Document QXJge5VzGJ1M6k49v56Mo2O8L
- 7-
Results The object of the tests vjj to determine what proportion of the
asbestos known to be present In the lining appeared as free fiber in the decomposition product.* No attempt was made at a mass balance between the material worn from the lining andj the decomposition product since It was not possible to collect all of tile decomposition product. However, the
percentages obtained in the fraction of decomposition product examined
are applicable to the total material worn from the brake and may be
compared to the percentage of esbestos originally present. In all but a few tests the automobile drum brake linings showed
less than IT* free. fiber in the decomposition product as compared to about
50% in the lining. An election micrograph of the decomposition product
obtained from a typical test in this group Is shown in Figure 3. In those tests where e significant mass of free fiber was released (Figured), the
temperature was in an extremely high range for the lining in question as evidenced by rapid drop in the coefficient of friction. Had these linings
been subjected to like conditions in a vehicle, the brakes would-have-
failed.
Similar results'were obtained In the bus and truck drum brake tests
and in the clutch test. The experimental model disk breke tested did
release some C>5%) free fibers, but no conclusion can'be drawn from.a
single sample.
'
.* *
\ **.
014
JWK007917