjH, II 0
Appearance...................
.Light yellow, viscous liquid
Odor......................................................... Slight, characteristic
Free Amide..............................................................9%> to 13%
Acidity (as acetic acid)..............
....... 0.1%, max.
9pcniaitiete
475 lbs. (approx.) drums (extra, but returnable) 45 lbs. (approx.) tins (incl.)
Santicizer 8 is a light yellow colored liquid that is readily soluble in all common organic solvents except the petroleum hydrocarbons, in which it is only very
slightly soluble. It is soluble in castor oil. slightly soluble in china wood oil and insoluble in linseed oil. In water it is soluble to the extent of about 0.13% at 23 C. and Q.21%; at 48 C. Its solubilitv in water is decreased by the presence of ammonia but is increased by other alkalies. Its retentivitv in cellulose acetate is about 90 PIIR and it imparts a high degree of plasticity. It is a solvent for both nitrocellulose and cellulose acetate.
Santicizer 8 is an excellent plasticizer for cellulose acetate, giving a brilliance and polish not obtainable with other plasticizers. Although the light stability of Santicizer 8 in nitrocellulose is not of the highest order, this plasticizer does improve the workability and gloss. It mav be used in such compositions either alone or preferably mixed with otber plasticizers, solid or liquid. In cellulose acetate, however, its light stability is sufficient to meet most of the ordinary requirements of molding compositions.
This product, being practically insoluble in petroleum hydrocarbons, is a valuable plasticizer for coatings designed to withstand gasoline and related products.
It can be used in combination with Santolite resins for that purpose; to illustrate, a lacquer made from l part Santicizer 8, 2 parts nitrocellulose and 6 parts of Santo* lite MHP was found to be unaffected bv gasoline and, also, to prevent corrosion of iron panels exposed to a salt solution of from 3%, to saturation over a period of ten weeks.
Some of the chemical and physical properties of Santi cizer 8 are:--
Empirical Formula . Molecular Weight
CoIIuCLNS 199.262
15
061AAJ3
TOWOLDMONOQ38571
Specific Gravity Refractive Index
1.190 at 25 25 C. 1.540 at 25 C.
Hash Point
174 C.
Solubility in water
gasoline
turpentine castor oil tung oil
...
linseed oil
common organic solvent
0.13r; at 23 C.
0.213r< at 48 C.
insoluble cold
very slightly soluble hot
15 gins, per 100 cc. turps.
......................
.soluble
slightk soluble cold
soluble hot
insoluble cold
soluble hot
soluble
Viscosity (approx.)
at 10 C.--3170 eentipoises at 20 C.- 750 eentipoises
The accompanying graph shows the relative softening effect on shellac of Santicizers 8 and 9 when incorpo rated at the rate of 10. 20. 30 and 40 parts per 100 parts (by weight) of the resin. The softening effect was measured by the load (in grams) required to cause a steel point to scratch the surface of the composition at 95 K. (35 C.). Santicizer 8 is also useful with vinyl resins especially polyvinyl acetate and polyvinyl acetal.
Fig. 1
Joftemno Effect on Shellac Of
SANT/CtZEFS 3 ANO 3
Santicizer 8 has some plasticizing action on such protein compounds as casein, glue, soybean protein and corn protein. Jt may be used alone or in conjunction with other materials such as glycerine or similar compounds. The use of from 10' , to 40' ( on the protein weight is suggested.
Santicizer 8 great!) increases the flexibility of shellac, having at the same time a considerable softening effect. An amount equal to 10rj of the shellac produces very pronounced results. It may be incorporated either by direct fusion or by means of solvents. It does not destroy the adhesion of the shellac nor affect the heat curing qualities.
14* 0614434
TOWOLDMONOQ38572
Santicizer 9
(Mixture of ortho and para toluene sulfonamides)
CH,
NH,
Appearance .. Melting Point MeltAcidity
Fine granular particles ....105 C. min.
..........Liquid* clear and light yellow pH 4.6 min. in dilute acetone (2 gram sample in 15 cc. A. R. Acetone and 35 cc. of CO; free distilled water).
275 lbs. Leverpaks
Qje&cfij/i/ewi
San timer 9 is a white solid, melting at about 105 C. Its solubility is quite low in coahlar hydrocarbons and negligible in petroleum hydrocarbons. It is readilv soluble in most other solvents, and in hot linseed, china wood, and castor oils. It is soluble in water to the extent of only about 1.0<at 34 C. Its solubility in water is increased bv the presence of alkali, being about 5% at 20 C. for a mixture of equal volumes of water and con* eentrated ammonia solution. It is the least soluble of our plasticizers in ethylene dichloride and in benzene, its solubility in ethylene dichloride being about 4% at 30 C. and in benzene about 1.5% at 30 C.
Santicizer 9 has a retentivitv in cellulose esters of onlv about 30 PHR and does not impart great flexibility.
Nitrocellulose compositions containing Santicizer 9 should not be subjected to prolonged heating above about 80 C. The sulfonamide mav accelerate decompo sition of the nitrocellulose and disintegration of the entire composition.
. Santicizer 9 differs materially from other plasticizers in its action. Relatively small amounts impart a gloss to polished articles and gives smooth working and uniform curing of molded products. It blends readily with most synthetic resins and does not impart the softening action of liquid plasticizers. Because of its adaptability to a wide variety of materials Santicizer 9 is particularly valuable to the makers of all sorts of molding com positions.
In some phenol-aldehyde resins Santicizer 9 appears to act not only as a lubricant but also as a promoter, giving more uniform and thorough curing when from 2 to 5% is used.
Santicizer 9 in amounts of about 20 parts per 100, has a temporary plasticizing action on protein compounds such as corn protein and soybean protein. It may be mixed in either, alone, or in conjunction with some other material such as glycerine or a related product. It* increased solubility in slightly alkaline solutions may also be of use in incorporating it into certain compound* where such solutions are used as swelling agents or actual solvents for the plastic material.
Santicizer 9 is a plasticizer for shellac but its action is less pronounced than that of Santicizer 8. It does not have as great a softening effect, 30 parts of Santicizer 9 producing about the same degree of softening as 10 parts of Santicizer 8. See Figure 1 for comparative effects of Santicizer 8 and 9 on shellac.
Empirical Formula Molecular Weight Specific Gravity... Melting Point . Solubility in:
Water___ Benzene Ethylene Dichloride .. Turpentine Linseed Oil
C7H9OAS .........171.21 1.313 at 25 25 C. ..105 C. (approx.)
1.0% at 34 C. 1.5% at 30 C. 4.0% at 30 C. 2.5% at 20 C. . Insoluble at 203 C.
17 061. <,935
TOWOLDMON0038573
Santicizer 10
(Ortho-cresyl para-toluene
sulfonate)
-
CH, --
0
0II
--S 0
1 0
Santicizer 8 or Santicizer 9. Some of its physical and chemical properties are:
Empirical Formula............... Molecular Weight.......... Specific Gravity..-.................... Crystallizing Point........... Flash Point ............................ Solubility in:
W'ater.................. Organic Solvents ........
ChH,0,S 262.312
1.207 at 15 C. 51.0 C. 182 C.
0.0008% at 30 C. ..See Chart, Page 37
Santicizer E-15
(Ethyl phthalyl ethyl glycollate)
Appearance Melt........................ Crystallizing Point____ Acidity (as acetic acid)...
........ White crystals Practically colorless
'......51 C.
...0.03% max.
o
-- c -- O-CH.-C -- 0-C.H,
200-lb. barrels (inch)
-- C -- 0 -- C,H, II 0
^leciflicafamA
Santicizer 10 is a solid plasticizer for cellulose esters and many resins. Its retentivity in nitrocellulose is about 50 and in cellulose acetate 30 PHR. From 15 to 20 PHR are required to give added flexibility to cellu lose acetate.
Santicizer 10 is quite stable toward beat and is resistant to hydrolysis. It is soluble in all the common organic solvents but insoluble in water. W hen used with cellu lose esters, Santicizer 10 imparts gloss, hardness and moisture resistance. In such compositions it is best used with small amounts of liquid plasticizers. Santi cizer 10 is suggested also as a plasticizer for phenolaldehyde, vinyl and polystyrene resins. It is compatible with shellac but produces less flexibility than either
Color (APHA).................... Specific Gravity at 25/25 C. Refractive Index at 25 C...... Acidity (as acetic acid).... Odor........................................... Sulfur (copper strip test)--
20 max. 1.180*0.005 1.498*0.002 ...0.02% max.
Slight None
55-gallon drums (approx. 500 lbs.), (inch) 5-gallon cans (approx. 50 lbs.), (incl.)
Qbe&cti/Uion
Santicizer E-15 is a practically colorless liquid with a boiling point of 190 C. at 5 mm. and a crystallizing point of 20 C.
18
0619936
TOWOLDMONOQ38574
This product is miscible with the common organic
solvents except the petroleum hydrocarbons. It is
miscible with vegetable oils when heated hut partially
separates on cooling. Its solubility in water is 0.0175%
at 30 C.
'
Santicizcr E-15 is a solvent for both nitrocellulose and cellulose acetate and for most resins. It is light-fast, and relatively nonvolatile even from the thinnest films. With both acetyl and nitrocellulose it gives clear, tough, flexible films which have greatly increased resistance to moisture penetration. This is an efficient plasticizer which gives practically all the desirable qualities except fire resistance. It is an active solvent and the amount which may he incorporated in cellulose esters depends only upon the degree of plasticity desired.
Santicizcr E-15 is highly recommended for use with cellulose acetate and with vinyl resins. It imparts slightly less flexibility than Santicizer M-17 but has less softening effect and produces somewhat tougher compositions.
Santicizer E-15 partakes of the properties of both B-16 and M-17 although mixtures of these probably cannot be relied upon to give results identical with those obtained by the use of E-15.
For vapor pressures of Santicizer E-15, see Figure 4.
Some of its physical and chemical properties are:
Empirical Formula .............................................CulligOs
Molecular Weight........................................................ 280.301
Specific Gravity
1.180 at 25 C.
Refractive Index
.1.498 at 25 C.
Boiling Point___
190 C. at 5 mm.
320 C. at 790
mm. (approx.)
Crystallizing Point
20 C.
Flash Point...................
193 C.
Effect of heating at atmospheric pressures--
Up to 300 C.................
Slight color change
After boiling at 320 C.
. Light vellow
Heat of Vaporization
37430 Cals. mol. 134 Cals. gm. 241 BTU. lb.
Viscositv in centipoises at ......................
. 0 c.
10 C.
25 C.
Flash Points
..................
*Tensile Strengths (in Kg Cm?) of cellulose acetate
films
0 PIIK (control)
25 PHB (control)
50 PIIR (control)
75 PHR (control)
*Elongation (in per cent) of cellulose acetate films . 0 PHR (control)
25 PHR (control)
50 PHR (control)
75 PHR (control)
Increase in color rating (AP1IA) due to heating at
100 C. for four hours ............................................
% Plasticizer decomposed bv 10% NaOH solution
in 20 minutes at
. 32 C.
80 C.
----------------------------- 1-----";;-'
,--......
icueuc Biicugui auu ciuugauvu values ait iui tump
In no sense are they to be considered absolute values.
B-16 295.3 136.5
51.3 380 F.
528 420 315 243
2.3 6. 12.3 13.3
5 max.
0 0
E-15 611.1 215.7
63.0 380 F.
528 472 256 136
2.3 57 14.7 28.
5 max.
0.93 11.19
M-17 1671.4 454.8
100.3 375 F.
528 468 266 144
2.3 10. 24.7 35.3
5 max.
7.09 21.28
10
Ubl'tbJ?
TOWOLDMONOQ38575
Santicizer B-16
(Butyl pbthalyl butyl
glycollate)
.
00 II 1 , -- C - 0 -- CH,-C -0 -- C.H,
J --C- 0-C.H.
I 0
Color (APHA)
45 max.
Specific Gravity at 25 25 C.
1.097*0.005
Refractive Index
1.490*0.002
Aciditx (as acetic acid)
0.02% max.
Odor...............................
Characteristic slight odor
Sulfur (copper strip test)
None
55-gallon drums (approx. 500 lb6.), (inch) 5-gallon cans (45 lbs.), (inch)
Santicizer B-16 is a practically colorless liquid which boils at 219 C. at 5 mm. and doe6 not crystallize at temperatures as lox\ as - 35 C. Its water solubility is 0.0012( , at 30 C. It is extremely light stable.
Some of its physical and chemical properties are:
Kmpirical Formula Molecular Weight Specific Gravity Refractive Index
Cull :<( ig
1.097 at 25 C. 1.490 at 25 C.
Boiling Point ...
Crystallizing Point Heat of Vaporization
219 C. at 5 mm. 345 C. at 760 mm. (approx.)
--35 C.
11570 Cals. mol. 124 Cals? gm. 223 BTC. lb.
Santicizer B-16 is a solvent for nitrocellulose and is compatible w'ith most resins, imparting a good flexi bility. Its compatibility with cellulose acetate seems to depend greatly upon the aeetxl content of the latter: the retentivity value for one sample of cellulose acetate of about 52% combined acetic acid content was around 40 PIIR while for another sample of 56f) combined acetic acid content the retentivitv was 100 PHK. Wiili nitrocellulose it gives clear, brilliant films which are flexible, tough, moisture resistant and have good weathering qualities. Santicizer B-16 probable em bodies more desirable properties than any other single nitrocellulose plasticizer, fire retarding action being about the only property it does not have. It imparls about the same degree of flexibility as Dibutxl Phthalate but produces less softening of the film.
Santicizer B-16 is a solvent for and imparl* plasticitx to many synthetic resins. It has especially interesting properties when used with those resins of the glvcerolphthalate and phenol-aldehyde types, in which it max be incorporated at various stages of resin formation. ^ hen added to a simple glvcerine-phthalic anhydride resin at anv stage before the final gel formation, it retards the rate of thickening and permits the acid number of the resin to be lowered without completclx destroying solubility. If such a resin is heated bexond the gel stage, the product mav still be thermoplastic although its solubility will be radically changed.
Santicizer B-16 has an unusually xvide range of u*e. covering not only the synthetic plastic materials hut also the natural resins. Its solvent properties, light stability, low volatilitx' and loxx pour point are impor tant factors to be considered.
Santicizer B-16 is miscible xvith castor, linccd and china wood oils and somexvhat retards gel formation in the latter on heating.
20
06 1 38
TOWOLDMONOQ38576
Santicizer H-IO i-wdl- crepe rubber 1ml appear?- to have no effect on vulcanized rubber. It ii- an excellent plasticizer for chlorinated rubber, from 10 to 25 PHR usually being required.
Sanlirizrr B-16 is an exceptionally good plasticizer for polvstvrene. whether for molding or coating uses. It maintains the excellent properties of the resins and in coatings greatJv retards weathering failure. 15*20 PHR is recommended.
Mixtures of Samirjzcr R*l(i and Santolite resins (MS preferred) may he used to plasticize certain compounds such as casein and corn proteins, being incorporated either as solutions in some organic solvent or in the form of emulsions. The proportions of the several components can be varied between wide limits: 1 part of B*l() with 2 to 10 parts of Santolite and 1 part of such mixture added to from 0.5 to 1.5 parts of the protein compound grcatlv increase water resistance. It should he noted that B-16 alone is not a plasticizer for protein compounds.
Santicizer R-I6 darkens and then decomposes on heat* ing to high temperatures at atmospheric pressure. The approximate temperatures and the effects obtained are given below:
lip to 200 (h From 200 to 500 C. From 510 lo 550 C.
Vcrv slight color change Darkens rapidly
Boils with decomposi tion, p h t h a 1 i c anhvdride is given off and the product becomes very dark.
The addition of water causes Santicizer B*16 to be thrown out of solution from those organic solvents which are miscible'with water.
Santicizer B-16 solubility in ethanol-water mixtures increases slowlv to 10% in 72% ethanol; rapidly to 60% in 81% ethanol and 100% in 81% ethanol.
Vapor pressures of Santicizer B-L6 are shown in Figure 4.
Santicizer B-16 is an excellent plasticizer for shellac when incorporated into solutions of that resin. From 5 to 30 PUR are suggested depending upon the degree of softness and flexibility desired. It is compatible with
m<'-i natural resins. 25 FUR in rosin gives a combina
tion that is flexible at 0
50 FUR gives good pla>-
ticil\ lo Kauri Gum.
Santicizer B*H> has a fair compatibility with paraffin about 55 FUR at normal temperatures and a greater amount when warmed.
it is a good plasticizer for chlorinated rubber and appears to promote adhesion. It does not give as great flexibility as does Santicizer M-17 but produces more than Dibutyl Phthalate. \bout 10 PHR is reeommended.
Santicizer M-17
(Methyl phthalyl ethyl glycollate)
f' ''j --c --0 --CH, --C --O'-CiH,
ly/ -- C -- 0 - CH3
6
SP/ieeificaiimiA
Color (APIJA) Specific Gravity at 25 25 C. Refractive Index at 25 C. Aciditv (as acetic acid) Odor Sulfur (copper strip test)
20 max. 1.220*0.005 1.501*0.002 0.02r; max. Slight, characteristic
None
55-gallon drums (approx. 550 lbs.), (inch) 5-gallon cans (approx. 50 lbs.), (inch)
21 061<i<i3S
TOWOLDMON0038577
(J
Santicizer M-17 is a practically colorless liquid with a boiling point of 189 C. at 5 mm. It remains liquid at temperatures as low as --35 C. and is a solvent for both nitrocellulose and cellulose acetate. It imparts a high degree of plasticity which is maintained undimin ished even in extremely thin films exposed to air cur rents for a long time. It is very light-stable and may be used in transparent or tinted articles without danger of yellowing.
Some of the chemical and physical properties of Santi cizer M-17 are:
Empirical Formula Molecular Weight Specific GravityRefractive Index Boiling Point
Cr\stalli/,ing Point Flash Point
CuIlnOe 266.262
1.220 at 25 C. ...1.504 at 25 C. .... 189 C. at 5 mm. 310' C. at 760 mm. (approx.) . Less than --35 C.
190 C.
Effect of heating at atmospheric pressures --
Up to 190 C.
Slight vellow color
250 C.
Light yellow
310 C.
Yellow
Heat of Vaporization
. .35170 Cals. mol. 133 Cals. gm. 239 BTU. lb.
Santicizer M-17 is not soluble in castor, linseed, or china wood oil or petroleum hydrocarbons, but is readily soluble in most other organic solvents. Its solubility in water is 0.09% at 30 C. but it imparts a considerable degree of resistance to moisture penetra tion in both nitrocellulose and cellulose acetate films. Santicizer M-17 is probablv the best cellulose aretale plasticizer available.
Where it is desired to use a hot mix and avoid the use of volatile solvents, cellulose acetate mav be dissolved directly in Santicizer M-17 by the aid of heat. By
employing acetate of the proper acetyl content and viscosity, and amounts of M*17 equal to from 1 to 2 times the weight of acetate, it is possible to make solutions which will flow or be workable at temperatures of from 120 to 180 C. and which will set to a tough, transparent product on cooling. The character of the product may be varied bv additions of Triphenvl Phosphate and Santolite resins.
The retentivitv of Santicizer M-17, like that of Santi cizer B-16, varies with the acetvl content of cellulose acetate. Thus the use of 2 parts of Santicizer M-17 with 1 part of cellulose acetate having a combined acetic acid content of 52% produced marked exudation of the plasticizers whereas when the same proportions were used with an acetate of 56% combined acetic acid content there was no exudation. This phenomenon of exudation, caused by the use of too large a proportion of plasticizer, can frequently be overcome bv the addi tion of small percentages of Santolite resins.
Santicizer M-17 affect6 synthetic resins in a manner similar to Santicizers B-16 and E-15 but usually it gives a greater degree of flexibility. Its action is pronounced with alkvd, vinyl, polvstvrene and many phenolic resins and with chlorinated rubber. Often as little as 5 PHR produces marked flexibility. It is not compatible with resins of the urea-formaldehyde type or with protein compounds such as corn protein, soy bean protein or casein. It mav be used with some of these compounds, however, when mixed with Santolite resins in the manner outlined under Santicizer B-16.
Santicizer M-17 dissolves Santolite resins, and since both are very resistant to petroleum products and also compatible with so many film-forming materials they make an excellent combination for producing naphtharesistant coatings. By varying the proportions of each of the three components--Santicizer M-17, Santolite resin and film material, (which is usually a cellulose ester) a practically complete range of properties can he obtained from hard to soft, from solid to liquid at slightly elevated temperatures, stickv or entirely noiltacky, brittle or flexible. Such compositions can be applied to a wide varietv of uses.
Vapor pressures of Santicizer M-17 are given in Figure 4.
22
0614440
TOWOLDMONOQ38578
The Phthalates
Dimethyl Plitlialate
0 r' , -C-O-CH,
- C 0 CH, 0
jP/teciflicatmn&
Appearance
Clear, water-while, oily liquid
Color (API!\)
10 max.
Odor
Not more than slightly aromatie
Acidity (as phthalie acid)
0.01r; max.
SjM-cifie Gravity at 25 25 C.
1.190*0.001
Refraeli\r Index at 20 C.
1.5155*0.001
Pnritv
Kssentially 100(<
Sulfur (Copper strip test)
.None
r(ocn/atneiA 55-gallon (approx. 500 Ihs.). (inch)
Dinietlnl Plitlialate is a colorless, liquid solventplasticizer for cellulose acetate. It is completely com patible with nitrocellulose, but is seldom used with 'hat material because it does not impart the desired qualities. Its boiling point is 282 C., its crystallizing point 0 C. anti its weight about 10 pounds per gallon. It is soluble in all common organic solvents and with
oils (except petroleum oil>) and has a >olubilit' in water of 0.1' , at 32 C. It lias excellent light stahilit\.
Dimethyl Plitlialate, having a rather low boiling point and high evaporation rate is apt to he lost from plastic compositions, leaving, them brittle. This is especially true in the case of thin films or those objects when* the ratio of surface to volume is high. In certain eases too. where the finished article will be exposed to severe cold, there is danger of the Dimethyl Plitlialate ervstailizing. causing not only brittleness but also a whitening and lack of transparency which mat he at least parth permanent.
Dimethx I Plitlialate is widek used hut cannot he Miid to meet ver\ rigid plasticizer requirements. Its use i> restricted almost entirely to the cellulose acetate field, and, there, as a genera! rule, it is used in combination with l)ieth\l Plitlialate or some other plasticizer. It should he noted, however, that although Dietlwl Plitlialate has a slightly higher boiling point and lower vapor pressure than Dimethyl Plitlialate. its los hv evaporation from cellulose acetate compositions is equal to that of DimethvI Plitlialate.
In addition to its use as a plasticizer. DimethvI I'lithalate is a very eflicient insect repellent. It appears to he quite harmless when applied to the skin and main tains its effectiveness for several hours.
For vapor pressures of DimethvI Plitlialate m*c Figure 7.
Some of its chemical and phvsicai properties are:
Fmpirieal Formula Molecular W eight Specific Gravity Refractive Index Boiling Point Crystallizing Point Pour Point Flash Point Flame Point Specific Heat Heat of combustion Heat of Vaporization
(ooU.r.O, PM.18
1.190 at 25 2.'C C. 1.515 at 20c C. 282 C. < <:.
.'ft0 C. pSiiper-cook) 119 <:. 172 <;. 0.27
5,709 ()al. grams 27090 Cals. mol.
139 Cals. gm. 251 HIT. II-.
23
061^441
TOWOLDMONOQ38579
Diethyl Plitlialate
Phthalate as a plasticizer for cellulose acetate. Its boiling point is about 295 C. and its weight about 9.35 lbs. per gallon. It is miscible with all the common organic solvents and diluents. Its chemical constitution places it between Dimethyl and Dibutyl Phthalates and its properties fall into that position, although it is more nearly like the former than the latter.
0 ( ! C -0^ , -C 0- C.H,
O
The evaporation rate of Diethyl Phthalate is too high for successful use as a regular nitrocellulose plasticizer.
Mixtures of Diethyl and Dimethyl Phthalates usually give better results than can be obtained by either one alone, the proportions generally used being approxi mately equal parts by weight.
yfiew'/fea/wnb
Appearance
Clear, -xater-white. oilv liquid
Color (API!A)
Not darker than 10
Odor
Yerv slightly aromatic
\eidit' (us phthalic acid)
0.01' ( max.
Specific Gravity at 25 2.') C.
,1.120*0.005
Kefractixe Index at 20 C.
1.5030* 0.0OI
Assay (ester content)
90r, min.
Sulfur (copper strip test)
None
55-gal. drums (approx. 500 lbs.), (inel.l
Diethyl Phthalate is u colorless, liquid plasticizer generally used alone or in mixture with Dimethyl
Diethyl Phthalate imparts slightly less flexibility to cellulose acetate than does Dimethyl Phthalate and its effect on moisture penetration is about the same. Its viscosity is considerably less than that of Dibutvl Phthalate and varies at about the same rate for equal changes in temperatures.
For vapor pressures of Diethyl Phthalate see Figure 7.
Some of the chemical and physical properties of Diethvl Phthalate are:
Empirical Formula Molecular Weight Specific Gravity Refractive Index Roiling Point Crystallizing Point Flash Point Specific Heat. lleat of Vaporization
C.JIi.O, 222.232
1.123 at 20 C. 1.5030 at 20 C. 295 C. at 700 mm.
-- 0.3 C. 152 C. 0.20
33550 Cals. mol. 151 Cals. gin. 272 RTF. Ih.
24
06
TOWOLDMONOQ38580
IHbutyl Plitlialate
O
j/X-| - - C - 0 - C.H,
V CO- C.H, " I: o
Appearance Color (\P11A) Odor Acidity (as phlhalic acid) Specific Gravity at 25 25 C. Refractive Index at 25 C. Assay (ester content) Sulfur (copper strip test)
Clear, oilv liquid 20 max. ..... Slight
O.Oir; max. 1.045*0.001 1.1005*0.001
99r't min. None
55-gal. one-time shippers (approx. 465 lbs.), (inel.)
I)ibut\l Phthalate. one of the most widely used plasti cizers for nitrocellulose, is a practically colorless liquid which boils at 340 C. at atmospheric pressure and 206 C. at 20 nun. and crystallizes at about --35 C. It has a weight of about 8.75 pounds per gallon.
It is soluble in all the common organic solvents and with oils hut is soluble in water only to the extent of 0.001 r< at 30 C. In spite of this low solubility, how
ever, it adds practicallv nothing to the moisture resistance of nitrocellulose films. It is compatible with imM lacquer resins.
Dibutvl Phthalate has excellent light stability which permits its use in colorless, white or delicately tinted products. Its retentivity in cellulose acetate is less than 20 PIIR and in that amount does not increase the plasticity. It is a solvent for nitrocellulose and gives a high degree of plasticity but greatly reduces the tensile strength and tends to produce softness if used in large proportions.
The stability of Dibutvl Phthalate and its high solvent power for most plastic materials make it one of the most acceptable plasticizers for general use.
For vapor pressures of Dibutvl Phthalate see Figure 7.
The viscosity of Dibutvl Phthalate (determined by the Iloeppler Viscosimeter) in centipoises through the range of 10 C. to 50 C. is shown in the following table:
Temperature Degrees C.
9.9 11.0 15.2 19.4 30.0 40.0 50.0
Viscosity Centipoises
31.9 29.6 25.5 21.4 13.1
8.9 6.5
Some of the chemical and Phthalate are as follows: Empirical Formula Molecular Weight Specific Gravity Refractive Index Boiling Point
Crystallizing Point Flash Point Specific Ilcat....... Heat of Vaporization
tvsiea! properties of Dibutvl
-4),
278.339
UHfi at 20 20 C.
1.490 at 25 C.
206 C. at 20 mm. 3 10 C. at 760 mm.
--35 C.
170 C.
...
0.3 1
30980 Cals. mol. 111 Cals. gin. 201 BTU. Ib.
25 C61`t4`i 1
TOWOLDMONOQ38581
Diphenyl Phthalate
0 (' 0
C0 o
ff/tettficafiom
\<k|..p.*e_a__ra__n_c_e,
t(h'.o..a..r.s..e....w..1hite.....p..o..w...die...r...o...r rfu..s..e...dl _s_oil:i,di
Free Acid (as Phthalic)
0.20' ( max.
Free Phenol
0.20r, max.
Ash O.O.V, max.
Moisture
0.r>0(`; max.
Santolite MHP being practically liquid al normal temperatures. Such mixtures of l)i)>hen\l Plillialatc with either Santolite MS or Santolite Mill* are excellent plasticizers for nitrocellulose in odorless, flexible ami adhesive coatings.
Dipheml Phthalate is completely insoluble in water and gives increased water resistance to all composition* in which it is used.
Dipheml Phthalate when used alone does not ii>uall\ impart a high degree of flexibility lint it blends well with other plasticizers and can he used in varied combina tions. This plasticizer is especially recommended for vin\l resins, polystyrene, etlnl cellulose, and -nine of tin- natural resins sueh as damar.
So"M` "f i,s ,'l"'",i,'al ,,h> si<'.......... r,i'"....
Kmpirical Formula *
Molecular eight Specific Gravity Befractivc Index Boiling Point (.r\ stallizing Point Flash Point Heat Stability
C ...I I,,(>
:m.:U2 i.2 at 2o 1 .'>72 at :r c.
|0,V c. 00' c.
221" C. Discolors quite rapidlx at 1 -*>0C < i.
Hake l:'>0 lb, containers (incl.) bused .>2.'> lb. Black iron drums (F.xtra. returnable)
in
Dipheml Phthalate is a white powder, melting at about (>() C. and readily soluble in ketones, esters and rhlorinated bvdroearbons. Its solubility in alcohol-, turpentine arid linseed oil is rather low. being in the neighborhood of o.O grams per 100 ec. of solvent at 2.V C.
Dipheml Phthalate is eompatible with nitroeellulose and with tlu' sulfonamide, phenolic, pohstvrene and viml 1\pes of svnthetie resins. In nitrocellulose lacquers it produces hard coatings that have excellent gloss retention and weather resistance. The addition of Diphenyl Phthalate to Santolite resins lowers their softening point, equal parts of Diphenyl Phthalate and
HB-40
IIB-10 is a high boiling liquid h\droearbon that haconsiderable merit as a plasticizer for ethvl etHulo-r. polystyrene and henzvl cellulose.
IIB-10 has the following plnsical ami chemical prop erties:
Appearance Color.
Mobile. oil\ liquid I.es- than 20(1 \PI! \
26
0614^4
TOWOLDMONOQ38582
Distillation Range S|>ecific Gravity Refractive Index Flash Point Flame Point Crystallizing Point Pour Point Fight Stahilitx Ural Stability
Stability to Acids ami Alkalic
Soiubilitx in \\ ater 1'thy ] Alcohol
3H)\:10(. C. ((il.V.TJ.V I'.) 1.1)01*0.00:1 m 25 IC.
1.5t>75 0.0075 at 25 C. 315 F. (171 C.) 385 F. (1% C.) 5 C. (approx.)
-28 C. ( -18 F.) (Super-cools) Darkens on exposure to sunlight Appears to he relatively stable at the boiling point in glass. Decomposes at 250 C. in iron. Does not readilv oxidize.
Stable in boiling 10' , NaOll or ifso4
Insoluble (. ce. Hll-40 in 100 ce. at 25 C.
OrthoMtrobiphenyl
no, I
B^iecificaJumb
\ppearancc and Color ..
Fight vellow to reddish
crystalline solid
Cry stallizing Point
3i.5 C. min.
Distilling Range:
O.V (,1-06 or.)
.5 C. max.
100' , (between 320.0 C. and 330.0 C.) 7 C. max.
Soluble in all proportions with
Acetone Benzene Carbon Tetraehloride Castor <)il FI t her F.tbxl Acetate
Finseed Oil Mineral Oil Skellysolve 11 Solvent .Naphtha Turpentine
llli.10 is useful not onl\ in straight polystyrene resin.**, "here it max be added to tin* monomer before poly merization. Imt aU in s|\rene eopolvmers and com binations with other resin.** where it acts as a blending agent as well a** a plasticizer. The compatibility with straight pnly-turnc resin is about 50 PHK.
IIB.Id is a soU cut plasliei/.er for the asphaltic bases used in certain coatings and seems to aid krushabilitv and gloss.
Although stable under normal conditions 1111*40 is not inphh resistant to oxidation when heated and is dis colored bv ultraviolet light.
QjeSoitfi/emi
Ortho-Nitrobiphenvl, also called Ortho*.\itrodiphen\ 1. is a iiglit yellow to reddish colored liquid or solid of characteristic odor. It is compatible with the cellulose esters and ethers, polyvinyl chloride, polyvinyl buty ral. poh vinyl acetate. pol\'9tyrene, rosin, rosin esters, modi fied ro.-in esters, modified phenolic resins, oil soluble phenolic resins, alkvd resins and vegetable oils. This wide compatibility, a low rate of hvdrolvsis. and resistance to acids, alkalies, and mineral oil, together with an unusually low price make ONB a very attrac tive plasticizer.
Some of the physical and chemical properties of Ortho* Nitrohiphenx 1 arc:
Fmpirical Formula Molecular Weight Molting Point
Boiling Point at 10 mm. Boiling Point at 760 mm. Refractive Index at 25 C.
Cp-lhC);N 109.20
Approx. 35 C. (Super-cools readily)
.Approx. 172 C. Approx. 330 C.
Approx. 1.613
27
Specific Gravity at 40 15.5 C.
Approx. 1.189
Viscosity at 25 G.`
38 centipoises
Viscosity at 45 C.
..... 12 centipoises
\\ eight gallon
Approx. 9.9 lbs.
Fla^li Point
. .113 C. (289.5 F.)
Fire Point
179 C. (354.5 C.)
^Obtained on supercooled materia
Practicallv insoluble in w ater (either hot or cold).
Readily soluble in:
Benzene KtliyI Alcohol Methvl Alcohol l.tlier Acetone Methyl Kthy 1 Ketone Kthyl Acetate Amyl Acetate (>rlho*Dichlorobenzene
Carbon Tetrachloride Perchlorethv lene Glacial Acetic Acid Mineral Spirits Pine Oil Turpentine Linseed Oil Soya Bean Oil Corn Oil
()rtho*\itrobiphenvl (ONB) plasticizes most resins, both synthetic and natural, the amount required vary ing with the resin ami the intended use. It may be iisol as the sole plasticizer or, preferably, in conjunction with one or more other plasticizers. The volatility of ONB is less than Diethyl Phthalate but greater than Oilmtvl Phthalate.
In nitrocellulose, the plasticizing action of OrthoNitrobiphenyl is similar to and in some cases superior to that of camphor. The two plasticizers work well together, or camphor oil may be substituted for all or part of the camphor in the formula. In lacquers ONB aids solvent release.
\\ illi cellulose acetate and cellulose aeeto-propionate ONB is highly compatible, 50 PUR giving clear, trans parent compositions of good molding properties and medium flexibility,
Ortho-Nitrobiphenyl is compatible with cellulose ace tate-butyrate and produces hard, tough compositions suitable for either molding compounds or lacquers.
ONB is very compatible with ethyl celluose and pro duces compositions of good weather resistance.
Compatibility with the several vinvl resins varies considerably. It is highly compatible with polv vinvl acetate, 50 PHR giving very flexible, tackv composi tions. In polyvinyl formal the plasticizing effect is greater than in cellulose acetate, 5ft PUR producing good flexibility but no tackiness. Temperature?, of 150"*1G0 C. are required for good flow in molding.
With polyvinyl butvral 50 PHR of Ortho-Nitrobi phenyl produces very flexible hut slightly tackv coin positions which have good weather resistance. This is about the compatibility limit. Temperatures of I2<B130 C. are sufficient for good flow.
Ortho-Nitrobiphenvl is quite satisfactory with polvvinvl chloride but requires a working temperature of more than 150 C. and the use of some stabilizer such as lead carbonate. The compatibility limit lies some where between 40 and 50 PIIR. 40 PHR producehard, tough, flexible, transparent compositions.
The compatibility of Ortho-Nitrohiphem I with pol\ vinvl chloride-acetate eopolyiners increases and the working temperature decreases with increased acetate contents. Yinvlite YYNW, with a 95 5 chloride acetate ratio, requires a temperature of over 150 C. for good flow, while YYHH with an 85 15 ratio flows well at 110-120 C. With both however. 40 Pllll gives verv flexible compositions.
With polv stvrenc, Ortho-Nitrobiphenvl ia highlv com patible and imparts flexibility without causing the undue softening and tackiness which result from the use of the usual types of plasticizers.
Ortho-N'itrobiphenvl ha good fungicidal properties when incorporated in plastic compositions.
Coated textiles, where Ortho-Nitrohiphem 1 was the plasticizer and the base plastic of the coating was polvviml acetate, polvvinvl formal, polvvinvl butv ral. cellulose acetate, Yinvlite YYHH, or polvstv rene, did not support growth of Aspergillus niger. Penieilliurn. Chaetoniium globosum or Metarrhizium. even after the coated textiles have been leached in running water for 48 hours.
Heating the coated textile? for 5 days at 105 C. resulted in some loss in fungus resistance.
28
TOWOLDMONOQ38584
S p e c if ic Gr a v ity
O !0 20 30 40 50 60 70 SO 90 too Temperature Degrees C.
20 Obl't't't?
TOWOLDMONOQ38585
i i?. :)
P efS S U ZE mm. O f P j.
30
061't't'ta
TOWOLDMONOQ38586
P/PES3U&E mm. O f My.
Fig. 4
31 0614449
TOWOLDMONOQ38587
l i... 5
S p e c if ic G/za v / t y
32
Obl^SO
TOWOLDMONOQ38588
Kip. 6
S p e c / f c Gr a v it y/
O IO 20 30 40 50 60 70 80 9o too Temperature Degrees C.
33
061`t`til
TOWOLDMONOQ38589
PRESSURE m m . OF Hq.
I ijr. :
:u 061<t<t52
TOWOLDMONOQ38590
SO 60 70 30 90 /oo 120 /4-0 /SO /80 200 Temperature Deg-pees C.
250
300
35 061<t<t53
TOWOLDMONOQ38591
General Data
Flash Points*
Plasticizer
c . Calculated c C.
Tricresvl Phosphate Diphenyl Phthalate Tripiienyl Phosphate Santicizer B-16 Santicizer E-15 Santicizer M *17 Santicizer 9 Santicizer 10 .. Santicizer 8 1IH-JO...... .. Dibutyl Phthalate Diethvl Phthalate Dimethyl Phthalate........ ......
455 235 435 224 430 221 380 193 380 193 375 190 370 188 360 182 345 174 345 174 340 170 305 152 300 149
`Drlrtmincd in Cleveland Open Cup.
Viscosities and Pour Points < of Liquid Plasticizers
Plasticizer
Pour Point (2) 0 C.
Viscosity in Cetilipoisrv 10 C.
Tricrcsvl Phosphate.. Dibutvl Phthalate..... Diethyl Phthalate. .. .. Dimethyl Phthalate........ Santicizer B-16.............. Santicizer E-15..... . Santicizer M-17..... ............
-26 -40 Below -10 -26 Below "40 -34.5 -26
450.8 32.0 19.6 30.1
136.5 213.7 454.8
(1) l'our point* were determined acrordinp to tbe method outlined in the ASTM Standard* on Petroleum Produrts. (2) The pour point temperature* are in Mint cate* lower than the rryatallizina point* due to the phenomenon of 'uper-coolinj."
161.0 10.7 12.7 17.1 68.2 02.3
160.0
3ft
TOWOLDMONOQ38592
Solubility of Liquid Plasticizers in Organic Solvents and Oils
Tricresy) Phosphate
8
Sunt icizers
B-16
p-r,
M-17
Phthulute
!)iButyl
I),. Ktlivl
hiMethyl
1IB. 4(1
Methyl Alcohol..
MM M M M MMM
s
Ethyl Alcohol
M M M M MMMM
s
Butyl Alcohol.
MMM MMM MM M
Acetone...
M MM M MMM M M
Methyl Ethyl Ketone
MM M MM MM MM
Ethyl Acetate..
MM M M M MMM M
Amvl Acetate.. .
M M M M M M M M \(
Ethylene Dichloride.
MMMMMMMM M
Trichlorethvlenc...
MMMMMMMMM
Carbon Tetrachloride
MM M MMMMMM
Chlorinated Paraffin
M IMM IMMMM
Gasoline (Skellysolve E)
M IM I IMM iM
Benzene ___
MM MM MMMM M
Xylene
.... M M M M M M M M M
M onochlorobenzene
MM MMMMMMM
o-Dichlorobenzene....
MMM MMMMMM
Chlorinated Biphenyl (Arorlor 1212) '
MM MMMMMM M
Pine Oil........
MM M M MMMMM
'I'urpentine ............
M SM M SM M SM
1.inseed Oil (Raw)........
Tung Oil......
................
M IM S iMMMM M s M s i M M M \1
Soybean Oil ........................... ..... M I M s I M M S \1
Perilla Oil...................
.... M
IM
s
iMMM M
Castor Oil..................................... ...... M M M s I M M M M
M = Miscible
I = Insoluble
S - Soluble
37
061`t'tSb
TOWOLDMONOQ38593
Solubilities of Solid Plasticizers in Organic Solvents (Grams Plasticizer per 100 cc. Solvent at 25 C.)
Triphenyl I'liOKpItHie
Sanlicizer y
Santiri/er 10
Methyl Alcohol 1 Ain 1 Alcohol lintvl Alcohol \cctone Metln 1 I'Aln 1 Ketone 1 Ain 1 Acetate Ann 1 Acetate 1 Ain lene 1 liehloride Triehlor Klhvlene Carbon Tetrachloride Benzene \Wene Monoehlorobenzetic o-1 )ichlorohenzene Turpentine Bine Oil l.iiwed Oil (Kaw) Tun" t >il So\ bean (til IVrilla Oil (lastor (>il Mineral Oil Chlorinated Bipheml ( Vroelor 1212) Chlorinated ParaOin Gasoline (Skcll\ 1.)
_ 335 160 135 310 ISO 270 165 100 310 210 330 230 340 320 30 120 13 22 12 12 27
<2 111 21 0-
37 o'
50 15 20 10
3 V. ft. s. V. S. 6. V. s. s. V. s. s. V. S. 8. V. S. 8. V. ft. s.
5 V. s. 8. V. s. 8. V. S. S. V. ft. s. V. ft. 8. V. s. S. V. ft. ft. V. ft. ft. V. ft. ft.
20 13 12 225 250 200 M0 310 250 215 300 170 250 215 35 10 15 15 12 1 1 V. ft. s. 125 25 1
\. s. *. means ver\ slightly soluble.
Dijiheio 1 Phlliulair
12
1 215 1 10
05 25 180 120 7o 00 15 111) 1 10 10 22 12 13 10 10 10 < 0.5 00 25 0.5
an
U6l<Ab6
TOWOLDMONOQ38594
Solubilities of Some Kesins and Waxes in Dibutyl Plithalate and Santicizers B-16, E-15, and M-17
IWmt
Dibutvl 1'hthalate
B-l<>
E-15
M-l
Alkyd Resins Phenolic Resins Yin\l Resins Polystyrene Sulfonamide Resins brea Resins Ambcrol...... Kster Gum Rosin Shellac Manilla Gum Kleini Gum Gmn Arabic GurnGhati. Paraffin Wax Carnauba Wax
...........
SH SH
S
s s
s s s s s
Ss ss s SH s SH ss
.. .
. . ...
III1
s s s SH s s s SH s ssS
SH SH SH SH
Sll SH SH SH
........... . . .
s
s
s SH
I II 1
..........
.................
IIIi SH SH SSH SH
SH SH SSH
l
1--Indicates that the material is insoluble. S--Indicates that the material is soluble. Where heating is necessary to obtain solution there is no separation
on cooling. SH--Indicates that the material is soluble when hot but separates on cooling. SSH--Indicates slight solubility when hot.
39 061<AS7
TOWOLDMONOQ38595
Denotes: of use N Denotes: oi'special value
Aroclors Dihnlyi Phthalate
Dietln' 1 Phthalate
Dimethxl Phthalate Diphenyl Phtholate II11-40 Ortho-Nitrobiphenvl Santicizer 3 Santicizer 8 Santicizer 9 Santicizer 10 Santicizer 11*16 Santicizer K-15 Santicizer M-17 Triphcnx 1 Phosphate Tricresyl Phosphate
SUGGESTED Vl \su
i2
", . 't
-- j
' if 2 | 14
sy - W <
- JS --
* X
X \
x\
\
, \
. *l X
XX
|
i X
X X
' X
X
x1
1
X
\
X
^1
X
\
1 X X
;X.
X!
! X
40
061*1`tSa
TOWOLDMONOQ38596
Cellulose Slieiia<
lflZER APPLICATIONS
TOWOLDMONOQ38597
TABLE OF CHARACTERISTIC!
TRICRESYL TRIPHENYL SANTICIZER SANTICIZER SANTICIZER SANTICI2;
PHOSPHATE PHOSPHATE
3
8
9 10
Molecular Weight
368
326
199
199
171
262
Color and Form
Colorless liquid White flakes White solid
Light amber liquid Granules
White cryst;
Melting Point
48.5 C.
105 C.
Boiling Point
295 C./13 mm 245 C./ll mm
Crystallizing Point
Non-cryst., solid at-35 C.
58" C.
51" C.
Specific Gravity.
1.165 20 C. 1.268'60 C. 1.171 at 65765" C. 1.188/25" C. 1.313,25" C. 1.207 15'C
Pounds pet Gallon. 9.7
10.5 9.76 9.9
10.9 10.06
Refractive Index
1.556 20 C.
1.522/65" C.
Evaporation Rate 6ms/ sq. cm/hr/100 C... 0.00000708
0.00000028
0.0002659
0.000053 at 56" C.
Solubility in Water
Less than 0.002% 0.001% at 34" C. 0.6% at 34" C. 0.13% at 23" C. 1 % at 34 C. 0.0008%
at 85 C.
0.002% at 54 C.
0.213% at 48" C.
at 30" C.
Retentivity in N/C `1J . 100 plus
too
too 25-30 50
Retentivity in Ac/C<8>. 0
40-30 50 90 25-30 30
Light fastness in N/C 11 Poor Poor Poor Poor Poor Medium
Light Fastness in Ac/C
Fair Good Good
Fire Retardation
Excellent
Excellent
None
None
None
None
Toxicity11'
See footnote
.]' in itnumi v in MTimc.KLU losi;
i.H) LIGHT FASTNESS IN NITROCELLULOSE
fca^Sttsanttlr
livitv if rxi>rrr<l in |mru of j>J*liri*pr }>pr )<K> piirtp of rrnn li> xveiflit. MrafiirrinnilK *prp not iii.dp Jirjornl lOOIMIIt.
(2 RETENTIVITY IN CELLl LOSE ACETATK Hip rrlPinivil) in ^r/C a dpiprniinpd aa for N / C exd xvrrp imtdp from an I l.S </< M.lniimi of Ac Cdi.oNpcJ in a.
are made aa for N/C. All tbe Ap/C plaalieiaer. m.y It to. il-16. K-15 and M-17 way be considered a* equal in atalnlity, S
42
061'i'it>0
TOWOLDMONOQ38598
OF MONSANTO PLASTICIZERS
SANTICIZER B-16
336 Colorless liquid
SANTICIZER E-15
280 Colorless liquid
SANTICIZER M-17
266 Colorless liquid
DIBUTYL PHTHALATE
278 Colorless liquid
DIETHYL PHTHALATE
222 Colorless liquid
DIMETHYL PHTHALATE
194 Colorless liquid
DIPHENYL PHTHALATE
318 White powder
?19c C./5 mm. Below --35 C.
190 C./5 mm. 20 C.
189 C./5 mm. Below --35 C.
206 C./20 mm. 295 C.
-35 C.
-03 C.
282 C. 0 c.
405 C. 69 C.
1.097/25 C. 9.1/ 1.490/25 C. '
1.180/25 C. 9.84 1.498/25 C.
1.220/25 C. 10.2 1.504/25 C.
1.047/20 C. 8.75 1.490/25 C.
1.123/20 C. 9.35
1.503/20 C.
1.196/15.6 C. 10.0 1.515/20 C.
1.28/25 C. 10.68 1.572/74 C.
0.0000881
0.0001106
0.000221
10012% at 30 C. 0.0175% at 30 C. 0.09% at 30 C.
100 20-30 bcellent tioellenl None
100 100 Excellent Excellent None
100 100 Excellent Excellent None
0.000221 0.001% at 30 C.
100 Less than 20 Excellent
None
0.000617 0.058% at 30 C.
100 too Excellent Excellent None
0.001925 0.4% at 32 C. 0.6% at 63 C. 100 100 Excellent Excellent None
Insol. 165 20 Poor
None
<) TOXICITY
Thr terma "toxic" ami "non-toxic" arc. acientificalljr apcaking. onlj 'flxtir*. A product mar be barmieaa if uard uuder the condition* conimonlf prevailing in indutlrial practice, but baxardoua if applied to aome unmuii application. In any propoaed uae where toxicity ia oonaidered to be a factor, we auggcal that you write for apecific information regarding 'lie available toxicological data which may apply to your problem.
general the poaaihle toxic effect# uf the product# diacuaaed in tbia booklet mj' lie described aa follow*:
The pbtbalale eaiera (Diphenyl, Dibntyl, Diethyl end Dimethyl I'hlbalatea) accm aafe for ell normel requirement*.
The phthalyl glycollatea (Senticiecra B-lh. F--15 end M-17) accm 1 < I" the ea(rat of any.
'I'ri|-lieny| Phoapbate ia definitely e haeard in article* connected w ith the food indualry but otherwiar aeetn# quite aafe.
The toxicity of Tricreayl Phoapbate depend* upon the iaotueric form* prearnt. The ortho iaomer i* conaidered the moat dangeroua. The para and meca iaomera appear to be much taler and the totalled "non-toxic" grade i* compnaed of a mixture of tbear two. "Tricreavl Phoapbate Monaenlo" conaiat* aoleiy of thi* ao-called "ortho-frre" or
"non-toxic" (trade.
Sanlicixrr* 8, 9 and 1(1 aeem to have #li|hl toxic propertir* and are nut recommended for any uac where they might be taken internally. The Sanlolite retina appear to be aafe for all normal requirement*. The Aroclort (aee page* 49-59) mutt be conaidered toxic under tone condition! of uac. They ahould not he uaed in connertiun willi the food induatry and conlinunur expoaure in the liquid or vapor phaar ahould be avoided.
ia
OoH-itjl
TOWOLDMONOQ38599
The Santolites
(Aryl Sulfonamide -- Formaldehyde Resins)
The Santolites are condensation products of aryl sul
fonamides and formaldehyde. They vary from hard
brittle resins to soft sticky resins, which for ease of
handling are cut with a sufficient amount of solvent to
make them flow readily. Thev are exceptionally com
patible with other resins and perform many functions
of an unusual nature.
.
The Santolites increase the retentivity of cellulose acetate for plasticizers and tend to prevent separation and exudation. For example, in a mixture of 10 parts of cellulose acetate, 6 parts of Santicizer M-17 and 6 parts of Triphenyl Phosphate, the Triphenyl Phosphate would probably begin to separate out after a time. This could be prevented by adding to the composition. 3 parts of Santolitc resin. Furthermore, the addition of the Santolite would increase the flexibility of the product and permit reduction of the plasticizer content. The figures given are only approximate but illustrate the point.
The Santolites make solutions of low viscosity. If one adds to a nitrocellulose solution of about spraying lacquer viscosity, a weight of Santolite MHP equal to 50%, of the nitrocellulose present, there is essentially no increase in the viscosity of the solution. The addi tion of 100% of Santolite gives only a very slight increase in viscosity.
Films composed of 2 parts of nitrocellulose and 1 part of Santolite MIIP are much harder than films made without the use of Santolite. Equal parts of nitro cellulose and Santolite MHP produce films of about the same hardness as though no Santolite were present. The addition of a plasticizer reduces the hardness of such films but a mixture of 10 parts of nitrocellulose, 8 parts of Santolite MHP and 3 parts of Santicizer B-16 gives films of nearly the same hardness as though they were of nitrocellulose alone but with increased flexibility.
The Santolites increase the moisture resistance of nitrocellulose films. An amount equal to 50% of the nitrocellulose weight reduces the moisture penetration to about one-third of that of a straight nitrocellulose film of the same thickness.
The Santolites are soluble in and slowly decomposed by alkali solutions. They are not soluble in varnish and paint oils.
The Santolites are compatible with vegetable proteins (corn or soybean) but do not of themselves act as plasticizers. Mixtures of the Santolites with liquid plasticizers (for example Santolite MS with 50% of its weight of Santicizer B-16) do, however, impart excellent flexibility. The particular Santolite and the kind and amount of plasticizer will be governed by the degree of flexibility and other properties desired.
The Santolites increase the flexibility and toughness of ethyl cellulose. This is unusual in that they do not have a comparable effect on cellulose nitrate or acetate.
The Santolites are also compatible with polyvinyl acetate resins, increasing the flow at elevated tempera tures and improving the workability. In this they are materially aided by the addition of plasticizers, the solid plasticizers giving especially interesting combina tions, Such mixtures are convenientlv made bv si in pi' heating and mixing, thereby avoiding the use of volatile solvents. Of the solid plasticizers, Santicizer 10 produces the greatest effect. Diphenyl I'hthalate next and Santicizer 9 the least.
When heated, the Santolites give off a small amount of formaldehyde. They become harder, the melting point is raised slightly, and subsequent evolution of formalde hyde takes place only at higher temperatures. Nitro cellulose lacquers containing Santolite are not especially resistant to heat even though the Santolite may have previously been heated to a relatively high temperature. Compositions containing both nitrocellulose and Santo lite resins should not be subjected to temperatures much above 80 C. or rapid decomposition of the nitrocellulose mav occur.
Although the Santolite resins themselves may have a very slight odor of formaldehyde, that odor will not be present in compositions of Santolites with cellulose esters or ethers.
The Santolite resins are more light-stable than many of the natural resins such as rosin, ester gum, elemi or damar.
44 06U462
TOWOLDMON0038600
The Santolites are valuable as ingredients of heat sealing lacquers. Thev should be used in conjunction with a plasticizer, either liquid or solid, and by varying the amounts of plasticizer and resin, the temperature at which heat-sealing is obtained can be raised or lowered as desired. As an example, a lacquer containing 100 parts (by weight) of nitrocellulose, 75 parts Santolite MHP and 75 parts Santicizer H-16 gives excellent sealing at 103 C. If the resin and plasticizer are each reduced to 50 parts, a temperature of about 113 C. is required. When 100 parts of Santolite MHP and 50 parts of Santicizer 13-10 to 100 parts of nitrocellulose are used, again the sealing is excellent at 103 C. but if 100 parts of B-16 and 50 parts of MHP are used, the heat-sealing properties are poor even at 113 C.
Solid plasticizers usually necessitate the use of sealing temperatures about 10 C. higher than are required by the same amounts of liquid plasticizers.
Santolite K requires a lower proportion of plasticizer than Santolites MS or MHP.
The solubility of Santolites in various compounds is given on page 48.
60 lbs. cans (incl.)
Appearance and Color....... bight colored viscous liquid.
Free flowing above 20 C. Color not darker than AP11A 70 when 25 cc. of sample is dissolved in 35 cc. of normal butyl acetate.
Butyl Acetate (by weight) ...........................19.0 to 21.0'(
Composition (hy weight)....
80% Santolite MS 20{ i, Butyl Acetate
(Tolerances--19-21', solvent)
Santolite MS
Sp. Gr. (a 25 25 C. Ref. Ind. (a 25 C.
1.2098 .1.5448 (approx.)
r^/tecf^ica/ion^
540 lbs. net. Non-returnable galvanized drums.
Appearance and Color
Pale yellow viscous resin
Color of Benzene Solution
APHA 70 max.
(25 gins, in 50 cc.)
Solution in benzene (1:5) ............................................... Clear
Solution in benzene (4:0).....No crystalline deposit in 24 hours.
Refractive Index at 50 C........................1.5690-- 1.5720
Santolite MS is a soft, practically colorless resin made by the condensation of formaldehyde with aromatic sulfonamides. At temperatures above 50 C. it is a viscous liquid.
This resin, like all the Santolites, is compatible with both nitrocellulose and cellulose acetate and, being a
45
061't't6J
TOWOLDMONOQ38601
solvent for both, it can be used in any proportion. It forms brittle compositions with both these esters but the addition of a plasticizer makes such combinations permanently flexible. It is easily soluble in the common organic solvents and thinners except petroleum hydro* carbons. It is insoluble in varnish and paint oils. Santolite MS is excellent for water-white lacquers which will not be exposed to extreme weather condi tions, its high gloss and lack of color being unusual in the resin field. To facilitate handling, this resin is also supplied as a solution containing 80rc Santolite MS and 20f/c butyl acetate. This is known as "Santolite MS-80% solu tion" and is a free flowing liquid at temperatures above 20 C. It weighs about 10.1 lbs. per gallon.
Santolite MIII*
SfoecifiiceUionb
Santolite MHP is similar to MS in characteristics, except that it is a much harder resin, softening at about 62 C. and being brittle at normal temperatures.
It is nearly colorless and is well adapted to specialty lacquers, fabric coatings, molding compositions and the like. Being incompatible with drying oils it cannot be used as a varnish material. Exceptional features of this resin are the ease with which it may be worked into practically any formula using a cellulose ester and the wide variation of properties obtained by its use. Its high degree of solubility makes very concentrated solutions possible and its extreme compatibilitv with plasticizers and cellulose esters removes much of the danger of blushing, sweating and separation.
Santolite MHP can be used in spraying, dipping or brushing lacquers to make clear, colorless, odorless coatings of good gloss and adhesion. It does not materially increase the viscosity of the solution and permits the building up of a high solids content in the lacquer. It is compatible with all the common plasti cizers.
Although Santolite MHP, when used alone, does not plasticize cellulose esters, it does increase the flexibility of ethyl cellulose and produces very tough pliable compositions of great clarity and brilliance.
Appearance...................... Hard, practically colorless resin
Color of Solution .. (25 gms. in 75 gms. of 26 butyl acetate)
APHA 80 max.
Refractive Index at 25 C. (25 gms. in 75 gms. of 20 butyl acetate)
......................1.4280-1.4310
Penetration (200 gm. load for 5 seconds at 25 C.)
2.0 mm. max.
Santolite K
9D<m/a*nete
60 lbs. cans (inch)
Appearance. .....................Clear, light yellow, sticky resin
Color
....Santolite K Color Standard* 2.5 max.
40
06 1 6 4
TOWOLDMONOQ38602
Kefractivo Index al 50 ('. \<id Number
1.5330.1.5390 10 ina\.
Comparable in depth of color but not in shade to the Gardner 1933 Standard.
Santolite K-5
(lD<mdaineb&
55*gal. drums (approx. 500 lb.) (one time shippers.) 5*gal. tins (approx. 45 lbs.), (inel.)
Santolite K is a soft sticky resin with the qualities of both the sulfonamide and alkyd types. It is compatible with cellulose esters and ethers. Santolite K has plasticizing properties of itself but for most purposes additional plasticizer is desirable and Santicizer M-17 is recommended, although others may be used ad vantageously.
Santolite K is soluble in practically all common organic solvents except the petroleum hydrocarbons. It is not compatible with drying oils so cannot be used in oil varnishes. Santolite K has a better light stability than the other Santolites and is of special value for increasing the resistance to moisture penetration of cellulose ester compositions.
Appearance...................... Clear, light yellow, stick' resin
Color........................ Santolite K Color Standard 2.5 max.
Refractive Index at 50 C.
1.5420-1.5520
Acid Number.....................
10 max.
500 IbB. net. Non-returnable galvanized drums.
Santolite K*5 differs from Santolite K chiefly in being somewhat harder at normal temperatures, and having less plasticizing action. The addition to Santolite K-5 of 25% to 30% by weight of a liquid plasticizer such as Santicizer M*17 will give a product almost identical in characteristics to Santicizer K.
47 0614465 TOWOLDMONOQ38603
Solubility of Santolites
Alcohol
Ksters......
.
Ketones...............................
Aromatic llvdrocarbon6
Aliphatic Hydrocarbons
Acetic Acid Ghcerine .
.
Drving Oils
Fattv Acids .
Vinvl Resins
...........
Shellac......
Paraffin....................................
Carnauba Vi ax
Aroclor Resins......................................
..................Soluble. Films from solutions in all alcohols except methv! are
permanently wet or tackv. From mcthvl alcohol they harden slowly.
..................Soluble. Films from such solutions drv hard.
-
Soluble. Films from such solutions drv hard.
.................. Soluble. Films from such solutions drv hard.
Insoluble. Santolites produce coatings which are not attacked bv
gasoline or related products.
......... Soluble if the acid is over 72% (bv weight) concentration.
............... Soluble. Heat 1 part bv weight of Santolite MHP in 2 part* of
glycerine at 120 C. until dissolved. Then adjust the solution to the
desired concentration bv adding more glveerinc or Mill*.
Insoluble.
...............Miscible.
................... Miscible.
................. Miscible.
......... Insoluble.
Insoluble.
..............Partial!) soluble. 100 grams of Aroclor 4465 will dissolve 4 grams, of
Santolite MS. 100 grams of Santolite MS will dissolve 30 grams of
Aroclor 4465.
Table of Characteristics of Santolites
MS
MHP
K
Color and Form
1)oh Point*
Flash Point . Specific Gravity. Kcfractivc Index
................. ........... .....
Soluhilitx in Organic Solvents..
Solubility in Drying Oils Ketentmtv(*) in N/C......... Uctcntivity(3) in Ac C............ Acid JS'umber . .................................
(') Uoniintv Sunioliir K Color Standard. C
hut not in uliiuir lo (hr Oardnrr
Standi
' >nliil.lr in aromatic hydrocarbon* containing r*t*r, or chlorinated hydrocarbon,
Soft, pale \ellow resin
295 F. 1.355 at 25 C. 1.5690 to 1.5720
at 50 C. Insol. Gasoline
Insol. Over 100 Over 100 ....Neutral
Hard, brittle, nearly colorless lumps
310 F. 1.35 (approx.) 1.5080 to 1.5110
(25% in toluene) Insol. Gasoline
In6ol. Over 100 Over 100 Neutral
Soft, viscous resin; No. 5 max. color(')
Flows slow)\ at 30 C.
400 F. 1.307 at 25 C. 1.5370 0.003 at
50 C. (approx.) Insol. Gasoline
Sol. in other organic sol vents^) Insol. Over 100 Over 100 10 max.
(') Rftrntivity it given in parti per 100 paria by weight of the N/C or Ac. (.. * W hile Santolite* MS and K can beat be removed from container* by warming
10 the flow point, Santoliie MHP i beat removed by chilling and ibrn breaking into lump* by itriking the aide* of the container.
48
061AA66
TOWOLDMONOQ38604
The Aroclors
(Chlorinated Biphenyls)
General Properties
The Aroclors range in form and appearance from mobile oily liquids to fine white crystals and hard transparent resins. They are non-oxidizing, permanently thermo* plastic, of low volatility and non-corrosive to metals. They are not hydrolyzed by water or alkalies. The viscous liquids and the resins will not support combus tion.
The crystalline Aroclors are relatively insoluble, but the liquid and resinous products are soluble in most of the common organic solvents, thinners, and oils. The main exceptions are that all the Aroclors are insoluble' in water, glycerine or glycols and Aroclor 5460 is insoluble in the lower molecular weight alcohols. Aroclor 4465 is only partly soluble in the lower alcohols. The liquid and viscous resins are light in color while the hard resins are yellow. For almost every Aroclor
described in this booklet there is a dark-colored grade of otherwise approximately the same physical and chemical characteristics. These darker products carry a lower price and can frequently be used where color is not important.
The excellent electrical properties, fire resistance and inertness of the Aroclors make them useful in many applications not mentioned in this booklet. The information assembled here is restricted to that which is considered pertinent to the plastic and coating fields only.
The properties imparted by the Aroclors and their
usefulness for particular applications vary in regular
gradients over the series so the selection of the right
Aroclor for a specific use can generally be made simply
by a comparison of the physical properties of the
several Aroclors.
.
49
0614467
TOWOLDMONOQ38605
GENERAL PHYSICAL PROPERTIES
Form
........................................
Aroclor 1221
....... Colorless mobile oil
Aroclor 1232 Aroclor 1242 Aroclor 1248
Practically
Practically
Yellow tinted
colorless mobile colorless mobile oiiv liquid
oil oil
Aroclor 127
Light vellov viscous oil
Color --N PA
0.5 max.
0.5 max.
0.5 max.
0.5 max.
1.0 max.
Acidity--Maximum (Mgm. KOH per GJin.).. 0.01 0.01 0.01 0.01 0.01
Coefficient of Expansion ............ re cr C. 0.000707
(15'-40C.)
re co F. 0.000392
(50-104F.)
Density--
Specific Gravity 25 25C. (77 77F.)
1.177 to 1.187
Pounds per Gallon--25UC. (77F.)
9.82
0.000725 (2SM00"C.) 0.000402 (77-212F.)
1.262 to 1.272 10.51
0.000678 (25-65C.) 0.000377 (77"-149F.)
1.378 to 1.388 11.50
0.000702 (25-65C.) 0.000389 (77-149F.)
1.447 to 1.457 12.08
0.000661 (25-65C. 0.000367 (77-149F.
1.538 to Ui. 12.83
Distillation Range--ASTM D*20 Mod.. C. 2756-330C.
Corr.
F. 527-626F.
Corr.
Evaporation Loss--ASTM D-6 Mod.
163C....................
................... 5 hr*. --
100C.
6 hrs. 1.0 to 1.5
Flash Point--Cleveland Open Cup . .....C. 140.6C. F. 285.0F.
290-325C. CoiT. 554-617F. Corr.
--
1.0 to 1.5
152-154CC. 305-310F.
322-365C. Uncorr. 612-689F. Uncorr.
3.04 to 3.64 --
176'-180C. 348-356F.
330-370C. Uncorr. 626-698F. Uncorr.
3.0 to 4.0 -
193M96C. 379-384F.
365-390"C. 689-734F.
1.06 to 1.28 0.4 Nonr
Fire Point--Cleveland Open Cup
C. 176.7"C. F. 350.0F.
238C. 460F.
334C. 633F.
None
.None
Pour Point--ASTM
C. Crystals at 1C.
MF. Crystals at 34^.
--35.5C. --32 F.
--17.7 to --20.7C.
--5.2F.
--7C. 19.4F.
8 m 123C lb" in 54F.
Softening Point--ASTM ... C. - - - - -
Refractive Index--D-line--20C.
.. 1.617-1.618
Viscosity--Savbolt Universal 210F. (98.9C.) Sec. (ASTM--. ' ' 130 F. (54.4 C.)
100F. (3 7.8C.)
30.5
35.4 40.2
1.620-1.622
31.0-32.0 39.0-41.0 47.6-50.0
1.627-1.629
34.0-34.6 49-56 80-93
1.630-1.631
36.0-37.0 69-78 185-240
1.637-1.634 at 25C.
43.5-48.5
260-440 1800-3800
50 0614468
TOWOLDMONOQ38606
OF SOME OF THE AROCLORS
UocLOR 1200 Aroclor J262 Aroclor 1208 Aroclor 1270
Liflil yellow oft Micky rrin
Light yellow sticky clear resin
Pale vellow
While crye-
opaque brittle taline powder
resin
Aroclor 4465
Yellow trans parent brittle resin
Aroclor 5442
Yellow trans parent sticky resin
Aroclor 5460
Yellow trans parent resin
Aroclor 2565
Rrown-idaok opaque resin
I n max.
1.2 max.
1.5 max.
-
2.0 max.
u oir> 0.02
0.175
0.05
0.028
0.07
1.26
0.000640 (25-90C.) 0.000355 (770-194F.)
0.000611 (25~65C.) 0.000339 (77-149F.)
0.00123 (25-99C.) 0.000683 (77-210F.)
0.00179 (25-124cC.) 0.000994 (77-255F.)
0.000656 (25~65CG) 0.000364 (77C-M9F.)
1.018 t 1.629 1.646 to 1.653 1.801 to 1.811 1.914 to 1.960
13.30 13.72
15.13
16.21
1.712 to 1.723 14.28
I.432 to 1.447 II.96
1.740 to 1.745 14.50
1.724 to 1.710 14.41
Wje-420C. '-'}^788F.
373~404C. Uncorr. 703-759K. Uncorr.
-
4j0-160C. 812o-860F.
Requires
vaeumn Requires vacuum
Requires vacuum Requires vacuum
-
I| (' to 0.2 Viir
0.48 to 0.56 0.15 lo 0.24 0.0 to 0.1
None
None
None
0.23 to 0.29 None
2.0 0.0)2
247C. 477F.
0.025 1.51 to 1.71
(t 260"-S br.)
None
0.21 to 0.21 None
Vlllc None
None
None
None
> 350C. > 662F.
None
None
'V i 36C.
34.9 to 38.0DC. --
46C.
lu 97K.
95 to 100.4F. -
135 to 160CC. 294 to 300 C
(hold pt.)
(hold pt.)
- 275 to 320Ir. 561 to 572F.
(hold pt.)
(hold pt.)
60 to 66 C. 110 to 15TF.
115F. 48.5 to 53C. 119 to 127F.
-100 to 105.5C. 66 to 72(7. 212 to 222 F. 140 to 162F.
1.6501-1.6517
- 1.661-3.667
3.660 J.665
"82 ^-4300
90-103
-
600-850 at 160eF
-
02-156
or IHO'C )
313.5
51
Obi*, 969
TOWOLDMONOQ38607
Chlorine Content of Pure Chlorinated Biphenyls*
Chlorinated
c
Biphenyl
Chlorine
Monochlorbiphenyl Dichlorobiphenyl Trichlorobiphenyl
18.8 36.8 41.4
Tetrachlorobiphenvl Pentachlorobiphenvl
48.6 54.4
Hexachlorobiphcnvl
59.0
Hcptachlorobiphenyl Octachlorobiphenyl Nonachlorobiphenvl
62.8 65.9 . ' 68.8
Decarhlorobiphenyl 71.1
*Tlie Aroclors are mixtures of two or more cblorobiphenyls and some contain chlorinated terphenyls.
Aroclors. Although every Aroelor is not included, the chart covers a sufficient range and displayed such definite trends as to permit assumptions to be made regarding others of the series.
Fig. 9
Specific Volume Ofafoclop 124Q ml./gm.
The Aroclors are compatible with most of the common plastic materials (see compatibility table on this page). The degree of flexibility imparled by the Aroclors diminishes progressively in the order of liquid Aroelor* soft resin-bard resin. The hardness of the resulting compositions increases in the same order. Usually a satisfactory balance between flexibility and hardness can be obtained either by selecting the Aroelor of proper physical characteristics or by using a mixture of two or more Aroclors.
The following compatibility chart will give a fairly good idea of what may be expected from any one of the
TMPEPfiTL/e DeCPE3 c.
Nitrocellulose
Cellulose Acetate
Cellulose Acetopropionate .
Cellulose Acetobutvrate
Kthyl Cellulose
Benzvl Cellulose
Polyvinyl Acetate
Polyvinyl Formal .
Polyvinyl Acetal
Polyvinyl Butvral
.
Polystyrene.....
Chlorinated Rubber ...
Compatibility Table______________________________________
1242
100 PHR
1
C
C
C
c c c c c c c
1254
100 PHR
1 c
<:
c c
too PHR
C
c c <: c
1262
50 PHR
1 I
50 PHR
C
C 1
100 1*11R
C
100 c c
4465
1 I 1 c c 1
50 PIIR 100 PHR 100 PHR
C
-C
5460
I I
I
c
c
1
50 PHR 100 PHR 100 PHR
C
c
C--Compatible in ail proportions I--Incompatible PIIR--Parts of Aroelor by weight per 100 parts plastic base.
The Aroclors are compatible also with coumarone-indene resins, ester gum, rosin, damar, rubber, asphalt, paraffin and sulfur. They are compatible with "A" and "B" stage phenolics but not with the completely cured resin. Aroclors are incompatible with manilla gum.
52 061^70
TOWOLDMON0038608
Solubility of Aroclors in 100 Milliliters of \ ariou* Solvent'
Aroclor Tvpe of Solvent
12-12
Cold
Hot
1248
Cold
ll.x
12 >1
C dd
li-t
1-"
<-.,.d
ha
Ariel Aortic Arid .
, SS
, ^^
Oleic Acid ...... Benzoic Acid ...........
S 10.0 31 1
S
1; 10.0 3- '
'' --
"* ` - --
Aldrhvde 40% Formaldehyde.........
II
. l
., 1l
,.
Furfural..........
VS VS
' '*
' '
s' s''
Amine Aniline.......... Pyridine....................
^.
.S
S
--
.......
132.3 "< MO W'
-
--
H I " 1 12..'"'............................
Chloro -- derivative
-\invl chloride* -- mixed Carbon Tetrachloride
SS SS
.
Ss SS
,,
S> S>
' 8.0>
Chloroform .............. Dichlorelhvlene
SS
SS ./
S* ;.
-*-0'*
Ethylene Dichloride Monochlorohenzene........
Ss SS
s -s Ss
"! \ SS
" -.8
Orlhodichlorobcnzene Tetrachiorethane.....
"* SS
' S>
" ", SS
"
'1'rirhlorethane.... Trichlorelhvlene.....
.S .S
$ S
Ss SS
^c S.
Drying Oil Tung Oil ...... Linseed Oil
ss ss
s s
Enter
Amyl Acetate...... Butyl Acetate......... Celloaolve Acelale. Cottonseed Oil ......
ss s
ss ss
s s s s
Dihutyl Bhthalate Diethyl Bhthalate F.lhyl Acetate...... . Fthyl Lactate .......... Lthvlene Glycol Diacelate Methyl A relate Tricrenvl Blioophatr .
Kther: Ethyl Ether
ss ss ss ss ss ss ss
s s s s s s
Ether Alcohol Carhitol.....
CrlWolvc.
224 >*t\ 30" 9(,'css
vs s
VS
s
Diethvlene Glycol f`p' Dihydroxy Fain f Ether
16.9 23*c 19 WA'
ss
y
)|) mo*c. -
Hydrocarbon
Benzene .................
Gasoline..............
Kerosene.........
Mineral Spirits
Baraflin
Bine Oil.........
'
Toluene.............
Turpentine
Xylene.................
Hydroxy -- derivative
Amyl Alcohol ....
n-Bulyl Alcohol.....
Fthyl Alcohol (3-A)..........
Glycerin................
Methyl Alcohol
Bhenol -- 90%......
Ketone
Acetone......................
VS
AS
AS
VS 2.0 s
VS VS VS
VS vs vs VS s s vs vs vs
.S
s
ss
23.3 29*c 80.0 TM*<'
4129.45 K29f`cc.
88.5 *rc. s
.S
s
vs vs vs vs 2.0 23` vs vs vs vs
__ --
--
-- -
AS
vs vs vs
I
vs vs vs vs VS \s VS VS .... s ss AS vs vs vs vs vs
3.:* -
-
-- --
ss
----
10 WC- 28 TM*t\
---
II
II
1320*0 22.2 8S*C- --
--
ss "'s --
ss
- -
Miscellaneous Carbon Disulfide ... . Nitrobenzene.............
Water.....................................
ss
SS
II
-- II
ss ss II
---- -- II
I -- Insoluble
S -- Soluble
SS -- Slightly Soluble
VS -- Very Soluble
Figures show grams of Aroclor per 100 milliliters of solvent at 23C. unless otherwise indicated.
53
I to'.
(...Id
h":
SS s
s vs
II AS VS
VS AS AS AS
A S VS VS V> AS AS VS V< AS AS VS V> VS VS
vs a;
VS A S VS AS
AS A S AS VS
VS VS VS AS vs VS S aS
s vs s vs
S VS
VS AS VS vs ss ss s
ss s s ss
vs vs vs AS < 5.0 s vs
VS AS
s ss ss 1 ss
vs vs vs vs s s vs
AS AS
s s -I --
ss
VS VS
vs II
TOWOLDMONOQ38609
DIAGRAMS SHOWING PRACTICAL COMPOSITION
For combinations where the resin is ester gum or Amberol and where the Aroclor is Aroelor 1254 or Aroclor 1262.
54
061^72
TOWOLDMONOQ38610
OF LACQUERS USING AROCLORS 1254 AND 1262
In the trilinear diagrams the compositions, represented b\ anv point in the unshaded areas, are those which produce homogeneous lacquer films. On the other hand composi tions represented by points in the shaded area? produce impractical, segregated, brittle or soft films. For detailed information as to the derivation and use of these diagrams reference is made to the following articles:
Jenkins & Foster, "Compatibility Relationships of the Aroclors in Nitrocellulose Lacquers," Ind.
Eng. Chem. 23, 13(>2 (1931).
'
Hofmann & Reid, "Graphical Methods in Lacquer Technology," Ind. Eng. Chem. 20, 431 (1928); "Formulation of Nitrocellulose Lacquers," Ind. Eng. Chem. 20, 687 (1928).
55 061 <,4 73
TOWOLDMONOQ38611
Fig. 10
Va p o r P r e s s u r e -
56
061^^7^
TOWOLDMONOQ38612
SUGGESTED USES FOR AROCLORS
Nitrocellulose Coatings The Aroclors function both as plasticizers and resins and inay be used alone with the nitrocellulose or in combinations with other plasticizers or resins. They impart weather resistance, luster, adhesion and de creased burning rate. Their excellent electrical char* acteristics (high dielectric constant and resistivity and low power factor) and their property of retarding* the passage of moisture and gases through nitrocellulose films make the Aroclors of special value in coatings for electrical insulating materials.
The accompanying trilinear diagrams show the practi cal compatibility limits of Aroclors 1254 and 1262 when used in conjunction with some other resins and plasticizers. Aroclor 1260 gives values almost the same as those shown for 1262. The legs viscous Aroclors have greater and the more resinous Aroclors less compati bility than for those showrn. (See trilinear diagrams on pages 54 and 55.)
To illustrate the differences possible to obtain by changes in formulation, three formulas are given below. All have excellent durability but the third is much
softer and more flexible than the other two. Onlv the solids contents are given. The amounts tabulated are parts by weight.
Aroclor Lacquers
No. 1 No. 2 No. 3
Yl second Nitrocellulose (drv) Damar resin............................. Ester Gum..... Aroclor 1260.......... Dibutvl Phthalate..........
Tricresyl Phosphate.........
100 80
--
20-39 20- 0
--
100
__
80 20 20
--
100
-- --.
80-70
39-70
No. 1 and No. 2 have excellent sanding and polishing qualities. No. 3 is very flexible but too soft for sanding.
Where extremely high flexibility is desired, as for example in lacquers for high tension automotive cables, the following composition is suggested:
15--20 sec. R. S.
Nitrocellulose........
.8 parts by weight
Tricresyl Phosphate......................... 10 parts by weight
Aroclor 1242..................................... 7 parts by weight
Fig. 11
TEMPERATURE DEGREES C. 57
06 1*1*1 7 5
TOWOLDMONOQ38613
Chlorinated Rubber Finishes
Aroclors 1242, 1254 and 1260 are recommended as plasticizers for chlorinated rubber. They give tough flexible compositions and may be used alone or together with the resins and oils commonly employed in chlori nated rubber formulations. From 40 to 60 PIIR are suggested. The Aroclors arc especially valuable as finishes for alkaline surfaces 6uch as concrete, brick, stucco, etc., and for acid and alkali-resistant coalings.
Etbyl Cellulose
The Aroclors are very compatible with ethvl cellulose, the liquids imparting flexibility and the resinous products, hardness. 7,5 PIIR of Aroclor 1242 produces great flexibility and just a slight tackiness. Aroclor 5460 in the same proportion produces a very hard and somewhat brittle composition. Aroclor 4465 produce* hard films which are not brittle at ordinary tempera tures.
For coatings of high glosg and exceptional weathering qualities, to be applied to rigid surfaces, compositions containing equal parts by weight of Aroclor 5460 and etbyl cellulose are suggested. If greater flexibility is required, one of the softer Aroclors should be used, either alone or as a replacement for part of the Aroclor 5460 and the proportion of Aroclor should be decreased.
Inks The Aroclors are U6ed as vehicles for carrying pigments
used in glass decoration. When the decorations have been applied and the glass is fired, the Aroclors vola tilize without carbonization and thus avoid discolora tion of the glass. Aroclors 1251 and 1465 are used.
Moisture Proofing
For use as moisture-proof coalings, the Aroclors are best combined with waxes, such as paraffin or carnauha, oils such as mineral oil, and resins such as ester gum or other synthetic resins. The simplest compositions contain only Aroclor and paraffin. A moisture-proofing compound composed of 96% (by weight) of Aroclor 5460 and 4% of paraffin (melting point 54 C.) has an ASTM softening point of about 82 C. and is very efficient. Substituting Aroclor 4465 for Aroclor 5160 produces a compound with a softening point of about 58 C.
Softening point and viscosit\ when melted mav be further decreased bv using mixtures of Aroclors. For example- a composition containing 40' , of Aroclor 1260, 56f '(. of Aroclor 5460 and 4% of paraffin will he very soft at ordinary temperatures. Increased propor tions of paraffin will also produce softer compound-.
Impregnation
The Aroclors may be u&ed to impregnate cloth, paper, wood or asbestos in order to impart moisture and gas resistance, adhesion, insulating properties, alkali or other chemical resistance, flame resistance, or lubri cating qualities. For tins type of work thev are used in combinations with other materials such as waxes, inorganic pigments, asphalt, tars, aluminum stearate, sulphur, etc. in order to obtain exactly the physical characteristics desired for the specific purpose. Aroclors 1254, 4465 and 5460 or the corresponding dark-colored products are suggested as most applicable.
Mold Lubricants
Recause of their inertness and low volatility, the Aroclors are excellent mold lubricants. As an example the addition of 1% of Aroclor 1242 or 5160 to a polvvinvl formal resin increases the ease of molding operation as well as improves the appearance of the molded pieces.
The Aroclors are equally applicable to other molding compositions, the particular one to he selected and the method of use being governed, of course, bv the molding material and the conditions of operation.
58 061't'(7o
TOWOLDMONOQ38614
1`iiinls mid Vnrnishos
The Aroclors arc soluble in paint ami varnish oils and
impart properties corresponding to the physical
character of the particular Aroclor. The hard resinous
Aroclors tend to give increased hardness to the films
while the viscous resins impart flexibility.
.
The Aroclors do not react chemically with oils, hence there is no advantage in heating together in making a varnish. They are best added as a "chill back" or as a cold cut in the thinning operation. As far as incorpora tion of the Aroclors is concerned, the only reason for heating is to make the Aroclors liquid so that they can he readily mixed with the oils.
Aroclors 4465 and 5160 will produce paints that are very quick drying and \ct have excellent durability. The weight of Aroclor used should be from 30% to 50% of the weight of the oils.
Aroclor 1260 is best for short oil varnishes that are required at the same lime to be flexible. The Aroclor may be considered to play the same role as oil. with the difference that it docs not oxidize and lose its flexibility on exposure. Resins of the alkyd, phenolic or ester gum t> pe or a harder Aroclor such as 5460 may be used in making varnish formulations. It is suggested that for two parts b> weight of oil, one part of Aroclor 1260 and one part of varnish resin be used. These propor tions can be varied as required. The Aroclors impart water and alkali resistance and in these qualities en hance the value of the other resi6 used in the varnish.
IMgment
Aroclor 1270 is a hard, white crystalline product of high im-hing point, insoluble in most solvents, resistant to chemicals and to oxidation. When ground to a fine powder it makes an excellent organic pigment for use with the various plastics. It may be used alone or with con\ entiotial pigments.
Rubber and Rubber Substitutes
The Aroclors, when in a liquid condition, have a solvent action on rubber. Aroclors 1254 and 1260 are milled into rubber in order to impart permanent tackiness and adhesion. A small amount of Aroclor 1260 added to hard rubber acts as a plasticizer and reduces the brittleness.
Aroclor 1270, being a hard crystalline material of high melting point, can be ground to a powder and then milled into rubber. The milling temperature being below the melting point of the Aroclor, the latter is dispersed through the mass of rubber and acts as an efficient flame reducer. This 6ame procedure can be used with the so-called synthetic rubbers (such as neoprene) to impart fire-proofness. From 5 to 25 PHR of Aroclor 1270 are required.
Vinyl Resins
The Aroclors are compatible with all the vinyl resins. The properties imparted depend upon the particular Aroclor and the vinyl resin used. The selection of the correct Aroclor for a particular use can usually be made bv consideration of the physical properties of the Aroclor scries.
50 061447?
TOWOLDMONOQ38615
I'hf information contained in this booklet is, to our best knowledge, true and accurate, but all recommendations or suggestions are made without guarantee or liability on our part, since the conditions of use are beyond our control. Furthermore, nothing contained herein shall be construed as a recommendation to use anv prod uct or process in conflict with existing patents.
Monsanto Chemical Company
ORGANIC CHEMICALS DIVISION St. Louts, L. S. A.
0O1AA76
TOWOLDMONOQ38616
Monsanto
Chemicals Plastics
061AA79
TOWOLDMONOQ38617