Document RaymQ9y4DDDeezNg1zaEm7nvz

TOWOLDMON0025117 WATER_PCB-00009586 MbD ff BIEtenDte SECTION A TRANSFORMER ASKARELS............................ '............ .1 I. Introduction......................................................... ,1 II. History of Trade Name Types........................ .1 Table I - The Composition of Transformer Askarels .............................................2 III. Interchangeability .................................................. 2 IV. Table II - Official Transformer Askarel Shipping Specifications.......................................... 3 V. Ordering Instructions............................................. 2 VI. VII. Stability...................................................................... 2 Precautions When Handling Drums. Tank Cart and When Opening Transformers.......................... 2 A. Keep Dry During Handling .............................2 Table III - Handling and Pumping Temperatures.....................................4 6. Use Ordinary Personal Precautions ...............4 C. Precautions on Opening an Askarel Transformer.......................................... 5 VIII. Avoid Environmental Pollution.............................6 1. Labeling Askarel Transformers.......................6 2. Disposal of Liquid and Solid Wastes ............6 3. Conditioning of New or Recycled Askarel .6 4. Teardown of Transformers for Repair or Scrap ................................... .7 5. Transformer Disposal........................................7 IX. Expected Service Life............................................. 7 X. General Characteristics of Transformer Askarel Fluid..............................................................7 XL Sampling Transformer Askarel Fluid .................. 8 XII. XIII. Evaluation of A&arel Received In New Equipment......................................... Dielectric Breakdown Voltage -- .8 Moisture Relationship............................................. 0 Table IV -- Relation of Dielectric Breakdown Voltage to Amount of Dissolved Water in XIV. XV. Askarel and Mineral Oil................................... .9 Table V - Approximate Solubility of Water in Transformer Askarel and Mineral Oil .... 10 Turbidity................................................................. 10 Check Points for Maintaining Askarel Insulation ................................................ 10 A. General Considerations...................................10 B. Modern Sealing Procedures ...........................11 C. The Older Sealing Arrangements.................. 12 XVI. Periodic Fluid Inspection and What Checkpoints Mean ..................................... 12 A. Visual Inspection..............................................13 8. Dielectric Breakdown Voltage .....................13 XVII. Inspection Checklist..............................................13 XVIII. Contamination in Transformers........................... 14 Table VI - Effect of Common Insulation Materials on Power Factor and Dielectric Strength................................................ 14 Table VII -- Effect of Common Insulation Materials on Volume Resistivity XIX. of Askarel................................................................. 14 ASTM Method for Investigating the Compatibility of Transformer Insulation and Construction Materials In Askarels.............15 XX. Refining Askarel for Re-Use................................ 15 A. Filtering Through Dry Blotter Paper to Remove Moisture and Extraneous Particles........................................ 15 XXL XXII. Table VIM - Water Removal by Filtering Askarel Through e Piper Press .......................... 16 B. Dispose! of Solid Wastes............................... 16 C. Solid Insulation Requiring Drying...............16 D. Earth Treatment for Maximum . Improvement of Power Factor end Volume Resistivity ........................................16 Table IX ~ Effect of Power Factor end Volume Resistivity .......................... 17 Cleaning Arced Transformers...............................17 Sampling Askarel.................... 17 SECTION B ASKAREL FILLED SWITCHES AND TERMINAL CHAMBERS ...................................... 19 I. Introduction........................................................... 19 II. Sources of Contamination.................................. 19 III. Sealing Switches and Terminal Chambers .. .20 IV. * Askarel Used Under Mild Arcing Conditions .20 V. Maintenance for Askarel Filled Switches ... .20 VI. Askarel Under Excessive Temperature or Fault Conditions ............................................21 SECTION C TOXICITY AND SAFE HANDLING................................21 I. Inhalation................................................................21 II. Skin Contact................................. ....................... 21 SECTION D ANALYTICAL SERVICES ON TRANSFORMER ASKAREL AVAILABLE FROM MONSANTO ..................................22 Types of Analyses Available: ............................................. 22 1) Routine Maintenance Check........................................22 21 Complete Analysis........................................................ 22 31 Analysis After Earth Refinement .............................22 SECTION E APPENDICES......................................................................... 23 Appendix A - Askarel Stability and Composition of Arc Formed Gas..................................... 23 Appendix B - Solubility of Gas in Transformer Askarels ........................................................ 23 Appendix C - Effect of Temperature on Dielectric Breakdown Voltage of Askarel .....................23 Appendix D - Comparison of the Approximate Viscosity In Seybolt Universal Seconds of Transformer Askarels and Mineral Oil.............................24 Appendix E - The Density of Inerteen 54201 KA 7336-9 end Transformer Pyranol A13B3B-3..............................................................24 Appendix F - Thermal Conductivity Values of Transformer Pyranol A13B3B-3............. 24 Appendix G - Heat Capacity............................................. 24 Appendix H - Coefficient of Expansion.......................... 24 Appendix I - Fire Resistance............................................. 24 Appendix J - Seals, Properties and Procurement ................................................................ 25 Appendix K - Caution Label............................................. 25 NOTICE: "Nothing contained herein is to be construed as a recommendation to use any product in conflict with any patent. MONSANTOMAKESNOWARRANTIES AS TO THE FITNESS FOR A PARTICULAR PURPOSE OR MERCHANTABILITY OF ANY PRODUCT REFERRED TO, no guarantee of satisfactory results from reliance up on contained information or recommendations, and dis claims all liability for any resulting loss or damage." 1 i i 0205413 TOWOLDMON0025118 WATER_PCB-00009587 C> 7 i A-V-: < 7:>v-/.-*'o';-' A-: ' V*'**-'* ,` v v --` V i" i; v r>': v>' -; 4:fv Vv-./-v4v .: >>V: ','54-.' ' pW, t- r - 'v :';*V V- |^4 ; Transformer . . . . . Askarel &*\r -.\ . .- `Si'fJ. '.V/i..-' , S^: :r: v.- i/V=:'* I. Introduction - V The term "askarel" as defined by IEEE, ASTM and the National*1 Electrical Code generally describes a broad class of fire resistant*; synthetic chlorinated hydrocarbon insulating liquids widely used in ' . transformers, reactors and accessory equipment operated at power,% frequencies. Askarets of various compositional typos are In use. (For the *; general properties end types see ASTM 6-2283.) Under arcing - conditions the gases produced, while consisting of predominantly non-combustible hydrogen chloride, can contain varying amounts of , combustible gases depending upon the askarel type. * . t ' i* S . , ' '' , '. . This manual describes the operating characteristics of transformer askarel liquid insulation as manufactured by Monsanto and how It Y differs from mineral oil. Appropriate handling and disposal procedures for both scrap askarel liquid and Impregnated solid materials aie given : > in accordance with the guidelines recommended by the American' s- V National Standards Institute. . ; : , *1 -v The Information Is based on facts gathered by Monsanto over 40 years ' as a producer of askarel, plus knowledge gained from the experience - , - of transformer manufacturers and users. This guide outlines the *. ; maintenance required for askarel fluid In "modern" transformers and -- offers suggestions for sealing and maintaining askarel In old units. By '* - following this guide, we believe users will obtain maximum service from . askarel insulation with a reasonable minimum of maintenance. If - questions arise relating to the designing and building of transformers, these should be referred to regular transformer suppliers. - .M <!-, . yV $P44Y;:' Y lY:v\ Vv' .-: ': .Monsanto gratefully acknowledges the assistance, guidance and the' ., contributions of certain data by the following:: * > . ' -y Edward L Raab - General Electric * \ ''r- ; .. . w, Dr. T. K. 9o8t - Westinghouse Electric . . . -t , ; / ' II. History of Trade Name Types ......................... 4 "Askarel" is the generic name for the fire-resistant liquid Insulation '; and coolant first used by General Electric Company in 1932 for their ;. Pyranol1 brand name fire-resistant transformers, Westinghouse Electric V Corporation uses their brand name, Inerteen.2 J t L ' 1 '.:\r' Ids/ .* ' { V .* k 'jfst-S`7Xr<:, -:U-, .\\-v oi', V;-M'.r'A^' 4!' Whatever the trademarked brand, the askarel contains chlorinated biphenyl -- one of the best liquid insulations developed by science. This*. *y t Inert material Is chemically ' stable, fire-resistant, heat stable,- ' non-corrosive, and has high dielectric strength under the operating/ . conditions encountered in transformers. , Y' : . x. In addition to manufacturing . Aroclor* {chlorinated biphenyl), Monsanto also mixes this dielectric fluid with chlorobenzenes to produce the presently used Inerteen and Pyranot blends described in Table I. , . , , * " . "NOTE: Materlali detignatad 'fire reilstert' generally ra more difficult 10 ignite, or once ignited, burn at a slower rata then coretending convention*! ' material*. This t*rm does not mean that fir* rtist*nt metarlali will not burn. / However, when properly used, Monsanto'* fir# resistant ASKAREL FLUIDS ere ` , > useful in helping cuttomeri meet their fire safety requirement!."-^ ^Trademark of General Electric Compreny ^ 'trademark of Westinghouse Electric Corporation - ' Registered trademark of Monsanto Company ' 4 020^^1^ Stott/ij>.Livi. i:.t ,i'ii v i.; i'v___ n TOWOLDMON0025119 WATER PCB-00009588 fe.yv \' ASTM Method D-2283, titled "Chlorinated Aromatic Hydrocarbons Tf&A'.lAskarali) For'' Transfonryan", also Hit* the composition of all' 'transformer asketels used at versus times since 10JJ2.4 < ,, V Jl y Monsanto manufactures similar transformer askarel fluids In England Sr; wfiere the trade name Pyrooor it used. . * , , ; 1 . : , V i ' ' V ' . ' \ . ' * \gi' III. Interchangeability. .In general all transformer askarels are interchangeable. However, it is V' suggested that the transformer manufacturer be consulted prior to y. 1 mixing in liprifieent proportions or total substitution. ,, ;V. IV. Transformer Askarel Specification* . ' .'* : Specifications for tlie three modern transformer askarel fluids are, ', shown In Tabt II. ^\ ; t ; ' ' ' V. Ordering Instructions !\ Monsanto's current policy is to sell askarel transformer fluids only to j' y transformer manufacturers. Others interested In these fluids should. contact the manufacturers of askarel transformers and not Monsanto. ^ , Tha translornrer name plate Indicates the transformer maker and usually gives sufficient dau to identify the specific askarel fluids used, VI. Contamination \T\\ Askarel insulation must never be mixed with mineral oil. Over two percent of, mineral oil by Volume in askarel begins to lower Its fire \ v'lrt" modern transformers, ihe principal "enemy" of askarel is ..contamination by water,; Keeping askarel. water-free will Insure M;'Jong time service, v i *.'^r - vv' ' ; i'.* ' : v ' j, .'Askarel Is heavier than water. If water gets into askarel insulation, only \fc-a tiny amount {approximately 126 ppm) dissolves - the rest floats on 2 top. Askarel in very insoluble In water, only about 200 parts per billion ftjr'&f askarel dissolve In wfctet, at normal temperatures. > ; . 'y / jt ' t ' _ v ' ' ' , ' ' '' " jy v VII. Precaution* When Handling Drum*, Tank Car*, and When , ft* -Opening Tranfformeri ''; . . ;U/Thf following art significant precautions: i * \ , .-v SKt'Or* ' ' .. ' hJ-A^fKeep Dry During Handling: '' in handling, storing, sampling and Inspecting askarel and in m1 "' mm. TOWOLDMON0025120 WATER_PCB-00009589 ..< ^;.J.,X.,W'O- '*# - ' **-''. ... ' C ?' '*"' ,? . " V " S*'' * ,, / " *> - ^'T.J.M - --.W^^'&ffy .. -' _ - -' ' ' .---.-n-'--- .*-.' ' -''--- - -T. ' *** .* . Trernfocrrser Aakarel Speoifrcetiom (New Fluid) - Spcrf'citioo Properties1 '; - . General Electrie Co. . Trantformer . Pyrenoi A13S3B-3 ; ASTM D2283 Type G ,--V- 'j_. Wettinghouae `^,1 . Transformer ,* Irtertaan 7&-30* ' ' ASTM D2283 Typa D - v Westmghoute *Cj-iV~T..' \ Tranaformer -l* . '*C .` Inerteen 100-42*', T- - --, ^ ASTM D22S3 Type 6 \'^y > ,;'J!'Cotor,'APH'A ^.-'^Co^dition ,- V '. ' - ';' Water content, ppm fASTM D1533-60? . '-VAcidity, mg KOM/g (ASTM 0974-55] v. / DieiectncStrength. 25C, 0.1 in. gap -t - (AS*M 0877-49) : -~ ' -2Dielectric Constant, 10C"C,60 Hr . (ASTM 0924-49) ' .' - -'--Volume Resistivity. 100"C, -' : - 500 volts 0C 0.1 inch gap. IQ9 ohm-cm ` (ASTM D1169) -' Inorganic chlorides. pom (ASTM 01821 and G.. Method E4C41B) - ' Refractive index, 25*0 (ASTM 01807) ' - Viscosity at 37.S*C (ASTM 088-56) _ Saybott Unrversa'Seconds - ' Pour Point *C (ASTV D-97-57) .. ,v. Specific gravity 25/15.5C (ASTM 01810) . Burn point (ASTM D92) '. ' .'.Distillation range (ASTM D20-56) corrected -- for stem and barometric pressure , 150 max. >. Clear 30 max. _ . 0.014 max. ,, 35 KV, mm : - '4.2 to 4.6 too . . . 0.10 max. .... ' 1.6110to 1.6120 ' 44 to 48 -38 or lower - ' 1.495 to 1.510 None to boiling - 1st drop 20CTC min. ' ; 40% max. below 270*C - 90% 379 to 394 - : 150 max. . "-''`-,3^^'*' Clw 30 max. - 0.014 max. C---l-e--a-r . 35 max, fjj'n.r *r%:. I.v.- '0fl.0ft1l mrna.x. y..-- . ]-35 KV, min. 435 KV, mm, V . 4.2 to 4.5 7 4.7 to 4.9^ f v' 100 . '. 0.10 wax. ' 1.6153 to 1.6173 -56 to 61 - - -30 or lower ; .1.5T8to T.528 None to boiling 1st drop 200*0 mm. .; 35% befow 270C . .,90% 379 to 394 100 ' ^ ^ 0.05 max^ v .. .T6240 to 1.6260 . 82 to 92 - ' - -17 or lower ; t.381 to 1.392 : None to boiMng .'10% 325*Cmin. 90% 360 max. & fixed chlorine . / .-.V Corrosion test, : / ' ^Cokjr.APNA */\ V- _ Ac'd'TY. mg KOH^g - - Inorganic chlorides ppm . ` ' Condition __ - -Scavenger content .- * . 'Typical Properties* .... - Coefficient pf ThermaJ Expanjxpn IASTM D1903), cm?/cm2/C ; Arc formed gases .'. lhm their private number ln*rteen SaZuiXA ?or irwrt** 70-5C and the* orrvats mnrX>w lntwn M201CM for Inerteen 10042. 56.4+0.5% ." 55.6% min. . * 43 i.0.5% ' After heating with aluminum for 6 hr*, at 200 to 220*C, the aluminum must not be corroded on either visua1 or weight inspection and the askarel should meet the following specifications: _ 200 max. 200 max. _ 200 max. _ ' * 0.Q14 max. ,, V ' . 0.014 max, t " . 0.01 max. . ' . . ' 0.15 max. Clear - ' . 2.0 max. ' ' ' 'v Clear . ' - . '0.15 max. ' Clear , - 0.115 to 0.135% ` 0.18 to 0.22% 0.18 to 0^2% . Diepoxide pfienoxypropene oxide phenoxypropene oxide 0.0007 f - 0 00068 : AUcrl| of ranous comdowtonal rycw* r* uwd. Under arcing condition* th* ga*s produced, whila consisting pn>dominant!v of non<ombust'bl hydrogen chlor*d*. Can include varying amounts of COmOust'bl* g* depending . upon the atkare1 type. lmuijuon *y*tem* incorporating these esfcerels and celluJotic or other organic materiel* may. whyn arced, oroduce Qaseoos which ary moderately ernmebJe. A* a precaution, such gases should be remowwl horn the askarel by bubt>i*ng dry nitrogen through the eskarvi and flushing the gas spec* w-th dy nitrogen prior any work n <j*> ih* aoo*<*ue- . . ' - - _ - ----- . _. _ . Jjheea quantities are final Wes epaertication* only to the aatam that they coincide with Monsanto's pttbMwd octficetion*. , ;_ -r.. ` *Th^ data d bawd Upon mn-v** teased Wi the laboratory end l not guarentaed for all wrr**< Write ee for eonplete wtae vecsfleatione for Aekarel fluid*. TOWOLDMON0025121 WATER_PCB-00009590 iret'-K- operating askarel transformers - taka tvary precaution to guard *8"%the askarel Emulation*v f*ro* *m exposure to high humidity and moisture contamination. -.Keep 5 or 55 gallon drums of askarel [^` -'dry; lay stored drums on their sides with the bung at the highest j^{: point from floor to keep water off the drum heed (which can be ft^VyJ.tucked into the askarel by the drum "breathing''). This precaution : RvS*1 ^ hecessary whan drurrn ara stored Indoors, which H tha m,preferredpiece forrtwafla;4^^^A;Vr^^'>;-*i s ` '* ' 7 4?</ ' ,*' V*' '. V j >:.$^To avoid laakaga the drums used for 'askarel are of heavy': > ^^construction. Sixteen gauge metal is used, with special rim seal and ;'; Kvbung construction. This drums, should be drained as completely bi ' ^^possiblt end then flushed twice with kerosene type solvent to 5 'remove all 'of the askarel. Accumulated liquids and.washings should ba collected and should be Incinerated at high r.A s temperatures, e.g., about 2000*F, to destroy the polychlorinated % j^^^blphenyls (PCBs). See Section A, VIII., :V; O', *. -* V , Tank cars used to transport askarels are In exclusive service and not used interchangeably for other products. All cars must be Unloaded through the top (dome fitting) either by pumping or with controlled pressure using dry air or dry nitrogen. If nitrogen has been used for unloading it It necessary to advise the shipper to that when the cer returns the nitrogen can be replaced with dry air before any one may enter the car. If the car is to be unloaded by pumping It will be necessary to use a dryer on the air intake line to ^remove moisture. . . , ^ All tank cars ara fitted with steam colls, which are available for unloading under extreme low temperature conditions. . . . * Vs ' ', ' . Convenient handling end pumping temperatures are given In Table III. . :. Use Ordinary Personal Precautions: +>* (-*** I*r Transformer askarel has been made, handled, and used for over 40 Ser * years. It can be handled safety with recommended precautions. If p*y 4. * accidentally spilled on hands, no serious skin irritation will occur. However, liquid askarel has a solvent action (similar to paint DISMS*L CF CJfUID 304(4 Table III Handling and Pumping Temperatures Product Unloading, Handling and Pumping Temperature *C Pyranol A13B3B-3 Inerteen 70-30 1 Inerteen 100-42 : 20-55 20-65 35 75 -thinner) on the fats and oils of the skin and prolonged contact . may lead to drying and chapping of the skin. In case of contact, wash the skin with soap and water; remove and Aettr* lli; ulian saturated clothing. Clean up spills with rags, sawdust and . absorbent day^Eye contact may result in painful irritation but no permanent damage, io tlUUR. ITaskartl gets in tfle eyes, nuSh with ' large amounts of water. As with ell eye first aid, refer to a physician. To relieve irritation, physicians have used an opthatmic anesthetic solution ek well as opthalmic cortisone acetate solution* amnt nil ' ( \- v . infrequent exposure to askarel vapors will not cause HI effects. . However, prolonged exposure to high vapor concentrations should JbV^- b* avoided. If hot askarel must bB handled in a closed or confined area, provide the area with mechanical exhaust ventilation -- or 7 TOW6lDMON00251 22 WATER_PCB-00009591 ^*,'rui '*' organic cartridge respirator approved by tto U^ S***^ On Opening an Aikarei transformer: ' i1 various compositional types me used..Under) thegesei produced, while consisting of brMomir. " 1" ' " " " an yield varying arnouhttM 'sii'tuiausni yiwm* mwip>ivnly(uic e askarels and cellutoiic^^j pother organic .-materials may,' When arced, produce gaseousi&' rt mixture* which arft moderately flammable. A* a precaution,|WsJj^ h'?,*>^gawi ehould; be ^removed'.from'the mkirei by. 'bubbHnfl elntilR ) 'nitrogen through the askaril <r>d flushing the gas apace yvithjdryi `i: 1 nitrogen before any work I* performed on the apparatus,?';- ifXttt-sw.-74*n?y rThe'American Institute of'Electrical and Electronic Engineers duld#^, yiler?fr)-M*Mht 1974 gives more detailed instructions and guldancrvb *"For Acctp fence and Maintenance of Transformer, Askant! in EQUff)% m&nt". This guide is published by the Institute of Electrical & 0ec-Jft` ! tronlcs' Engineers, lhc.,, 345 East '47th Street,, New York, New Yofk^1 " -10017. Wo recommend that users of askaret treosfornrara rater to jhli v: ^.Vlll, Avoid Environmental Pollution'.**** ,*/'!rv ' {; Transformer askarels contain polychlorinated biphenyls (PCBij which W* A'; have been used In thd United States end elsewhere over5 the pest 40 ; years,for many' industrial and consumer applications. Duilng the jitst ft4 several years evidence has accumulated to Indicate that PCBs are widely V ^ dispersed throughout the environment and that they carvheve adverse >V V'; ''1 ^ The United States Government'!* Interdepartmental Talk Force ' ,PCBs, Com-72-10419, In their ;March 20; '1972 report tided,T' , ""Polychlorinated Biphenyls .and the ^Environment",, recommended. , .restricting PCBs to use.ln capacitors and transformers/-:iv, , J ^ . tocunifiil nui*Ur |* AHilC 107.1- 197V. i CrriU i* b c.J This report is distributed by the National Technicai'Information r.' Service^ U.S.Departmenl of Commpce.'Springfieid,Virginia*'* tevlfcf A Auelnq 117 i rl 77i* nttA <4 sA*.c yt &Ati&hk.JX2ihZ 'A document titled, *'Guidefinetfor Handling and Disposal of Capacitor and transformer, Grade Askereft, Containing , Pol/chlorinatad {Biphenyls", h8S been prepared and is available from the American Procedures and guides for safe use/mamtenance and disposal of'*! el and .askareUoaked./n3!^*'* used,in electrical equipment;,/' .*1. , Source of (ethnical Information and advice.Vor Fadefal/Kv` State/loca^ authorities and ell others concerned.'.', 2. , Encourage development of suitable disposal.feciUtief.arid keep all concerned Inform^-S/;V'V? V- 1 ?t4 /?*</' Organizations active tfln or represented by thii ANSI committee,]/ include: National Electrical Manufacturers Association, Electronic L:-V''- Industries 'Association, Institute; of Electrical and Electronic^ ^t'^ .-f i 'Engineers,`American Society'for Testing and Materials,' Eltitrid ^ 1 xii fi',? Eight and.' Power .'Association; Certified ^Ballast Mahuf*ctyrert;,t v<A( Association^' Environmental* Frotectlon ' Agency; -Office-'\&' '" Environmental AHajrs; General Seryices Administration; NetionaiJ ' TOWOLDMON0025123 WATER_PCB-00009592 -------------------------------------:----------------------------------- ^v BureM of Standirdt;' Department of the Army; Rural ^Electrification Administration; Division of environmental ; , Research. TVA;''American Public Power Association. Water .1 B Pollution Control Federation; Food and Drop Administration; . 'National Fire Protection Association; Underwriters Laboratories; * ^nd several section* of thy-S. Department of Interior.1 > ^ tht following are pertinent excerpts taLen from tfie ANSI Guidelines $^**areltransformer:7 ^ r &l"f I- LABELING ASKAREL TRANSTORMC RSIRi 161 % ""'/.//, 4.2,2.1 New Transformer*. All new vwnfoemort that,' O.contein RGBs shell have a label of adequate durability,; permanency end prominently attached to the tank tty the / :manufaclumf. given adequate wambg end instructions. A ' lu^/ .tuggcstedlabel includes the following: r " /; *V?pV' CAUTION: The insulating liquid h thh transformer t rjl ^ ` contarns polychlorinated biphenyls (PCBsl Care should be ^ taken to prevent entry into the environment, in case of / malfunction ' or hsk^ consult the snstruetton manual ory 'r ,/ the manufacturer. ?" ' ` 7 * 7 ` - . . -7r ^ 4.2.22 In Service' Transformers. The transformer manU'7' ,V (\ '` lecturer should make available suitable laMs with a similar ' warning as shovm In,4.22t.for use on existing trensfonnet*. , ' V'"' V ' *' ' DISPOSAL OF LlOUID AND SOLID WASKStPg. IS) 6*^0 V v',' d. f.CS. 1 General. Disposal of askarels and askaref soaked \ 'X*7'v^V materials should be accomplished by means in which there fs A ' 00 Hgnifkent release of askaref to the environment. At. \ vV*.-'Vrpresent, disposal Is accomplished by carefully controlled,: [ A frefneraffon of fkjuids and soaked software/and bycon- LtStL,'"'* trolled landfill burial of apparatus and other hardware from " ^ *-r * which askaref has been previously drained and washed. ;I - Present knowledge indicates diet proper incineration '' jnust involve e suitable balance between dwell time and . temperature in the incineration plus oxygen availability and, . finally, suitable scrubbers to remove the HO drat will be formed; for example, 2-second dwell time of 200CFF and 3% excess oxygen in stack gas, or 1.5-second dwelt time at / 270CTF and 2% oxygen instock gat. '' These facilities should meet the applicable requirements . of the state in which they are located and should control \ effluents within the limits set forth in thh standard. ' Controlled landfill or deep- well disposal can be used where permitted by federal, state, and local regulations. . r, The ANSI Guide lists the locations of facilities that conform * with the above requirements. Monsanto has such an incin- ` eiator at the W. G. Krummn'ch Plant. Department 831, . Sauget, Illinois 62201, where arrangements can be made for scrap askaret liquid disposal for a modest fee. For disposal of solid scrap a controlled dry land-fill can be used where : permitted by Federal.State and local regulations. . 3.V-CONDITIONING OF NEW OR RECYCLED ASKAREL 6&S!h, <* 16) .' '; t 4.21.3.1. Askaref Conditioning Equipment. The condi . ifr * Honing unit should be located either In the storage tank area * SJi'JVr'fe' 'or to H*e main transformer manufacturing area for filling vdth askaref. 4.21.3.2 Fuller's Card}. Conditioning of new askaref or recycled askaref requires fuller's earth treatment The spent V* fuller's earth fn cartridges or bags, when replaced, shoutdbe 7 lo drain thoroughly over drip pans to remove as; ' much liquid eskarel as possible. The cartridge un/ of steel . x T/v'mTeAsMh..INc.o.A.n.Ts.Etr.Du.c.t.Wio..InT.H.s.h.Ao.Su..lKd.A.b.Re..Ep.lL.a".c.ec.od.n.itn.a.in.th.ee.r.f."oSrTdEisEpLosCitOioNn. ' ''fyiC/i*' doth bags filled with fuller's eerth should be placed in the BURNABLE ASKAREL WASTE" container for' dispotivon. * 'y &0 J^rr 1yB1 /- ------- \- Ir r* x\ . > . i.i.f V, )' *, K 'f \.l ' fj -J |,.V *x: 1 ` ; 1 '' i . V' ;* 1 Lt * s ' k :pi 'j , $ s/ 020^^19 jV.i VWXfS TOWOLDMON0025124 WATER_PCB-00009593 0205420 4k : TEABDOWN OF TRANSFORMERS FOR BEPAlfC^^ SCRAP (Pq. 16) /; . 4.2.1.4.1 Drain all askarel from the unit either into 4>\, / holding tank or reuse or into the drum labeled 'SCftAfJ'k ` ASKAREL'* for disposition, and then allow pjff/cbnt-thieVli > for all of the askare! to drain from the core and cells. -fy. 4.2.1.4.2 Remove the Core and coll assembly froCnthe/} transformer. Sufficient absorbent material should be placed .4 < on the floor to absorb any askare! fluid that still drips froth'S, dte transformer. .1 . '"t / 4.2.1.4.3 Place all materials in the appropriate sefrege/"! ; containers during the dismantling for later disposition. - ` :} 4.2.1.44 AH used materials, including rags, sawdust/ i i tape. etc. regardless of quantity, shall be put into the/: : appropriate containers for disposition. -t *. / s., : $ ** TRANSFORMER DISPOSAL (Pj. 17) *' ' 1' ` ` :<f* .. * 4.2.3.6 The ultimate disposal of an askare! filled Irana-'./J . former may be accomplished in either of two ways: -- ..-v.. . (1) Complete drainage and dismantling with the proper /': ., disposal of the askarel and askaret-soaked components described in 4.!.$. ` f; ; * ' ` vV .(2) Disposition of askareI trensformert by means of funk * or scrap dealers This should be avoided unless a transformer \f.. is first drained, followed by seeking the interior with e *>. suitable solvent. Accumulated liquids and washings are to fye/l disposed of as described in 4.1.6. ' . -'-v \ * ,/ 7: ;y y v, V. 1 ' . * * IK. Expected Service Life > ^ . Manufacturer! Indicate that properly detuned and installed askarel '/ . transformers are expected to give trouble-free service for at least 30-';* years. Since their introduction In 1932, the manufacturers report,' , finding the overall failure rate to be less than 0.6% for all units under _ ' test end service conditions. The Edison Electric Institute's report (1866-1958) on their member utilities publishes the failure rate for *., askarel transformers as 0,13 per hundred banks per year. , Mr. Frank M. Clark, who invented transformer askarels at the General'* Electric Company In the early 1830s, made the highly pertinent comment based on his many years of experience with G.E. PyranoT > (askarel type) transformers that ~ * , ; . ' ./' . 'The important thing h to keep then) dry - otherwise leave them' . '*' ' alone* . V y/'4;;.4s: / ' v-V- These words of wisdom became especially applicable in mora recent^ years when welding shut rather than gasketing became the main method *. of sealing askarel transformers. These units are sold with the ' understanding that tha liquid is in a normally hermetically closed - system.-1' / r\ > v., - ;'r-'-'/'/ '*'-'r ' X. General Characteristics of Transformer Askarel Fluid - ^ Appreciation of the following characteristics, as given In the IEEEJ Guide, leads to understanding the reasons for selecting dielectric breakdown voltage and moisture as the prime practical tests to Judge d the quality of transformer askarel fluid. Also, due to , these characteristics the power factor of transformer askarel will ta normally., much higher than the corresponding values for mineral oil. -. -1 ` Mi . In comparison to mineral insulating oil, askarel is a relatively polal|; material; l.e., its molecules are dipoles, free to rotate around their axes'; - and responsive to orientation by electrical forces. Askarel also exhibits^ a much higher dielectric constant and capacitance than insulating oil/) and these differences must be kept in mind when Interpreting electrical . test dale. Because it is relatively polar, and possesses high solvency power, askarel, s Is much more electrically sensitive than mineral oil to traces f> extraneous soluble polar materials, and consequently the choice^: V...' ... TOWOLDMON0025125 WATER_PCB-00009594 2^Vi ,`........................... ftJbrikd<>wn vo)to`bf>tK*;tl ^;not'eener)ly adversely affected by. v'i'V-. jAlH-fneny 6f the iolubJfc polar meterialitowhlch It* power factor and' j&vresiitWltyf Specific >esistancej ere so sensitive, In'fact, the dielectric 'V; 'a fj^-'Ueakdowh voliage' of ;eskaf$l H.somewhat greater than * that of: *TM}xlpsuleting 611,'Therefore,'the`value* itsigrved'these dielectric fluid* In ' * d .{Al VWthinsulallng (slf, askarel must be kept dry. It can pick up moisture ....................... . ,.... .. ,, ............................ "Representative samptei, .Whether'of the complete content* or only ' parts thereof,. are extremely important from the standpoint of yr *;-V` ^>valuation of the quality of the product sampled, Obviously careless ' {.sampling procedure of'contemlnbtioh In the sampling equipment will 'V'eesutt In a sample that Is not truly representative.'This genera'ly leads to;'}* ' ^erroneous conclusions concerning quality and Incur* Joss of time, 7* jjfji effort, and expense involved In securing, transporting, and testing the i.w^lemple. It Is strongly recommended that;ell of the procedures end/ ; SP&/precautions outlined in the latest revisioiVot ASTM D 623 (Sampling ffly'.Electrical Insulating Liquids) be followed,-**'('{4^'..-% *< V' ^ Af;* ;''because of the high specific gravity (relative density) of askaret :. \.*>v '! (greater than 1), water and some other impurities are most likely to be . fw j found at or near the surface. The top sample, therefore, is considered to - yti'represent the worst condition/' : < ; ; r;* t* m<%.' < . - " 1 " .......... ;. XII. Evaluation of Askaret Received in New Equipment ,* sJ5 '. .' Some users of askarel equipment find it desirable to make "as received V tests" on all equipment. It is quite common to use the dielectric * tt. ,.'v\ y^lbreakdown voltage test and visual appearance as the most significant: - ' tests. If suitable equipment and trained personnel are available additional information may be obtained from the power, factor, color; ptv*A end moisture content tests.' V `.-V-\ 1 -V- A*i'*;- ''v.-;'' ' : -V?w.> "`v ; y'r-tw*-* *.*, kY^'/ln sampling askarel contained in apparatus extreme care must be 'ij- . exercised In order to obtain;* ippresentetive sample. ASTM Method i1:tv,D 823 should be followed. "> ' `; 1 ,!\ v:v; t,; ' New equipment with askarel exhibiting the following cherecteristics it jf<i'ftt>ntldered eccapteWaj i< \ -i m- ' ' 7y V' ... J\ ; : I ' 'Dielectric Breakdown->.J - V , 30 KV min. .^ 'J?!, Color i'.'l-'Vl * aM1 - 300 max. (Straw color) J. Condition Visual. Ca 2'" i1-*,- ,. Water Contam,; irv./-. 35 ppm max. ^ower^actpf at 2R^|V? . /} ASTMMethqds ..." 0 877 * D2129 ' D1702 ' ' ' D1533 J 1 D 024,0 )50 P^er Wfactorr `ooff aasskkaarreetl ttaaken from new transformers,'v ^^7.4^: i.1VV'?traeAabcsttonras eanrud^4 aawccjxeasrssroseryo eq1u11ipr*mnneewnat can reflect the presence of: , moisture, dissolved polar compounds, or other contaminants and-': $j`'<Vmay vary with the type of equipment from which the sample was 'i [V'T,ji''taken due to the different ratios of liquid to solid insulation and to the high solvency 'power of the askarel. Given an acceptable',.,' j T.|>^t^.water content end dielectric breakdown voltage of the askarel as 1; Indicated above, * a; high power factor seldom impairs the \ r'ierviceability^ of. the askarel within'rather broad limits and i*' i'tt't .1: ,V, tfj'.i;* v * ,, .` .} U' TOWOLDMON0025126 WATER_PCB-00009595 ,,, Indicative ot the degree of exttaneoirt iolubfe poler ^netniefiJ^&^jS present :: ..; .; .' Recognizing the pottibillty of ewlde ring* of bower (ectori being recorded for askaret in new equipment, it it difficult to establish.fJekw*i ; tingle limit Which would be acceptable to both suppliers artd lof all.applications.However, at abroad guide, power factor!Upyjrfe&j to about 10% it 25*Cend 60 eyelet per second (hertz) do not ln)|t?s\% general indicate any abnormal contamination providing that thaj^V;^ ethjr Criteria.(water content, dielectric breakdown voltage, etcjvfc$\tVii ' *r* '* Mnrh higher power factors 'may indicate 'excessive 1. f/the misapplication of tbe solid materials used ini^^.'i^ k 1-iykhtkH with '4K* ktla'id .''krtrf . tk/utlrl 'K* tIJ-VAI >y:^: r,$:. l#|| W'' iiit ft] t! mm ;' less, an analysis for water is necessary. If water it found in excess of 40 V-.; **,.& i ' . ppm at>pom temperature, Its 'source shotitd be located and corrections '< v.^* J >.S{$? 'b.-\ y r* .V`\vV -.v v^O: When* the moisture'content approaches 126 pprri (saturation level at>H.` ^i v'f'roorn'temperature),''the dielectric breakdown voltage of askaral drops'-V-:*1 below the value required for, efficient insolating^the moisture content l\'y <> , should not be allowed to rise over 70 ppm/sampled It operating ) temperature. If the moisture content Is found to be in satisfactory V vv; range and the dielectric breakdown voltage tsToWritbe transformer.'.,. ' ; .* >: manufacturer should be consulted; M?i\r ' '! - y-\ : r^Vv-1 ' Table IV'shows the relationship of dielectric b>eakdown voltage moisture and Table V indicates the approximate water solubility limits ' >?. in askaral and mineral oil. s ^ J * \\ *>> * -v'i iy I , * s' '! % "^y',w : Table IV ' - / r> , ) y * \ Relation of Dielectric Breakdown Voltage to Amount of Dissolved' ,c.' 1 uV 'z-v > ,>:. Water in Askaral and Mineral OM f-;'r ' Vj '*} * - '' N` vr^y^v;.'^ Breakdown Voltage (ASTM DB77) ,^vs i Wff? a Water ContentJPPM), " T* * r AskareJ ' ' * * yt* Mineraf_Oi[ o ! .. r ' yonvV ` !' 60 Ktf J 20 v * -v * ??.!> 39 Vv . 40 >.h J'SV . yrrj.t' / 4t , 30/ > " 60 ' ' ' V , .40 . ................... ^ 80 i f - V t 38 : P : . - 2i *;?f 110 < . 6 1-0 i __t$$_ f . _ i> >V: Y-ii v\ /, ; gj* y W _ . _ ; * *. j v, '} ' ;vT1 !. `vy'' ;v' < ' nfrM^ K TOWOLDMON0025127 WATER_PCB-00009596 S&-V ^ ' fe* TibltV Approximate Solubility of Water In Transformer fv-Ji AikaralandMineralOil v.- : ; '> 'C^, / Amount of Water IPPM) Di$! 'xaj ... 1939 *. j^VV * -,tvV'V- ''3> , .- 8 ' 10 ' - a ; <' -r . . - 13 ' V'.ys - 20* 4 * f65 V, '/ 33 v M 'i v, 58 y ` 170 -. ?' BS 130 ` J ^3-iXIV.'turbidity ,f;^ ^ -*'-:/; :' - ' " ' 13V'.',, V may be the visual sign of undissolved water, or may indicate dirt. ri? Cloudiness may also result from cold precipitation of tin tetraphenyl eifr* "scavenger" that was used in the earlier Pyranol transformers. This fife-jv scavenger begins to come out of Solution around 16*F above zeroi To radissolva it requires heating to l&O-ZCXTF and agitation.- ' ., y y - t High dielectric breakdown voltage will quickly indicate that any , t!V' turbidity present it hot moisture; that the Insulating efficiency of the - xjry askerel Is still excellent. However, if the dielectric strength Is below 28 fc$;. KV, moisture sliould be determined, using the Karl Fischer method r&$>\(ASTM D1833-80). y v. y;---; , - y-y.fV, i?,/' indies tor for molstvr*. ft h by It the most important maintenance test ^; V for transformer eskeret., . t ; , ' > XV. Check Points for Maintaining Askarel Insulation . A. General Considerations: . Modern askarel transformers with welded construction or silicone . or Viton* gaskets (hand hole-cover, switch and terminal compartment covers) and with properly constructed bushings require little maintenance. With properly constructed trans formers, annual or semi-annual visual inspection end dielectric breakdown voltage test of the eskerel fluid should suffice for routine maintenance checking over many.years of service. ; v ',y.: However, many askarel units were installed in the early 1930s - before the development of some of the better modern gasketing' . . materials and before improved designs were developed for sealing .out moisture. Such early units should be, and can be, modernized.; , ' Leaky or deteriorated gaskets should be replaced. If the askarel ' . has become contaminated, if should be reconditioned. At the same y y time, a general clean-up of the unit and possible refinishing may be / desirable. '; . . ,. ' ' >''/! C If ft Is not convenient to take an old transformer out of service for v y { general repairs, leaky gaskets can be sealed temporarily by painting '' over the leaky area with epoxy cement, . . , .... *y . ' ' KvfTf y.A survey users indicates a good number of early-built askarel transformers (over 20 years old) are kept In continuous service In yV--^critical installations . by the following steps (instead of sff^^ffnodernlzetkip),;;^^;.. ^ ^ . . ' ....... ::t *:f**yThe operating units are equipped with compound pressure gauges > for reading pressure above and below atmospheric. Positive ft*' ' i *&' 4 ` . ' iQ,^ redemark of E. t. DuPont DeNemouri a Company, Inc. -,v i`: ~______- ___________________ ________________ _ fcV i; J v' ' ' ' "' ' ' ' ' ' v 's .V."' <, s , 1. ' S * 3* 4 r'>\-u ,,V` - - i ... , y:. y ft". y,y: u TOWOLDMON0025128 WATER_PCB-00009597 ' -`.wv/owjigr ----------- --------------------------------------------------------------- -------------- -------------- -- procure it maintained on the then by introducing nitrogen at 2 3 pounds above atmospheric, Regular workmen in the area daily record the temperature and pressure. If a sudden pressure dropM^^y noted more nitrogen is Introduced and the gaskets are checked leaks with soap solution. Leaks art sealed by applying ..cement/ . . -/ y. : VV./. <; AiZ/ii , ' Modern Seeling Procedures: .* Transformer purchasers ^should specify the following modern > techniques for sealing: .. V Welding Construction: Covers, radiator connections, switch/?// / and terminal housings, instrument connections, etc. should v r be welded. , ,v, \ ' / '/ 2. - Bushing Connections! A number of bushings have been'/y,'? , ' developed .to' obtain a proper seat for the electrical i; connection through the tank ^wall. They are classified ,m)< */ ^/.follows: . 'r. ' / ; v.-`, 1). Welded Type - {Bushing flange welded to tank wall)/ v 1 . a. Cast resin bushing with a molded seif to theV'V . bushing stud and external stainless steel or coppet':^^^ -.? b, Rolled flange bushing with the metal to porcelain f/./'1. v seal at the cap and fierce made by being rolled ` * * ' x grooves In the poroelain over silicone rubber rings/ ' ` * * ' The seat between the cap and stud is made by!f/tj ' . t "Welding.-' * ` / ?' i `'r -4 /. > c; * Porcelain or glass bushings with metal to glass or, *> < metal to porcelain seals/* ;' / T//! * 2) Bolted Type (Bolted to tank wall) ' ' ; '* .' a. Cast rasin bushings with either cast or metal flanges/?/ ` ' ' * containing recessed gasket groovat. . . AV.5?* <. , t b.,'Porcelain or glass bushings with .flanges containing >'/> * i .recessed grooves or gasket stop.// \ The gaskets may be either of rectangular or circular cross-section, .' >? usually % inch thick. Bushings with recessed grooves are suitable ' to use with cork, cork-nitrile rubber combinations or nitrile rubber, a.(- as well as gasket materials such as silicone or Viton. ,A ` / 3. Small Sire Connections: When not possible to weld, small -. , . size connection seals should be made with Flexitallic** stainless steel rings. The surfaces must be machined and,'/ ' parallel. The filler between the steel laminations of .tha'.* J , Flexltallic ring should be either silicone or Viton. / J V*r 4. Gaskets for Hand-Hole Covers: Modern design specified V : / " 'silicone gaskets. Such gaskets must be retained in a groove? ' , V The groove preferably is machined Into the flange or cover. ; v . . However, It can also be formed by welding concentric statl ?' r*; , , strips to the flange or the cover. Generally the gaskets should ,' v * '1 be 5/16 to 1/2 In. thick for covers, depending on th# depth/V j : of the groove or stop. A rectangular cross-section js usuallyi // ' ' used. . , v'V -`//v? ' ' i{ * " ' The silicone material should be DowCorning No/50 /y Silastic** or equivalent. This Is a low compression set/y material. For best sealing 20-2b% compression Is recommended, with ample clearenoe In the groove or stop toy '' . allow for this compression. ' ` > ; No cement is required. With reasonable care the gasket_to r removable without damage and Is reuseable. ^ : f\\- . '' V . '` ' y "*[: <. ' Silastic 60 is slightly swelled by askarel which contributes to*/ / * the tightness of the seal. It is not deteriorated by askarel fluid v .. or vapors. It resists weathering and it is thermally stable and/./ / 'Trademark of FlaxrtaMic Gatket Company 'Trademark ol Dow Corning ` TOWOLDMON0025129 WATER_PCB-00009598 flexiblet ireptritlna'ttmp*rturti. It. it in excellent r :>... ' ', vV-;\Q.'.: ` j ,i~, V ' NOTE ? Dow Jborlfitnlngg,, Midland, Michigan Witt supply Hit of :; v-y V>>*v r r;vlj* ^/cvr-V* ''*< w ; gasket, fabricators : to . all transformer .V.yu^v - ; ,s K\ ) $fy {''>,^,.>1. *;/''*yI;iiViy jfefcjfJ'JJf?^^-W^Mma?dmnauntfiuaVfca^ct$utuotreeerf';s;t.<*o,*rr ru_s*_e_r_s_'.<_Thwey wwillsalnso ofurpnis*h *te*ch; nical'.:K''>, h.\;/>,* 'v .f?oiv;yl?vii- i [Tt-vP^* '^J<^f't>WtsV^:V'';'^^V^ fijJfjhebldeV'Seallng Arrangements: -V foliowing is'recommended for Scaling with the cork * *i''i-j'^f'ltrils rubber jComWnatlom:: s' ' .........................^'`^'^ ( \Jse Armstrong NC*fr67 cork-nltrlie material or equivalent,v'; The gasket can be cut from e single sheet or by icarflng strips; \ of the material. A convenient method for Joining strips Is to j ^ $. */ make a Keystone Type Joint. For this purpose, Westinghouse, 'A >JVV Sharon, Pennsylvania, offers their gasket csjtter Style No. 328: ^^.Bei5Gl, (about j>'. The Joints - and also the gasket - should be cemented to the Jf'i`i;l,v^flenge, using one of the above cements. Excess cement sboiild > . 5?r|*v^'; *?* ** flowed toreach th> Interior of taeVantformar.^y.;;' m^y- - After installation end bolting, the outside edge of the gasket. ' should be coated thoroughly with epoxy cement to Increase' weath. er resistance, J*. ", -v v!,.9 - "; '.; V'V-.y ,;-' - This epoxy cement Is e paste to which a'curing catalyst Is v added Immediately before use. Typical are: ' v . Epoxy Patch Kit al-C ' * *; Hysol Corporation, Olean, New York , ;V-I . I>/ Scotchcast** Resin *4 1"\ I V Minnesote Mining & Manufacturing Company y;-yi,V* I \'\y St. Paul, Minnesota -'/i{Vy-:J 'C./v Adhesive A*1 and Activator Type B ` - , Armstrong Products Company f! v/' ?'; i,* ;^Viy'J * ; Argonne Road, Warsaw, Indiana -1 - .< . vV d. Adhesive 98601, Synthetics Organic Company,**. 'iS M?r'Vv Cleveland, Ohio, used with activator diethylene triamlne (Carbide and Carbon Chemical Company) ; .j- Straight Nitrile Rubber: When straight nitrile rubber was l originally used. Invariably the gasket Was recessed in a groove. M This was to prevent gasket flow and to protect the material' ' >1 .against excessive compression. Although this type seel was : l, . not cemented, the nitrile rubber gasket Is not reuseeble, ' : v,':>:; V'-- ' ' "c grooves or stops hive already been provided for the 1 nitrile rubber leal. Silastic 60 can be easily substituted and Is > **>Xreoommended.'Thfi conforms with modern practice. > ^ r i *v o * ' " ' ' '. ^XVI.-Poriodic Fluid.lnspection and What Checkpoints Mean gOn a regular schedule at six, nine, or twelve-n^mth intervals - make ; f^a simple visual Inspection bf your askaref Ir^uletibn and run a dielectric '' &bnA<loiwn;iwlMte*&'!^ -:L* 5 > \ ' iV,/ 'i:l ^ ^ of ClKtrle Compfty , ' ' ' ^Mrademark ot Minnesota Mining ft Manufacturing Company - 5`.`r AVi.-V 7''h,VV,'V^ 0?055 Pc TOWOLDMON0025130 WATER_PCB-00009599 , * ' ' ,IJ'v. liquid. After'.long term Use thlfj} light brown. The fluid shoukt or cloud!ness/W^:* YV--VJjJL ,, i, red Or blue cast -- indieat*^s|\ Sfc materials) from the solid lnsuletion/Svi noted, check the oomplet# T and* 'notify th` e trans* form"eyrL^fifrl indicate an arcing condition^ ' Other color changes alone .ere not danger signals since the1 ", diefectrlcbreel(do^n,yo!tage is not likely lobe Impalred/ft; Y'/^^VrSi Dielectric Breakdown VoltagiV' ' `"V V'!'/ \yl- Y ^ X WSJ '*V U>t" If the dielectric breakdown voltage has decreased significantly' * p) from the last Inspection/ or If it pat gradually decreased below 28 ^ * ' KV range (at 25*C) V RUN A CHECK,FOR MOISTURE,Use , 'ASTM PJ3|lKarlF|schi|;:Mifhcid)yi>U ** uM ' ^IMn w$ , *l|i .`;.V'(JiA / , ;> transformers have service records.of 26 to 20 years on the ongtfut . Y.'yVs M"". * <'-askarel,>--jVs'wV* V* i-J;. ,<i2wfd `' * \ s ' * ''St7-.Vl'>U-3 1 * ! XVll>; Inspection Checklist', X' *' u ' 1 " askarel It clear -- even though darkened to light brown, has no Jfi sediment or turbidity, has dielectric breakdown voltage over 26 KV-"g^ive It thelnspection XJK^H [r; ^`'v -v-" ft ............ ' y r,AJy' $**%, ^ V> V'Y/yX"* *, '2. If eskerel it clear' but has foreign color of blue, dreen, red., . H is ' v-pJ^ j'S*1 h , 1> ** , y ,v'/ "oepxetrraatcintignghaczoalrodr"whfreonmthinetedrienalelcmtraictebrriealask.dTohwisnkvnooltat,geofstiatsyeslfo,vaenr.;-'*/.j.-^P'jj 26 KV and moisture remains low. However, this rare occurrence calls for checking into the condition of the interior construction : > V* and consulting the transformer maker. However, when sampling : / / J, the fluid cere should be taken to avoid getting color into the.-./askarel from paint that may be Inside or outside of the sample . ' ^ ! \ *}; , If the moisture content is found to be above 70 ppm al operating e fetsVcUn''WfeV .1 op. eratin.g. __t_e_m__p_e_r_a_t_u_r_e .y.^the eskaref k ready for simple 'refining". If the moisture Ik near thesaturation level (about 126 ppm at room temperature! a thorough inspection should be made.; f for water droplets In the transformer. tank, and even for' ;..'S?jj "globules" of water floating on the eskarel surface. If found, the / ' J ^ . transformer manufacturer should be consulted .for reconditioning. < 4 both the transformer and the fluid. ;1* * . S/} .* V* f;'=1 *wV *U. ' ' V'"-'- : J>V;fe. " If askarel Is dark brown to black, if black particles of carbon *r* ' seen, and dielectric strength is low i'. i the askarel has been broken down by arcing. It cannot be refined and should be removed and * *.)}} . * incinerated under proper conditions. (See ANSI ConMni>te^C107*7^k-^r i .-rnpnrJi ng. U"v*' rrf` uf ItShunt' anrf` ** . v. ewTvrnew/es. r-H30 Er-oadvreYrNew VerUi New YorMOfrlSW^ V fyN an"y* oMf tthheessee ffiivv\ ee^'ssiimmppyllee ,ii\nn.ssrppeec-cytitloihonnpStteesittft aappppeeaarr oouutt bbff tthhee^yT|V. ^j ordinary or'tt*he' re-*la*tions-th'ip- *be--t-w--e--e--n---a*p-p-e--a-r-a--n--c--e--andj*te-.st values ^. . abnorma1l,,; contact^your, framformer^-supplier for'e complete.-O'Y'1,'* ,r>:?;. :aoaiyki. r !( *' ' i i, \ > Whenever a sample is to be shipped to Monsanto, please follow tbt/Y Vv'C, directions shown under: "SAMPLING ASKAREL", ' i--V - - - t`. . ........ >. ' . - .WViL* ujcrJ.Lei) TOWOLDMON0025131 WATER_PCB-00009600 ftp . r|,v XVIII. Contamination in Transformer! . Moisture. particulate matter end arced decomposition products an fcriowrt to be serious contaminating Influences on transformer askarel. The power factor test normally Used for the detection of contamination j^ ln tninarat oft fitted transformers is of little use for Urn purpose in . kV>g askarel filled transformers, due to the extreme effect of extraneous KfjPeolubl* polar materials,'This increase in power factor at illustrated in y Table VI has no adverse effect on dielectric breakdown volte?*. ' < - ,* p:; &W*V/V Table VI ' ' * " ' ' V?V* ' Effect of Common Insulation Materials on Power />,1 i.-: Factor and Dietectrle Strength _ t; vW/H .......................................................... .) ? i' ` \ >V 1 >, y\ Materiel Immersed !, y.> yV-y Askarel Alter Exposure Power Factor, ; > Percent at 60 , eye.. IQfrCy Dielectric 'Strength 26*C , None (contioD vJ . Black varnished doth ( s>- > . Copper '.>' `.4<!W,l?'< V ,-Y Pressboard V\v.-' Manila paper * v :> . Phenol formaldehyde resins -,< ShellK . ' Iron !'>"); tSynthetic rubber . \.v ;. . 1.0 85.0 1.6 1 .2.0 ' - f-B 16 " 6.0 < r 6.o . 70.0 35 KV . . 42 , 40 ' 37 f 39 - , 41 . - ' 36 ' 39 ; 39 Similarly. trace contaminants from' commonly used construction materlali can lower the volume-resistivity of askarel, without affecting Its dielectric breakdown voltage. This is shown In Table VII. * > . ' \' r '* TebleVII : Effect of Common Insulation Materials on Volume Resistivity of Askarel / Sample ; 1 . / *'. . . \ . Volume Resistivity x 109 ohm-cm (at , I00C., 500 Volts ' _ PC., 0.1 " gap) 1. New askarel before heat aging ' 2. New askarel after heat aging 96 hours at 100*0 3. After heat aging with 1 sq. inch specimens of; - a. Phenolic resin tap changer material / * ; ' b. Paper (' '1; 'f ' ; ; e. Grade A pressboard (ten) `' `' . d. Grade A pressboard Igray) '' . e. Grade A pressboard. laminated strip ' ; ' f. Cotton wrapping - g. Glyptaf 1276 cement, cured 48 hrs. at 110*C 2.000 > ' 1.900 v . * 1,200 750 600 600 400 300 100 ; V. V ;: While trace contamination easily lowers volume resistivity from high veil, It is important to note that heavy contamination (as when arced] i7A>-^'does not lower the resistivity below the order of 10^ ohm-cm. at 100*C. - ' fThe different behavior of askarel v. mineral oil In these respects can be ^r.Veummarlied as follows: ' % High power factor and low volume resistivity In transformer vV/ / mineral, oils are fcommonly regarded as "danger signals" that the oil has deteriorated and broken down chemically or excessive, ^-''moisture is present,v\V:,-'SV : 'V'1--""': ;J This is NOT TRUE of askarel liquid insulation unless the dielectric breakdown voltage Is low or the moisture content is high. . Manufacturers of askarel ty- p e transformers point out that fl Is q uite/ ; welt known that aikarel transformers with initial power factor of thrjC>"i' askarel fluid in excess of 50% at room temperature end 60 Hi are giving ift/ satltfactory aervice life. However, there need! to be assurance that both&f,^,, dielectric breakdown voltage and moisture are at latiifectory level! and Y . do not thow $dvt(te tfgrxif.V, f . \ /./ . ,/J . XIX. ASTM D32B5 Method for Investigating The CompabXfe^ - ibility of Transformer InaulBtion and Construction Material*Y/Y. In Askarel* . - Y ' : > ' ' ' ' - . ' v/VY This method uses the chinge of electrical and/or chemical : * characteristics of transformer askarel resulting from its controlled >?>>- 4 xpoosiuurre tto` in--su-la--ti*o--n a--ndJc...o..n..s..t..r.u.-c*tsi.o..n....m....a..t.e..r'ia*'l*s. 1I--n ord.e..r...t.o....e.Jvalu4at*e ,-f ( theiIr Immediate major ''contamination" effect on the askarel JIukLyY'Y Delayed cor long time contamination effects may not be detected. ., fh * /yY The method also utilizes various physical tests on the insulation ahd. pY.I construction materials after controlled exposure to the askarel to ;/.*V determine the compatibility of these materials with transformer askarel, ' '; Properly proportioned Specimens of the insulation or structural, i; ?? materials are immersed in refined askarel for 168 hours at 100 1*C in a forced draft oven.Changes in electrical and chemical properties of the, Y*V transformer askarel are compared against a control sample of.the.vY-V askarel treated in the same manner, in absence of the test specimen*." */Y f Dissipation factor (ASTM D B24J change Is one of the ctiterit used. The/Y- askarel fluid is refined by absorptive treatment to a dissipation factor'; , level of 0.05 max. at 100*C and 60 Hz and 0.01 max. at 25*0 and 60 Hz. Corresponding values of the askarel fluid after heating 168 hours atY'/', 100*C in absence of a test specimen are 0.076 and 0.02 respectively/ .' The maximum dissipation factor levels suggested for the askarel after f heating in presence of the test specimen are 0.20 at 100*0 and 60 Hi. r'\- and0.04at26*Cand60Hz. // : - Y-V XX. Refining Askarel for Route ;>v A. Filtering Through Dry Blotter Paper to Remove Moisture and ;-, Extraneous Particles: : \\ Most operators prefer portable refining apparatus, such as a plate Y ' press fitted with a dolly, available from Sparkler. Mundelein, . . Illinois or General Electric Company, Pittsfield, Massachusetts; or V* > ' the earthen cartridge filter type available from Industrial Filter-./*/ Corporation, Lebanon, Indiana. Filter paper liners for the plate YY press are available from Cad Schleicher end Schuell Company, :; , ' Keane, New Hampshire and manufacturers of filter presses listed . ; . . above, vv--- YY/'Yv - ' ' ; ' '! 'YV;' f The filter paper must be dried Immediately before use. For best f ; . results, spread the paper for maximum surface exposure In a hot, air circulating oven and heat it for 4 to.6 hours at 110*C. r-. r Circulate the askarel hot (but not over 40*C) through the fHtw Vs;/ fitted with the dry paper liners.. , v;" - /* After filtration the dielectric breakdown voltage of the askarel .V; should be 35 KV minimum. - . 'v . . . . V Y/YY PRECAUTIONS:* ' ' ' '` 1. Filtering should not be done when the relative humidity' exceeds 76%. . ' '` ' 2. Any flexible hoses and gaskets on the refining equipment <r: -> W:* should be lined with or made of materials that will nbt * be softened by contact with askarel fluid. (Materials lined with Sticone, Viton of Teflon* pr flexible metal, ' r ; materials are suitable.) Y ,` . ' trademark of E. I. DuPont t>fN$moun$t Company. Me.' ' f. V 0?054?B TOWOLDMON0025133 WATER_PCB-00009602 Plipostl of Sotid Wants: *-f . ; V ; ' '** '* \/Y< . jy-jk pSPi^ , ANSI 9uldi<iQ,,tO>1;1874l> Section ,4.1.6' gives'detailed}** V ^ 4M-- li iC.Jy'Solld InwUtlon Requiring Drying ^ : i '** ' f **'C ] %; It the solid Insulation of the transformer requires drying, consult >V'v the transformer manufacturer or' an apparatus service shop, as to V-'* ^''uchcesaoven drying Is prafarred.VVfVi'tf(. * / "v; 16^; Earth Treatment for Maxlrnum lmproverrent of P6wer factor and ,- Volume Resistivity' ** * V'-'.* ' v \ ` " ' v ; *,\ We question whether pumping end'filtering the fluid solely to achieve a change In power factor or volume resistivity alone Is ' Yw }[ Justified In today's ecological climate regarding PCBs We recom* 4 mend that in these situations the original transformer.manufac*.` ;; \j turer be contacted. iU\{ ^V Procedure: r '* *" >'' .-W . ' J'\ *v The askarel liquid should be relatively dry p/tor.to the / > i following earth filtration, > , V ; ; * 1 ,, / * ' As a coating on the filter paper surfece use finely divided (v : Attapulgut* clay or Fuller's earth dried and activated by\V heating for 12 hours at 300-360"F immediately prior to use.' , The amount of earth used should be 0.1 to 0.2 percent by`:-X ' Weight on the weight of the askarel to be treated. Askarel ' v weighs about 12.6pounds per gallon. . v ' i. > '. V To deposit the earth evenly, stir one-third of the earth with a ; ; f smalt portion of askarel in a clean container. Pump the ' ,, , . .. mixture through the filter and follow with two more'.. ' one third portions. Then circulate askarel taken from near v the top of the transformer, pass It warm (not over 65*C) > ;Y trough the earth-coated filter and feed back through the fyp. V '* bottom transformer outlet. Continue circulation until the V, ^ . r./^ ftuld Is clear and test shows that'the electrical properties are w vfully restored. ' * ' ' *. ' '! '"'V- vV.'2.r/'; Effect of Earth on Removal of Scavengers ' {' "ryJlCiV Only slight and Insignificant loss by selective absorption of ' ^'<.V\tln tetraphenyl and apoxldes occurs when askarel is refined/.; : by treatment with 0.1 to 0.2 percent by weight ol earth. To'/l y yvaJ<:,'removi significant amounts of the scavengers requires rapt* 'vi;' (pVeilfmark of Eftpethertf Minerals and'chemicelsCorp. ; v'' y '**' A V; ...... Table IX . * Approximate Relationship Showing the Insignificant Effect of Power Factor and Volume-Resistivity ort * r Dielectric Breakdown Voltage of Transformer A*erel 4 &,*" '* ' ^ s Volume" R esiatlvlty f; ` '*"*' *' . \Power Factor11 j x 10* ohm-cm (at Breakdowli 160 eye.) ;. 100"C, 600 Volli ' Voltege r. . Cleaning Arced Trantformeri If e unit has arced so that the askarel i< no longer fit for use, a thorough'*; cleaning of the unit is. necessary before refilling with new askarrtV-jj Insulation and returning it to service*. Follow this procedure Insuring VM It taken to prevent iny loss of liquid eskarei to effluent streams. i; a* l `*;1 A, Drain out ell dark/carbon-contamlnated asksrel. Arrange to have ./.$ . v,.jV -/.< i* * `*L.......... - " Jd Incinerate unde^ proper ponditiont. (See ANSI.N; I 07 report) ;% ytH i ,i;?< V. ,*] Carefully brurh carbon depoiltt from Internal peril end Imuletlon,' 't* ' toft brittle btudi imeklng'tun that Imuletlon ta not ,, ^ywf an oil,rx>f a cleaning ....... . . ,........................ t, i ___________________ _________ ...* V`*1 * V "'* iv ;* r>y ' ' y1 y- - D.v Flush e se' cond tim e wi'/th' fr/>esh eskarei; drain; then fill to tht - proper level with new askarel. ^ g" * - >' ^ l \y-Vi-\ / 5 .*** *i'.. s.,. ' //'* ' ` E.'. Energize transformertowarm the fluid for 24 to 48 hours; then/ ... -? - circulate the eskarei through,a filter/returning it to the ur^it muW'A : f ..vvWV.'*.. `s'V*'` / ` r 1 ' ' 1 s XXII. Sampling Askarel ': : fy\ ^ . 4 '. . 1 , . i A$S*5{`^,Vv;rt ,/ * o ,'v 7 ' ' Take a sample as close to the top of the liquid surface as possible. ManyV_/ . ` large asksrel transformers have a built-in tamping tube near the turfaoe,' for convenient sampling. Then, to make 'sure that your`sample truly ;. . represents your asksrel insulation,'take another sample from the '?' J` y1 'A * 1 *V y 1 ' * i' -i'` ` r wbouttvomm. Ii f paudvdmitkiovni anl sampling tluwbev wcoinnnreecvtiuovnes pare wcomnhtri"vevud ov<n> t*he* jjf'jj V v.''* ' . ,-'f \ valves for easrer sampling, make the tubes of dean glass, stainless steel/* r* :Vs'a/.frfirAt -v;.' i ' *.* -J'% rV"*- aluminum or tin for rigid types; end silicone, or yiton or Teflon tubing \ >; - K': / '*r..- v / 1 y1 * * j-`/j ; ^ ^' y;> ' Use NEW containers for the atkarel sample. A new and thoroughly '/: y'( i c | : j* ^ ' / * pre-dried, small-mouth quart glass bottle fitted with a Bakelite** screw/^' \\r.': >/ v * cap with aluminum or tin cap liner |s recommended for quick, on-site/y V^!4.Av: 11: ` , testing. (If complete analysis U .to be made* I bplnt sir* sample &;;V t /.t. ' *. / !-V- o* .>.!. *hat the new bottle doe* not. stand open to collect dust or/^ Rinse the sample bottle and cap lining two or three times//' el from die transformer, then fill It. tf the samplt will be V) mptly, e dear glass bottle can be used. If sample b to be / ^finitely, use an ember gte^lxxtle or`wP \f* il^VVj':-1 TOWOLDMON0025135 WATER_PCB-00009604 Jr ft/'. .'Make sure thit the tskerel it et least at warm ei the surrounding <Cotd liquidi cen chdne rnoHture ftom humid elr.i * Wtwn sampling askarel from transformers, It it best to taka the > when the Unlt warm nd operating fct average or > ; maximum load, especially for a check on moisture as reflected by EwtY\,>?i dielectric breakdown voltage test. Sampling the warm askarel ,= rnore truly represents Its condition during operation, KfcW; ' V . V - . -- ^ 'v Experience shows that water will migrate from a transformer's :' solid Insulation to the askarel liquid and vice versa, depending on <-i 1&V& lfmPf|lure' Therefore, when the transformer it hot, the moisture K'i'Jw I* most likely to be found in tl>e liquid. This accounts largely for ; * ^,v;v periodic variations In dielectric breakdown voltage. For example, e - *v*A relatively high dielectric breakdown voltage may be found during winter months and a relatively low dielectric breakdown voltage ^ fc'Vi V*. during tire summer months on samples taken from the same unit, 'If*.' ' 1' ' ' When testing has been completed, the remainder of the fluid : .vV/V -tample should be destroyed by high temperature Incineration ' described InSectlort VIII. T .. - . ' m+pH-. wVi'' |C): ''>1 0/05*3! TOWOLDMON0025136 WATER_PCB-00009605 I. Introduction "1 : ' ' High voltage leads are usually Connected to askarel or mlneiat oil-titled,.*? network transformers and power centers through terminal chamberi'^ and twitches. In tome cases terminal chambers are not used, and the./, high voltage leads are connected directly to the switch terminals. Thf^/ r, may be filled with either etkare! Or mineral oil. Switches are usually/; rotary or drum type fitted with a revolving block and porcelain unit as/, the principal element arranged for three-phase service. ^ Askarel transformers with attached switches have been in use for about' 30 years. When they were first introduced, the availability of insulating'Vt and gasketing materials was rather limited and even the best materials at *j. the time had no service history. As a result, inadequate gasketingT? materials such as cork, nitrile rubber, and nitrite rubber-and-cork?. particles were used. While satisfactory for a limited period .these materials cannot be depended upon for the expected long life of ^ the equipment. V v. y/. S/-` 1 The terminal chamber is usually above or below the twitch^ compartment and separated by a steel wall through which the bushings ^ re inserted. When bushings are properly selected and correctly,/ installed, there is ho leakage from one compartment to the other. With poor bushing seals, and the terminal chamber above the switch, potting compounds or cable oil can seep into the askarel. When the terminal / chamber is below the switch, askarel can drain into the terminal; chamber.- ' V:V`"'V . "V II. Sources of Contamination - There ere three possible sources of contamination for askarel In- switches and terminal chambers; they rank in this order of frequency: / (1) water entering through poor gaskets; 12) decomposition products /' from arcing when switch is used to break magnetizing current; (3) * entrance of pothead or cable compounds through leaky bushing seals. Unlike an askarel transformer where the amount of contaminant Is likely to be very smalt (probably only trace amounts) in relation toth# volume of askarel fluid -- in switches or terminal chambers with faulty seals, the amount of contamination can be relatively large. > y f; Experience has shown that, based on the number of installed ! askerel-swltch units, the percentage of failures is extremely small. When investigated, it has been found that most failures originate in the switch chamber. Water is the chief source of contemination. However, heavy y contamination of askarel with petrolatum and asphalt material, due to,^ leakage, have caused a few failures. . '/ . ,V\y. ' : . ` i k Petrolatum is used frequently for filling terminal chambers. When either cabte oil or petrolatum seeps into askarel, no great harm results. TheV; fire resistance will be somewhat decreased and power factor of the * askarel will increase with an accompanying drop in resistivity. While highly undesirable, it H doubtful that failure of the unit results. Whore < > asphaltic compounds ere used in place of petrolatum, the danger It * increased somewhat because asphaltic contamination may caute excessively high dielectric losses in the askarel. .. :: y ^ When the terminal chamber is below the twitch chamber, the potting compound can be contaminated by askarel if the bushing seels ere ' leaky, This is undesirable because the eskerel will increase the power /1 factor and conductivity of the potting compound or cable oil end , develop heat from dielectric loss. If this mixture is drewn into the cable 0?ObV3? TiCi) TOWOLDMON0025137 WATER_PCB-00009606 `fablerfailurt' Is likely* vIhisagiln emphasizes tht " ^f^P***^* K I'yjv ', ^ ini'idling Switches and Terminal Chamber IEEE,.Guldt JcK,.Trartkformer;^jkarel; caMl aiterv jarlnQi i'4(f ^.> . ':V\ S;*'Atkaral Is used, to'some extant, In apparatus where It is subjected v %o*IJoht Intermittent drclng.r such as in self-contained Induction f .-/' v:Vvh </j; /$.* fegufatorir'`Whei1e<'operating switches ate continually producing ^*s arcs; 1^transformer de-energlzing switches, etc., Under*1; ' * ' iW^TtV^normaroonditlohS,'deterloratiort of the askarel li very slight.* '-.Vf',: ' *' s*v; wHnoewnevaesrK, iIrmeipiroperly adjusted or defective switches In this type of ' t M\ ,t .,>fi/t?*>y: especially for irvA/^iiM * AusvAttfiMi *i\H nrnlnn/ift iM;:lnullnfrequfleunidtl.y ^Y'1' - blackening lg^'4:^?.;malntflnl,>g^>cavenge^atthe,apprpprlataconcentration/* v I V'V(Vv:' ,* U j '4* '* V\f`l Malntonanc* for Askarel Filled Switches (* '' SsU1''A*: Switches used for grounding after .power source has been.' * *)'/ '** * I Vr*? >* V deonerglred will not undergo arcing. v'v v '' - "' " .r. * , >' `y- . v :. '. ?.rj .: " -' ' 1 ' !" *``1 '* *' - \t V1'^' ^ 8. Switches interrupting magnetizing current will be subject to V', -V .; arcing the amount of decomposition wjIJ depend on power SnV , interrupted, lime and frequency of operation. As a general rule, 'K:* yi.*!-! *.:. the liquid should be checked after 6 to 10 operations. > i '>' > ** 4* > `-'J < vi >;*},! > jiV* V- -1, On newly installed switches, check the askarel at 3, 6 and 12 month Intervals; if found satisfactory, check onoe annually ; thereafter. With proper attentioonn to the gasketing of covers \f . and bushings, experience will prol ably indicate that less ` *, \ *, J %: 1 r \ , i i , ' >>? ? i V V' >Vl*.r ' ^ if`vV ,\ . ^ *' \*\ .' s /' '* 2 frequent inspection it warranted. A'3 J:! - 2. . Check askarel for: t , a.; Dielectric breakdown voltage (ASTM 0877): It should ]\tf, be 26 KV minimum. If dielectric breakdown voltage _, ;* u'.-s3,low, confirm presence of water by Karl Fischer method jfi?7,i' r,?<'ASTM D-1633. Filter to remove moisture. Dielectric V'//'* ' strength should then be 30 KV minimum. / "j , b. - Presence of carbon from arcing: Fluid should b..e. ; : ^..rolatively free of carbon. If badly arced and very black, , ;. )')'. ..j; 'V-WK y - ; v, , s * ;`.Uv, v i i' A \'nl- 4t-V'-:.vV ,>Vv )- replace fluid. If only minute amounts of carbon era . present, filtration is recommended. Check power factor ^ : Eic'T'V' ' ij`11.1 liquid (should not be over 6% at 25"C and 60 cycles). ' 1 : Flush out switch thamber with several gallons of fresh * - ! askarel before refitting, II there is discoloration, high power factor, detectable change \ ; In specify gravityor refractive index, or if fluid flashes below. -( tt&f, there Is a possibility of seepage of potting compound - .1- Irito the switch compartment. In this case, correct any leaky bushing Mats' with. propet. replacements and fill withnew r;;>.-vV: V'/-askarel;-u' 'Ii i'rl'i 4A`tf 'terminal -'chamber ;.ls 1 I ' TOWOLDMON0025138 WATER_PCB-00009607 : _____ '.'ii*cj* ggfc pMM,Bki*7**Z * <r '. ' v/j ,. - ms. , . by swelling and cracking of the exposed edge. In T : severe deterioration, liquid seepage is usually present,'> , > 6. Check for leakage at packing gland of twitching shafty'lf/ leaking, repack with a Silastic ring type Qasket. -: A'rVi^v - . -v '.t '\j "v VI. Askaret Under Excessive Temperature' pr' Fault? Conditions . .a. \ *? ;; /The IEEE Guide also points out that, > "Chlorobenzenes used In transformer asksrels begin to boll at temperatures of about 205*C, under atmospheric conditions. If th# ! v*material Is heated to such high temperature in a sealed yt*ri% ; pressure develops. Pressure will also develop in the system if tha^t .. askaret Is arced sufficiently to generate copious hydrogen chloride ^ fem%^rr/v ;:a;;: . *" r 'Therefore, it Is recommended that wherever possible, sealed^ 1:* s-Vv"v. - fey " ,/ ' ' ( \' `< ->. ` askareMitled equipment be provided with pressure relief devlcos.7 Th$se devices mutt be large enough to provide immediate relief at ' a definite pressure, and to prevent further build up of pretsufe If - decomposition continues. It must be remembered that the ( presence of devices of this sort does not necessarily preclude the . rupturing of containing vessels, since pressure build up can ba . extremely rapid under violent arcing conditions." v k^v^.v.- & YV.Y'-.v : . ' - vVW* *M mIwl- iiif \ m '' "< - S($flnin . Toxicity& Safe Handling if i\ . vr I. Inhalation ' ' / At ordinary temperatures the chlorinated biphenyls in Askaret have not ' presented Industrial toxicological problems. The hazard of potential 1 toxic exposure varies with their volatility: the tower-chlorinated, more- 1 volatile ones present more of a potential problem from the standpoint ./ of both inhalation and skin contact. When Askarel fluids are used at-j elevated temperatures, engineering controls must be applied, either by ... the use of closed systems or by affective local-exhaust ventilation^; together with genera! workroom exhaust . : ^ v^ >: , w; Hi': v;Wv ;; ill kfcYv: Vapors of Askarel at room temperature should not be breathed Wa.:< confined space, and ho vapor of any fluid evolved at elevated .temperatures should be aljowed to be dispersed into the general v - .workroom. i'yv :' :$yv lYYr.-v Y r':-' a-' v ' ,A; , 'L Inhalation tests on animals indicate that the maximum safe concentre-Y tion of vapor is In the range of from 0.5 to 1.0 mllligiem per cubic { meter of air. The threshold limit value (maximum allowable concern tratlon of an 8-hour working day) set by the American Conference of Government Hygienists are 1.0 milligram of the lower-chlorinated - biphenyl compounds per cubic meter of air and 0.5 milligram of the / more-highly-chlorinated compounds, per cubic meter of air, y Y'? II. Skin Contact - ' '' " r . ^V Prolonged or repeated skin contact with the Askarel fluids must be* avoided by the use of gloves and protective garments, because of tha y possible occurrence of a condition called chlorecne. Although reports, of this condition caused by Askaret are rare, it can be produced by< excessive skin contact. If the fluid is spilled on the skin tire skin shouldY ; be washed In the usual manner with a soap aolutlon. . Y j: ' A burn caused by contact with a hot Askaral should be treatad Ilka any r . ordinary burn. .* -' t-iYi ^'-'y 3' . r * r v < ' . For disposal instructions Of Askarel fluids, see Section A* VIII,pegs 6. 0?05^34i TOWOLDMON0025139 WATER PCB-00009608 .'/loffi tfflO '4 clMr^ci 4/ Ars+lysfl ^ *-*-> fro*i '. : '. " * !y.,;' Analytical Services X-s'.' v,v-a on Transformer Askarel BIl'i^i^lJl'^aiiable/Ilroni^MonsantoJ tm. fii Trantforrrw user* not wishing to make their own fluid analyses can obtain the service from Monsanto. Simply contact Moroentp/ff ^pacify what analyses are wanted. You will be sent the proper-sited, clean temple container, fitted with a proper label. When"# Sv ydu; receive this, carefully'take your sample^ (following the procedure for tempting in this guide). Send the container J\'Mohanto' laboratory. Charges listed Include temple container and laboratory costs. The charge* *r* those in affect March 5 ROUTINE MAlljtENANCt CHECK >*4, ; ' Total Cherja: *30.00 T MT 1,'|. < 'ihV'1''.#' 'W ` `i'.JVHj ,,...... .................................. . ....................................... ^ Total Charge: $75.00 ...... ?. . . ., &<1) To determine the extent of fluid contamination, (2) earth refinement to determine what degree of restoration of alecirleet and Q Insulating properties U possible, (3) check teat to tee how tire fluid responded to earth treatment/< + > ,/ ' y o r . .4 yf 'V^j 2li) Complete Analysis: to determine the axtentol contamination 1* *-"* \ Properties Tested >`,h Free Chlorides ^ Color and Condltloo\^*J< >Y* Acidity ` 1 |V>lf^'Specific Gravity * {, ^.y **f \ k ' Dielectric Breakdtown Voltage >.: . f.*5; i Refractlvi Index *j -A Power Factor, Dielectric Constant, and Resistivity fv . jli w- w ' ' - ` >, ' ' , . , *Vyb) Earth Refinement Retponte: r. : - /'/'. Consists of treatment for 2-5 hours at 50-60C. with 0.1 to 0 2 percent by weight of Properly conditioned Attapulgut clay Vv' ahd then filtration through dry filter paper. s-, t <. i , tYd Analysis After Laboratory Earth Refinement: \;-V\ .t-i; iM iw'.' . ; Properties Tested 1 y *]' Refractive Index \ . .y ,r ^.v'V Water \ * Free Chlorides _ Acidity1' V'%'1 >- Dielectric Breakdown Voltage ' ' ../.Y 4 Power Factor, Dielectric Constant, and Resistivity ,, '' hi To determine whether the entire lot of the askerel fill responded to the same extent ft':ffQuUad) VtV \\ ,1 v/ j\V Properties Teitod ;V v'y/ ' , ( ` 4 B/ Color and Condition ` , *'* ` ,, . V,KjFtefractive Index ^ Free Chlorides ! Acidity IDielectric Breakdown Power Factor, Dielectric To arrange for the tests described above write to David Wood \1 V/ ^ 'J` Monsanto Industrial Chemicals Company ^' V BOO North Undbergh Blvd/.-'^'i/.; * < , LouitMissouri631 W|V'.-iifay::,* ' fsampias to ba tested should be clearly marked for identification and sent dlractly.to? * Monsanto Company V V', '1, -.'- - , , j,w* W.G. Krummrlch Laboratory .^ ..V'?'.>'* K^'Seuget, Illinois 62201 'Ms-'- ' " - ' - / Attention: 4^rKutf ' rr.fl, C/eccIt*tr. V'VvYv1 v*,V ; .**'*y '..* 0?0S'|3^ AS- ` TOWOLDMON0025140 WATER PCB-00009609 m .!ir . * ' f w; V , SOLUBILITY OF GAS IN TRANSFORMER ASKAR ELS 'fI,o'. f^e..v'*T v-,Y >. ./vVii y'\':;v ASTMTYPESDANDO ,, , *t , t '* . iU * % ;?rV ,:\. ; ,: j' i,,f' i < *' , . . y *' ' Percent of Gat By Volume Corrected to: * . . - `t.o ' - f Y'Wl. `'``iv. V . <} V. 26*C 760 mm 1. * i. 0*C;.760mm ym '' V.;v...V xx locro. V ,'* XX iooo`?'<' -V ' 4 ' ' Carbon dioxide v" . .. 71% ' '*' 47% {- .7 >' ': JiiV *' .;* v * i . .Air :',.kr. * ,* .. 6.7 '> ' Nitrogen . ^ * Hydrogen chloride1 V . 6.0 ' 376 : -v . 1 In ebience of iceveoper 4.9 , 46 60.9 ! 4 68 , - 66 ; ! 'V 6.0 i ` < 4,4 /fi ,,> ;; K< . '.I >acwl </*! i___i.-'j :. Jr,'*.1 *', > 't v.r,-'i*,4A ,.' TOWOLDMON0025141 WATER_PCB-00009610 APPENDIX D '<Wi!V COMPARISON OF THE APPROXIMATE VISCOSITY IN SAYBOLT UNIVERSAL SECONDS F transformer askarels and mineral oil Pyranol p- V.f-r' '* A1333B-3 IOC Mineral' Oil J Inerteen 70-30 * 1,000 > V -1,000 2,800 .100- * : ' - ,160 ' 195 'V 70 : : 85 f 8b <-V :/; r'>>; 49 . *' '60 . .'. 39 . : so.-y1\ r'l-^Ar.*,'r 34 40 > , 34 1 *` * 40 , *, . , 30 . 30 ' 30 ' 33 I/O' APPENDIX E ^7 -~ Ms' "viy* THE DENSITY OF INERTEEN 70-30 . AND TRANSFORMER PYRANOL A13838-3 : ;C`., Approx. Density gm/cc. . , . ?. ' ' V'' ' 'jV1'^,i Ttmp.*C v' ' 0. 20 . : i \ 40 ' . *, 60 , 4 1 80 - ' y-Inerteen .-. '7 .v-y 7030 - Pyranol . ; B A1363B 3 . - . / 1.674 -b" bb /:` r&?7 * V : .- -L -' . V 1.652 , 1.555 - ' 1.629 * \` 1.532 > 1.607 * 1.510 < 1.485 ' M88 APPENDIX f ' ' ^T'.'^' .. / _ . The thermal conductivity values of transformer Pyranol A13B3B-3 at 27*C and 68*C are 26.2 and 26.8 x 10 s calories centimeters1, degrees centigrade1, second1, respectively. Or, approximately 0.06 BTU per (hr.) (sq. ft.) (*F,| per foot. This same approximation applies to Inerteen 70-30. .' APPENDIX Q Heat Capacity '` c' > ' , Overlhe~lemperatura range of 26* to 126*C the specific heat of transformer askarel is close to 0.30 calories per gram par degree. . ' r . i APPENDIX H v: Coefficient of Expansion ( ^, ,, . .. The average coefficient of expansion of transformer askarel over the temperature range20to 100*Cis0.0007oc/ccAC.Or># gallon would increase to 1.056 gallon! on heating from 20 to 100*C. ;, , . ; iyc APPENDIX I m fc Fire Resistance ' . Askarels of various compositional types are used. Under arcing conditions the Qases produced, while consisting of. , predominantly non-combustible hydrogen chloride can yield varying amounts of combustible gases depending upon the ^ I "VfjT I | askarel type, 1 1 - * ''V-' . `I" v w Insulation systems incorporating these askarels and cellutosic or other organic materials may, when arced, produce gaseous ` mixtures which are nmoderately flammable. As e precaution, such gases should be removed from the askaret by bubbling dry . nitrogen through the askarel and flushing the gat space with dry nitrogen before any work Is performed on the apparatus. Tr'VV-l I rju . K J- tfv-v'V' v".'- .v... vs V.v`^`7 >S:'V ` ;-Cv/ ' ^ A-> -i*. ; TOWOLDMON0025142 WATER_PCB-00009611 APPENDIX J Stall properties and Procurement Dow^Corning Corporation, Midland, Michigan with Districts at Atlanta, Boston, Chicago. Cleveland, Dallas, Los Angeles, New York City, Washington, D.C. and Toronto has available Bulletin 09-019, August 1962 entitled "Silastic Design Data". This lists the gasket fabricators throughout the country from whom the "Silastic 50" gasketing can be purchased in sheet, extrusions or molded shapes. Generally, Silastic 50 sheet goods are stocked by local die cutters, hence, could be generally purchased locally. Usually small Quantities of gaskets are die cut. If larger quantities are needed, tools are made of the same type used to cut other lailomers. Where the gasket is extruded for fitting into a machined groove or between gasket stops, Dow Corning advises use of a tcarved joint. This joint is then cemented using Dow Coming's Silastic 140 (clear) or their RTV 731 (white) materials, which air cure. Dow Corning points out that the local "rubber" fabricators purchase the Silastic 50 In billet form. This is worked on a roll mill in preparation for sheeting or extrusion. Then to obtain the desired physical properties the fabricator must oven cure the Silastic 50 for 24 hours at 480*?. SPECIFICATIONS* ASTM D676 ASTM D412 ASTM D412 ASTM D395 Color Specific Gravity at 77*F Hardness. Shore A. Scale Tensile Strength, psi, min Elongation, percent, min Compression Set after 22 hrs at 300F, percent, max White 1.20+0.02 45 to 60 800 250 30 "All physical properties measured on 0.075 inch thick samples molded 5 minutes at 24CTF, and oven cured 24 hours at 48CTF. APPENDIX K______________________________________________________________________________________ Caution Label The following or equivalent caution statements should be fixed on all containers of transformer askarels and the transformers themselves: This product contains Polychlorinated Biphenyls (PCBs). Care should be taken to prevent entry into the environment through spills, leakage, use, vaporization, or disposal of liquid or containers. Avoid prolonged breathing of vapors or mists. Avoid contact with eyes or prolonged contact with skin. If skin contact occurs, remove by washing with soap and water. Following eye contact, flush with water. In case of spillage onto clothing, the clothing should be removed as soon as practical, skin washed, and clothing laundered. Monsanto MONSANTO INDUSTRIAL CHEMICALS COMPANY 020^36 8PECIALTY PRODUCTS GROUP 800 N.LINDBERGH BLVD. ST. LOUIS, MISSOURI 63166 The information herein regarding obtaining optimum results from askarel fluids in your transformer has been accumulated by Monsanto for over 40 years from the experience of makers and users of askarel transformers and It is believed will be helpful. Nothing herein shall be construed as applying to other than askarel insulation. Data and maintenance suggestions herein do not apply to the other components of the transformer. All operating and maintenance suggestions recommended by the manufac turer of the transformer should also be carefully followed. Because these maintenance directions apply only to the askaret insulation, Monsanto disclaims any liability for damage to property or injury to persons arising from transformer operation. TOWOLDMON0025143 WATER PCB-00009612 .. i >s ,, A } ' < ' "SSS : , t LbJlS b)t$OV*J vote'** v,;.'; /1 i #n*m rpv;j?|LiiwW -.km: T.' *>* ll ttyfa. I v*rf ;, > 'ifef .......... ... // **< "WSXPS.^ . tynf 1 ftf. . ________ T____ c-&3 * ftf-.'M** - v;-. '. ; Auf* trot * 4 ft,-. Wtomim&maitA .' .r.?. vt>kWvAnK- ....... ____ i>.. j.ff..#.!.yj.r.... . ... " pebfflfnnv^li *V * *r * :'-f1 '. '.\"V><>'- > *'. r /Li *p*wr V* \ * ' -;. '' rL $i vauAk '! * > emumAt .' A ` > '" r, j'..'olo Cr-HOfXHk' 1tlS.Hio.IS A <rf'<>/> ,. ` trA"Mt$*rth>h4t**\ ^ii tvtJpr. ti$*Kn?0r ) , ,t </2' *f**l< . S_^__k_ H__O__/_j_U__ . _ . 7 t - ------ nezA.>--*--u--f-l-r-t- -------- * ' '; V l Montiito fStyri WW A9j `> 'It v Atl*dk'k*tvQC20 V f,,t ; , * opu#H#i{ttix\tlr^r>a * * t> #`l/ftf04jC?i * , `' , .\ .- Mp/)rtPte ^ue.'fp ffcGCow/wy ***** nft/wrt-*M* Ar*^t. Beorrnnjdutn fff. % fibPMjufmmipttt * X thAm ^ * * J j ** v \"`''yT','lS`'itfc?ci*i9jte''v>r>to$& "O'*' " \H t"?,`-'h-^^ 'ftftm., , .. ________ ' - < -^ v;km'HS'T , u/ 1 ^ fOS. Cn*ty t"<3s-A ?tf> Aw 'i - 'C,-|^,S.W/r, nfa hwMWM i' J>f AldiMriNA' tr , ' Afjr f 0 'U'iQ f(A> * p ' pM M Ar^wifty A <> * ,, ...... ` ... . k*PflA.'>ta AvU't'it fati Tortf^ ^r^4Mi <Wt# ' \b1 Tin<k',$\4i~,- ' ;-.: Wi yxh'k&Qt i v , v- ^ ft, ^ ... ,..,- .,.-0 ; v..' V-O". ii..N,ys-"1'.'-;' '.v^' .lll* ffo$rt ^dtor, OtyBl<* : ' '' ,- rjit2<rt*$ >1, ^ J 7 1 ' SjPcWw^f/iuwjtfSpi/rfcAf/rfd G...t.A...ti/.n, tlf.t..b..t.y. .H..v..M...v..r..ii.i.a...:--_.-^---* >.>-. - rf'" ^ >/ ; .v . ; r* e*nt*t.. - .,... )Vi>'r-:: AW'JJ^/ptfAt WiPwW, 2njFl<W >;' , Wcnr . -\ i ^ _ s '/ ~ V ' t ....+?s?L.'.-` Hr.n. fto/gft*S.A.V. ,; - ^ , Itpar o }599 i . ,,Sa<1 &re*f9*11l&*'i3 A ` SAtPt/f r ' .-?. ^: tfc-AWit0 (ScantJthavM Ak :V'vsoftd!ffi*fi t06 r. f> . f n A$V <,, '* 4;< `ll'A ; Pot Qt<k*B- tint A^Utt* ^ v S.- ibAv ffWftrtJJ k ^1 a* iMfpAmu'*imfiw *f e * >f i,f. f>0 $t to Ha rttM iv> ^ f# - ,* `. # . ; * v V;fs:lf: , h *- * < Sds&irfif/ais; t ftpnch) ? * -T* ,, ; .. !f; ".. gate Mwt am'I'I T f i /7 , 1 i '', 4* 5pL>?* *V i< V 1- " 1 h*nAuV4*W* \ t A wtt" * " W<>> f A*.'' ; . it Miwm ' i, { ( ":: ............ r^ jMt v ^ ' ' /MtlT ^ ^ fiilH lrr4pi Vh Mfhh o it (itola 4 < pi*b9njt4 Hn , t Ht ^ } ( - 1 1 J* u ,ri * > t' I ^ . 'A .J/ ^ . i .. * rttac/ouA hf6AMnt p Pk fartVertt o * : e .'ft'.* *' ' it;. ..\.a j ' ` .i ',..'.iV '; p,'!'-, u t s l%i <k. ^47'rv`A^ ' ' '' " .`. ,v.,...v.r .I.-,. -.r .. Afao**'f ! .- ^ ft / ffaay*iKMr*4w bh&w '' l < V ' fjf'VL .;;V'.:X i-1^:. ' : "" ------------------- r' `4" ^r".................;...t^W-r..Av'e,til Cf.iTit'Y . -. .atAfHci......,..,... ...... ..,, ^onsanio Vfcft. Ij f r* V A' .y . > i * ^ Ir I'I I I I I .A ^ t ' 3 . w * .^..4*. TOWOLDMON0025144 WATER PCB-00009613