Document QXm120qkqd6y7qpOOLoQ97oME

TO m* irniwl 0. W. Schnellenberger PNOM (HmMPMkMMMI N. A. Flaten/J. H. Pritchard eu r-nO? i uniterm goptiCV.V74) OATC 12-16-82 NAF-29/JHP-13-82 MX-322 RIBBON BLENDER CLEANING MONITORING RESULTS SUMMARY Filled Resins personnel were monitored for exposure to asbestos and antimony trioxide <Sb203) when cleaning the MX-322 ribbon blender. The clean-up procedure includes purging the vessel with 3M lbs of PBT prior to the actual cleaning. Personnel were monitored when the ribbon blender was cleaned with and without the PBT purge to deter mine if the purge was reducing exposures. The results showed that the PBT purge did not reduce exposures and that all exposures were below the OSHA and Celanese limits. The highest exposures for asbestos were 5 fibers/cc and 2.3 fibers/cc STEL with and without the PBT purge. The OSHA permissible exposure limit for asbestos is 10 fibers/cc STEL. The highest exposure for Sb203 l were 0.094 mg/m3 and 0.84 mg/ms 8 hr. TWA with and without the PBT purge. The OSHA limit for Sb203 is 0.5 mg/m3 8 hr. TWA and the Celanese 8 hr. TWA limit is 0.15 mg/m3. Since exposures were not reduced by the PBT purge, the PBT purge could be eliminated. The exposure data and the clean-up procedure were reviewed with the SHE Department. It was determined that the cleaning of the ribbon blender by gently sweeping with long handled brooms from out side the blender is acceptable. However, vacuuming is still the method of choice and should be used whenver possible. Also, the results show that when asbestos is handled according to the present Bishop Plant Policy for the Safe Handling and Disposal of Asbestos (Section VII-4), exposures are well below levels that can result in a health hazard. Personnel should continue to follow the Bishop Plant policy. Please review the data with the personnel involved and post the data on your bulletin board. DISCUSSION Between certain production runs, the MX-322 ribbon blender in Filled Resins must be cleaned of SEO material to prevent contamination of non-SEO formulations. SEO blends contain both asbestos and Sb203. The clean-up procedure calls for 3,000 lbs. of PBT to be purged through the vessel before it is opened up and cleaned. It was unknown how effective the PBT purge is for reducing exposures to asbestos and Sb20j. This monitoring was to determine if the PBT purge could be rafcfiSiwi*-.!-' V 12 I 602 FEB2283 '5 NAF-29/JHP-13-82 -2- Deceaber 20, 1982 eliminated to help reduce coses without increasing exposure to these compounds. Personnel were monitored during the clean-up procedure with end without the PBT purge. The asbestos and Sb202 samples- were collected and analyzed according to NIOSH method P&CAM 239 and S2. The results show that exposures with and without the purge are below OSHA'and Celanese limits and that exposures are not reduced' by the PBT purge. On the first part of this survey, the baseline level of exposure to asbestos and SbzOj during the normal clean-up procedure was established. The MX-322 ribbon blender clean-up was monitored twice. Both times, 3M lbs. of PBT were purged through the vessel prior to cleaning. The STEL exposures to asbestos ranged from <0.05 to 5.0 fibers/cc while the 8 hr. TWA exposures to Sb202 were 0.077 and 0.09A mg/ms. (Table I) On the second part of this survey, exposure levels were monitored twice when no PBT purge was used. The asbestos STE1 exposures ranged from <0.05 to 2.3 fibers/cc and the Sb202 8 hr. TWA exposures ranged from <0.001 to 0.084 mg/m1. (Table II) The OSHA STEL for asbestos is 10 fibers/cc. The OSHA limit for Sb20j is 0.5 mg/m1 for an 8 hr. TWA. Celanese has established an exposure limit for Sb203 of 0.15 mg/mJ for an 8 hr. TWA.1 Neither OSHA nor Celanese specifies a STEL for Sb203. Samples were taken only while personnel were cleaning the blender (STEL type samples). Therefore, to make comparisons to the 8 hr. TWA limits, the 8 hr. TWA exposures were calculated from the short term sample data and the assumption that employees were not exposed to Sb203 during the rest of the shift. Current monitoring shows this to be a valid assumption because all monitoring results were <0.07-mg/m* for an 8 hr TWA.2 The range of exposure levels to asbestos and Sb203 were the same whether or not the PBT purge was used. In either case, exposures did not exceed OSHA or Celanese limits. The results indicate the PBT purge could be eliminated from the clean-up procedure without increas ing exposures to asbestos and Sb202. The monitoring results and ribbon blender cleaning procedure was reviewed with the SHE Department. Monitoring results indicate that gentle sweeping with long handled brooms from outside the blender is acceptable. However, it is recommended that vacuuming is still the method of choice and should be used whenver possible. It was also concluded that when asbestos is handled according to the present Bishop Plant Policy for the Safe Handling and Disposal of Asbestos (Section VII-4), exposures are well below levels that can result in a potential health hazard.1 In particular, the policy states that: A. All asbestos contaminated areas shall be cleaned by vacuuming into the SEO Dust Collection System. 000528 KAT-29/JHP-13-82 -3 December 20. 1982 B. High pniiuri air will not b uaod for cleaning floors, veils, beats or equipment, sec. in erees vhere asbestos tutorials era used. - ... C Where vacuum outlets to the SEO Dust Collection System are not, accessible, loose asbestos shall be cleaned up by vaeumisg . using an approved portable vacuum cleaner or thoroughly . dampening the dust prior to sweeping. D During any clean-up operation, employees shall wear respiratory protective equipment, disposable coveralls, and shoe covers. It should be noted that all operators and operator helpers were wearing dust masks, disposable coveralls and gloves. Therefore, the actual concentrations of exposure to these compounds were less than what is shown in Tables I and II. The ribbon blender cleaning procedure will be monitored period ically to ensure that exposures to asbestos and Sb202 do not exceed permissible exposure limits. CONCLUSIONS AND RECOMMENDATIONS 1. None of the exposures exceed the OSHA or Celanese permissible exposure limits for asbestos and Sb203. 2. The PBT purge step does not help to reduce exposures to asbestos and Sb203. 3. When asbestos is handled according to the present Bishop Plant Policy for the Safe Handling and Disposal of Asbestos (Section VII-4), exposures are well below levels that can result in a potential health hazard. 4. Personnel should continue to follow the Plant Policy. In particular, as stated in the policy: a. All asbestos contaminated areas shall be cleaned by vacuuming into the SEO Dust Collection System. b. High pressure air will not be used for cleaning floors, walls, beams or equipment, etc. in areas where asbestos materials are used. c. Where vacuum outlets to the SEO Dust Collection System are not accessible, loose asbestos shall be cleaned up by vacuuming using an approved portable vacuum cleaner or thoroughly dampening the dust prior to sweeping. d. During any clean-up operation, employees shall wear respiratory protective equipment, disposable coveralls, and shoe covers. 000529 NAF-29/JHP-13-82 -4- December 20, 1982 3. Monitoring results indicate that gentle sweeping with long-handled broom* from outside the blender 1* acceptable. However it la recommended that vacuuming is atlll the method of choice and ehould be ueed when possible. 6. The ribbon blender cleaning will periodically be monitored* to > ensure that exposures to asbestos and Sb*0 do not exceedfe&j permissible exposure limits. -' - REFERENCES 1 Barrett, C.D., Celaneses Policy on Handling Carcinogens, November 15, 1982. (CDB-241-82). 2 Monitoring results to be Issued when the study is complete. 1 Ille, G., unpublished letter, September 20, 1982. Hawtk FMm____________ N. A. Flaten NAF/JHP/lat cc: R. G. Brandt E. J. Heinz R. G. Hilbrich H. W. Hill G. Ille W. H. Meyer A. B. Milam D. A. Reck C. A. Amond File: 1060.1 1060.6 C. D. Barrett - Dallas D. Unrue - Louisville Central Files (3) CCCTC Unitexms: Asbestos Antimony Monitoring Filled Resins Environmental Bishop 1982 000530 i8i JS* J :8J?T AtCol td4 s*HM H(0 O-* Ou # o0 < a< ^g'Sog ? m wc m^B u. a o co o oo aS 00 BJ5 2 co fH U A* cj.H O. fit 040 &m um la uu oa sI o2 Hlf 000531 jjs s*a ^ 4# S3? 3* I a J3 53 * sis 3 .H S3* h SO a SX N So 335 N OX NO CM U n CO 0 * ~ ' v eg A 2 35-a. Ii3 I 99 5 O 5 O .>oa o 0>O S3I ii: a 9 H 0 a *o ho(9 w0o ^a 0oo3 v3 o 3 3o CO o CO 0 1 CO Va *o 941 W9 ,a* 0431 *O4 O <89 93 -8 co ^ S3 3 so SO M ^ tx CO CM g 2 3 SiQd "/-%. ess SMO M X O CO 3e 5 d 3 td O <-s 3-5 Hz3 Ca3O 'X1--0 CoO ao o N O O co coo M 5i2 o CM Aco * CO o V >0 oCO oo oo V CM CO U"> 4 o o V CO 9> CO CO 9 CM N O 6 *wJ <oo9 Xm A9i 3d* H CA H <9 H CO 35 90 3^ Jb H CO 35 90 34* >o B^ I W1 M9 u uo *oo* O CM ao 35 AO --t 38 M9 uu m r* U CM CO 35 57 ss M9 O CO > n O N CM I 4kJl -4 I A CM o *o 09 9 >a 0 (A O ids N 0 aa U > r* X ~+ 04 MO* WI O 0% A OA 0 S3 CM o oI CM : rf ygr*Yr,f ^i*i y l;51 _.i * pi. z 5|B3 KNh 313 8 a ch so o *upj, -uu9 Ptut hU9 xata*i *_ 333.5 3 8 8 5; e U u M H SJSgl H p0M ^0 w04 703 ri 1 * N # 000532