Document QoveDMd71o9ra8yRvZD3Kzn7

DISTRIBUTION LAST PAGE KN'-77t '10. Copy No 11 . E, I, DU FONT DE NEMOURS & COMPLY- ...... ' 11 ........... ' *' i|` > M l I . l ,. , ,.-VT`"S *V "! 1 X ' NEWPORT PLANT PIGMENT COLOR RESEARCH REPORT TITLE; "AEFLAIR" PRODUCT QUALITY WORK DONE BY; D, P, SCHUSSLER REPORT WRITTEN BY; D, P, SCHUSSLER , REPORT APPROVED BY; C, W, ANDERSON PREVIOUS RENTED REPORTS; KN-76*-4 CR, D, NELSON! PROJECT CODE; 8I-1Q2 PERIOD COVERED; APRIL, 1976 TO JULY, 19.77 NOTEBOOKS; E-8437, E-837Q, E^-12474, E'-12478f E-^12485., E^12937 TECHNICAL ASSISTANTS; L, I, ASAY (APRIL, 19.7E TO MARCH, 19771 P, CERESINI (MARCH, .1977 TO JULYf 19.77! ABSTRACT We have determined that the dominant facto?? governing flAfflair"1 Luster Is the face area per unit weight of the mica flakes.. The dominant factor governing opacity la the weight percent Ti02 of the pigment, The best examples to use to compare DuPont "Afflair" products with competitives are DuPont's NF-138-D and Mearl's Superpearl. Physical data shows that Mearl's Superpearl is superior in luster and opacity because its surface is free of the raudflat cracks (or crazing) found in DuPont "Afflair" products. DU P050108570 OBJECTIVE ~ l`^ The purpose of this study is to determine those factors controlling '^flair" quality, particularly luster and opacity, - SUMMARY AND CONCLUSIONS o Relationships between physical data routinely ' gathered on ^Afflair" products were examined. Through the use of the ESD program RAMAR, we have found that the opacity of an "Afflair11 product depends on its Ti02 content. The luster depends on its face area/unit weight. With some exceptions, it can be restated more simply that the opacity depends on the diameter of the place and the luster depends on the thickness of the flake. These factors account for the greatest differences between "Afflair products, i o DuPont "Afflair" products are in general deficient to competitives, comparison of products show that DuPont products have a higher surface area/unit weight. The higher surface area is due to crazing, or mudflat cracks, in the Tip2 coating, Methods of hydrolysis that avoid crazing, demonstrated in the laboratory, result in products equivalent to the competitives, PATENT STATUS No patents or patent filings have been made. PROGRAM No further work is planned, PUBLICATION STATUS The material in this work is not suitable for publication. SPECIAL SAFETY PRECAUTIONS None. ENVIRONMENTAL CONSIDERATIONS None. DUP050108571 T' 2. t \ :Ti"'AB'"LE OF C'iO"N' 'iTENTS% INTRODUCTION THE OPACITY VS, DUSTER GRAPH EMPIRICAL DATA CORRELATIONS DUPONT "AFFLAIR" VERSUS COMPETITIVES ' Page- No , 3 3 4 6. DUP050108572 * > 3 T INTRODUCTION The work described in this report is in large part a continuation of studies initiated by R, D, Nelson, For additional background information, the reader is referred to in the Monthly Summaries, 1376, by R, d , Nelson, This report is concerned exclusively with the properties of pearl Cor white) "Afflair" and competitive products. No only do pearl "Afflairs" account for most of the sales volume, hut they are also more easily studied than colored "Afflairs", Detailed descriptions of each DuPont and. competitive code are contained in the Product Data Sheets issued in 1976 by R, D, Nelson, The physical properties' of "Afflair" of interest in this report are defined: Duster is the amount of light reflected at the "mirror" ! angle hr the shininess, It is measured as total specular reflectance, ,t $r , Opacity is the amount of light reflected at an oblique angle. It. is measured as total diffuse reflectance, TDR, Interference hue is the color observed at the "mirror" angle only , it' is measured as the ratio of blue ref lectance at the "mirror" angle, s b /r . Absorption hue is the color observed at an oblique angle. It may differ greatly from the interference hue. It is measured as the ratio of blue reflectance to red reflectance at an oblique angle, d b /r , partitftflnri'ty is the relative amount of graininess and is ' governed by the particle size distribution of the flakes. It is measured as the weight percent retained on. a 30 micron sieye in wet screening, THE OPACITY VS, LUSTER GRAPH A construction found to be very useful in describing "Afflair" product quality is a plot of opacity, TDR, versus luster t TBR, Figure 1 shows such a plot for some DuPont products, some competitive products and some experimental samples. The points on this graph are concentrated in two areas along diagonals. The first group lies along a line where TSR +10 TDR = 1200, These products are made DU P050108573 - 3 r- FIGURE l T- OPACITY. VERSUS LUSTER FOR REPRESENTATIVE "AFFLAIR'- PRODUCTS DUP050108574 ^4 THE OPACITY VS, LUSTER GRAPH (Contd.) from unclassified mica (excepting NF-152-D, see KN-77.^11 and include the precalcined mica products. The second group lies along a line where TSR +10 TDR = 1600. This group is composed of pigments made from classified mica. Referring again to Figure 1, the opacity-luster graph, those pigments on the TSR + 10 TDR =* 1600 line have a greater ability to scatter light per unit weight of pigment than those on the 1200 line. One might describe the di agonals on Figure 1 as "iso-quality"lines. There is substantial variation along each of the iso-quality lines. Within a group of "iso-quality" pigments, with higher luster must be less opaque, it is shown in more detail in the next section that the variation along each line depends on the % Ti02 of the sample. Ideally, those pigments of smaller particle size contain a higher percents <gt of TiOy and have more Opacity (less luster) than larger particle size pigments. EMPIRICAL DATA CORRELATION We routinely make a number of physical measurements on our "Afflair" products including % TiOo, face area, surface area, particle size, etc. Relationships between these quantities have been obscured by the large volume of data available and the tediousness of sorting through it all. With the help of V. Bacchetta of ESD and the use of the computer program, RAMAR, relationships between these variables have been revealed. Data from 14 DuPont pearl "Afflairs" and 5 competitives were used. RAMAR produced a table of correlation coefficients relating ' our quality parameters (TSR, TDR, etc.) to the various physical measurements {% Ti02, face area, etc.). A small portion of the table of correlation co efficients is reproduced in Table I. A correlation coefficient is a number between -1 and 1 that shows the statistical re lation between two variables. If the correlation coefficient is i, the two variables are perfectly, directly proportional. If it is 0, they have no statistical correspondence. Negative values show an inverse relation. Examination of Table I shows that luster (TSR) is very dependent on face area/unit weight and, indirectly, thick ness. Face area and thickness are not independent variables? they are two descriptions of the same variable. For con venience, we will use face area in developing this point. DU P050108575 -5TABLE I RAMAR CORRELATION MATRIX FROM "AFFLAIR" DATA VARIABLES % Ti02 2 Face Area (m /g) Avg. Diaxn ) Thickness {u) TSR -0.042 0,830 -0.312 -0.760 TDR -.852 -0.420 -0.603 0.077 DUP050108576 - 6~ EMPIRICAL DATA CORRELATION (Contd.) Table I also shows that TDR is highly correlated with % TiO, and average diameter. Again/ these two variables are interdependent. Particles of smaller diameter have a larger surface area/unit weight and thereby require more Ti02 to attain the same coating thickness. Exceptions to the in terdependence of diameter and % Ti02 are found in precalcined micas, which have Ti02 contents out of proportion to their diameters. We will use % TiC>2 in the following discussion because its relationship with opacity is linear and direct. Figure 2 shows a plot of TDR versus % Ti02 for a large number of data. The equation for the correlation line through the points is: TDR = % Ti02 x 1.93 (0.24) The figure in parenthesis is the estimated error in the last two digits of the multiplier. Figure'3 shows a similar plot for TSR versus face area. The data are more limited than for the TDR * % Ti02 correlation. The equation for the correlation line is: TSR - Face Area (m2/g) x 889 (156) The estimated error (in parenthesis) is larger, relatively, than the error in the TDR - % Ti02 relation. The larger error is probably due to the difficulty in making accurate face area measurements. There are certainly many other important factors in describing the luster and opacity of "Afflair" products in addition tp face area/unit weight and % Ti02. But the largest differences between "Afflair" products can be accounted for on the basis of % Ti02 and face area alone. Alternately, with certain exceptions, the luster and opacity depend on the thick ness and diameter of the flakes. DUPONT "AFFLAIR" VERSUS COMPETITIVES It is apparent from Figure 1 that DuPont "Afflairs" at the time of this writing do not have the high values of TSR + 10 TDR observed for many of the competitive products. NF-138-D, made from classified mica, approaches the TSR + 10 TDR - 1600 line more closely than the other codes. Because it is made from classified mica and has a high face area/unit weight, we expect that NF-138-D should fall on the 1600 line. It is apparent then that factors other than those SO far discussed limit the quality of DuPont "Afflairs". DUP050108577 DUP050108578 TSR (LUSTER) FIGURE 3 - TSR VERSUS FACE AREA FOR PEARL UAFFLAIR'? DU P050108579 -9 d u p q mt "AfTm,m* v e r s u s ceontd,i Table 'll compares several of the physical properties oi NF~138-\D and Mearl's Superpearl. The fact that Superpearl Is more opaque than NF<->133t D follows from its higher Ti02 con^ tent* However, since their face areas are similar (given the error in this measurement! and since they are both ma4e from classified micar we would expect n f ~138d to have a much higher Itster, We.finally note that the surface area of Superpearl is smaller than that of NF^138HD* The higher TiO, content of Superpearl would lead one to predict a higher surface area for Superpearl, Figure 4 plots the % Ti02 versus surface area fcm^/gl for some DuPont products and some Mearl products, we see that all of Mearl's products have a lower surface area than is ex-*pected from their Ti02 content, One may think of % Tio? as a type of surface area measurement. Because the coating thickness must in all cases he the same in order to obtain a pearl Cor white1 pigment, a specific amount of TiO, is deposited per unit surface area. The Mearl products show a higher surface area than DuPont's'by their TiQ_ content, but a lower surface area after- the coating is applied. The most reasonable explanation is that the coating applied by Mearl is less porous* Figure 5 compares s e m photographs of pigment flakes at 2a, aaox of Superpearl and NF^138~D, As we expect from the surface area measurements, there are very few pores and cracks in the Superpearl coating* The e if ~138h d coating is heavily cracked, IvN'-77~12 describes two methods for overcoming the , deficiencies in NF-KL38d , One method, developed by L, 1, Asay, is to- recoat NF138'D with a thin T1Q2 layer to fill in the 1 cracks, A second method, developed by R, F, Graewe, is to apply a coating that does not craze, Graewe's method uses rapid caustic addition during the TiC>2 coating application. Both recoated NF~138h d and the product of the base addition method show the craze~free coatings characteristic of the Mearl coatings. Table ill compares the luster and opacity Of NF^138r>Df Superpearl and the two experimentals, Recoating NF^138^0 results in a pigment more opaque than NF^138HD but With similar luster. The caustic addition method gives a high luster product with opacity similar to NF'-138<-D. DUP050108580 10 - TABLE XI . PHygLCAL PROPERTIES QF EF^138~P ANP KEARL^S SPpERPEARL NFr-13E-P TSR TDR % Ti02 Face Area (m2/g) Surface Area (m2/g) 1107 41 21.5 1.23 5.5 1117 53 26.7 0.97 4.2 DUP050108581 WT. % T iO - II ^ DU P050108582 JSpjV.3,38 r* SUPERPEARL FIGURE 5 t - $EM PHOTOGRAPHS OF SUPERPEARL AND NF^I38rU AT 20.raaQE DUP050108583 r* 12 rv TABLE XII LUSTER AND OPACITY OF SUPERPEARL, NF-138-D AND TWO EXPERIMENTALS NF-138-D Superpearl Recoated NF--138-D (E-12474-24A) Caustic Addition Method (1915N-118) TSR 1107 1117 1139 1266 TOR 41 53 49 43 DUP050108584 DISTRIBUTION; 1 E, Gonick ^ Wilmington 2, W* St Struve * Newark. 3, E, J, Mead <r- Experimental station 4, j, E, Romano Newport 5 S, A. Hapka *- Legal - Wilmington 6. * E. E, Jaffe/circulate/Pile ~ Newport 7, C, W. Anderson Newport 8, - R, Z, Fortney/V, A, Romito ~ Newport 9. * J, c, Chaney * Newport Id* At D, Volk Newport lit R, 0, Nelson ~ Newark 12, 0, P, Schussler t* chestnut Run 13, Central Report Index r Chestnut Run 14, n i* ,, <* w 15, Newark Research File - Newark 16, Numerical File ~ Newwfai aia uZ 17, Library Newport 18, Extra 19., 2Q, DU P050108585