Document QMJwpYneZDDk2v3z9eMo451v4

' CGKriuLu iW*^- Ore ^ *> 'I .if . :'; > ' <r TO* Mid fefjainborg March 6, 1972 - -?:M' *.' ' FROM* jnisr--! . c RBi Dry Bom Xpplioatifie of^V*' V ` MONO-ROTS'*) , Updating andf - \ cc: R. CUWM H. mT- E. QO&* J. Gadis Vv J. X. Chapin, Jr. * ` 5"- ` Project Status. PHRIUOMGMREaSgSiJ WRtEBtPiAOfRlWT' A V WRG 000923 . PLAINTIFF'S EXHIBIT jj WRG-654 *'<*' rth-jactive t To develop a nethod of applying cement!tiousmm Uligghhttwweeiight material; namely, MONO-KOTE'*) 1fireproofing insulation, conveyed by air through a dry hose system and to pro vide adequate amount of water for hydration of conveyed material, by either cold water vapor or saturated steam vapor, forming a slurry within the application nossle barrel immediately prior to naterial being propelled from nozzle orifice and providing a uniformly hydrated spray of material from orifice opening. The air conveyer blowing machine should have ease of mobility so as to be easily moved on construction sites. The dry hwj.. of workabi^fc^ ^application nozzle should provide .ease r' l of" sprayed material;T* ' * id - - -.>r. < - . - History* .`Zonolite se-Research. ' `P V . v'> ,; April 1964^MQNO^KOTB^ dryJicfset. tests at Zonolite Blue Island* Plant. Illinois* conducted by Ralph J. Bragg. The original project objective was the same as our 1972 reinstigated dry hose studyt* to develop&a method of^application for lightweight insulating; rfili.and fireproofing coatings of a cementitious nature which will result in increased performance, product workability and lower overall costs. Also to broaden the market for MONO-KOTE and insitu placed insulation materials. Pilot work on the original Zonolite dry hose project was conducted during June and July of 1963 which led to our. disclosure No. 262 and to a working rapport with Meyers Bros. Equipment Co. The principle Involved with the Meyers machine consists of conveying a dry blended cementitious mix by air through a *ui table hose and effecting binder activation by cold water hydration at the instant the material passes through the *Pplication nozzle. rGRACE 25067029 TO* from* Jtoeenberg Barry 1972 Attempt* jnachix* 29 to cm type M,-K;rjfireproofing with Meyers prototype vthe$ihai/<'eejpe&lieftsity>to. b In`the range of ft.3)*too'i*ihf to-'W practical. Reformulation of the product led to the composition known as MK-6, wherein vermiculite content was nearly doubled, and the air entrainment ingredient was omitted. The type of binder used in MK-6 was chemically identical to that in Type M.K., but set time was 30 minutes for MK-6, compared to 5-7 hours for Type M.K. I The MK-6 composition was tried under field conditions at Zonolite Blue Island Plant, Illinois on April 8, 1964. After preliminary trials, the Meyers machine was set at maximum output of productivity equaling 80 lbs. of MK-6 in 6 minutes and 2.3 g.p.m. of water at 110 lbs./in.2? the ratio of MK-6 to water was 5.9 lbs. per gallon of water, at that period Type M.K. in a wet hose system required a ratio of 4.55 lbs. of M.K. per gallon of water. It amounted to a 29% reduction in water over Type M.K.; whereas MK-6^formulation at that time actually demanded more water, per^poxyid than .Type M.K. in a conventional wet hose plaster .p{*np>: r> f- Dry density-of the tested MK-6 was 21.1 lbs./ft.3. It was calculated.that 19.6 lbs. of MK-6 and 1.5 lbs. of chemically combined water constitute the volume of 1 ft.3 of cured MK-6. Therefore., a board foot of MK-6 equals 19.6 or 1.55 lbs. Based on that particular volume, 32.25 board ft. of MK-6 was obtained per 50 lbs. bag. Surface hardness of dry hosed MK-6 was found to be twice as great as wet hosed Type M.K. at the same density. An Acne penetrometer No. 149 with a 1 in.2 piston gave a Penetration resistance reading of 116 lb./in.3 for MK-6 and 59 lbs./in.2 for Type M.K. Fhe 1964 dry hose project was eventually stopped owing to an unacceptable dust problem in the system. Several approaches at various modifications were made, such as dampening the dry material at the blower machine outlet with a water atomizer. 25067030 TOi iffOHi 1 ** A. Berry Pag* Thraa March 6, 1972 fhis helpad to control th dusting problem, but addad resistance to the material Clowability causing: the dry hos* to block up at varying intervals. Regulation of the water regulfijtor^required, constant attention, causing it to be- impractical for actual? field use. The application nozzle used in the 19$4 project, was manufactured by Universal Machine Co., Winter Haven, Florida; nozzle designation A264 was made especially for Zonolite dry hose project, to be used in unison with the Meyers blowing machine. Universal now sells this particular nozzle as a standard stock item for watting dry blown cementitious materials. Model A264 nozzle consists of a straight through metal barrel with a 1.5 inch inside diameter, a capillary groove is located in the center of 6 inch long barrel, which feeds water to a jet ring with 20 mil holes set at 30 angle, confluent to the flow of dry material. The water jet ring provides a spray curtain of water in a vortex motion; hydrated material then passes through a choked (1.5" to 1.25") nylon nozzle 3 inches in length. As previously stated, the dusting problem was never really solved, to make the process suitable for field use. MO:;o-KQTE (R) formulation designations mentioned in this report will be more clearly understood by the reader after noting the following: Type M.K. was the Veraiculite Institute name for What is presently called MK-3, consisting of 100 lb. o Z.O.U. Gypsum to 7.88 ft.3 of vermiculite plus asbestos end air entraining agents. MK--.6 had double the amount of veraiculite by ratio to Type M.K. or 100 lbs. Z.O.U. to 15.76 ft.3 of vermiculite, air entraining agents were omitted from the MK-6 formulation hX-4 formulation is almost the same as Type M.K. or MK-3; the asbestos bulking agent is replaced by cellufloCk in MK-4. ry Hose Project Reinstatement: November 1971. Several tests were made with the existing equipment from the 1964 project, consisting of Meyers Bros, blower maching, water pump and Universal nozzle A2S4. All test material in this series is t<-4. a moderate and unacceptable amount of dusting resulted from A264 and the water jet holes became repeatedly clogged with M0NO_kote slurry. After widening the water jet holes from 20 mil. to 32 mil, several more tests were conducted, resulting in the si'ne amount of dusting. ipQ: ffOUi Arnold Rosenberg JM \* Berry page Four March 6, 1972 Tliwinr. ^ only signifieantVchangei.ffcei widening th wmtar jots, wm decreasing^thirUh^^fh6e^f*^Lo9ginga: -Further teits Were *made using s Therm-O^Fla3cV gun ftknufactured by I. C. F. C. 0.,'3TbH0t", Illinois; this type of nozzle was used by Cafco at one tine, Cafco now use a universal nozzle specially engineered for handling fibers. Asbestospray Co. also uses the new universal nozzle which incorporates atomized water by compressed air energy. The Therm-O-Flake gun and cold water tevts resulted in severe and unacceptable amounts of dusting with poor direction control of propelled hydrated material. t orv Hose using Saturated Steen for Hydration: November 22. 1971: After seme deliberation as to ways of preventing the dusting pro-* blern, it was reasoned that the easiest way to atomize or vaporize water and also to reduce surface tension, would be to generate steam. We established early in the test series that a fine vaporized spray of water vapor-did.a much better job of hydrating the fine material particles.' and also arrested the dusting problem, as opposed to using a solid water jet. yThe first approach with steam was made- with the Thermo-O-Flake gun which was designed for blowing fiberous mixtures; material enters the gun*at the rear an underside, then turns a 90 degree angle. Compressed'1 air from an internal stem located in the*center of the gun, propells the material to the open orifice, and becomes hydrated as it passes through a water curtain at the diverging cone shaped opening. Orifice opening on the Therm-O-FlaJce measures 3 inches inside diameter. The first thought was to use steam as a dampening medium introduced through the internal compressed air stem and to com plete hydration with the existing water curtain at the nozzle. However, upon Conducting the first test run, it was noted that the cold water curtain could be completely omitted; saturated steam provided adequate hydration, resulting in a minor amount dusting. 25067032 jq. Arnold ROSahEerg" I Jamepufr. 3er*y Pag%fave- }r 1972 r.rrff-` X-Ji- 7H: largo alu*inum,9aBt bQdyiqfthe Thexmo-O-Flake gun* tpf very ricao rtaSufaiwiiato- tadnilM became to hot to. hindU. > 8 loco t was foo^it^at W)^fS|^id adequata hydration and also ##rve as ^propellantwit appeared that tha small sod simple lt>on type .hoszle would bitf more suitable with staam. Tha EZ-On j^sign of nosssla is. tha one most ccnsaonly usad for wat hosa IDDO-KOTE spraying; it consists of an obtuaa 5 inch long aluminum nips 1.5 inch insida. diamataVr with an intamal ccmpraasad air tarn 0.25 inch insida diamatar. Staam from a portable staam generator using 1.5 gallons of water par hour was connected to the external fitting of tha compressed air stem. Several adjust ments ware made to the distance of tha internal stem and and tha noxzle opening, also several orifice diameters were triad to produce an acceptable hydrated slurry which could bar applied to metal test deck with a very minor and insignificant dusting situation. This work lad eventually toj^ie writers invention disclosure Ho. 1025 in Eabruary 1972. /; The firsts H.taam and.'dry hosa yad pilot dack, was firm/ tested ixsaAirtuary 1972.- *4 -JSfI _ Fire endurance:.time , was .44 minutes*- MK-4 was used. It-was. noted during the ,ire test,, thatr.^jjpoderate amount of jdelaminatipn.-was occuring at the interface jo&ttpie first and second applied MONOKOTE thicknesses; this appa^gntly was due to a delay in thickness build up-during application^:? Bie 10 minute dalay was caused .by a blockage in the dry hose-system. v, A surface skin had apparently formed on the first coat and the delayed second coat did not properly bond or knit at the interface It is now realised the MK build up must take place within a short period of time between layers, probably no longer than five minutes interval between passes, when using the steam system with minimi um hydration. The amount of water converted to steam for hydration in this first pilot fire specimen, was 0.89 lbs. staam/l lb. MK-4; The tw maximum parameters found in this steam and MK-4 ratio are: 0.28 to 1.2 lbs. steam per 1 lb. MK-4. The maximum delay in time between passes of MONO-KOTE build up is in actual fact, related to a certain degree, to the amount f steam used for hydration. 25067033 Arnold SS?i "ll5.M;n7 * V' M . ,7;' ^.n workable'ratio as a guide fpr further research should be ^ojcimately ar>5 Ostfcjotfl Ijfi MK-4> It should be noted rt ^k-4 in a vfet ho`*e system Requires approximately 1.0 lbs. ter Pr 1 > WC-4V after minor adjustment to the EZ-On noszle internal stem, lotting stem end 1.5 inches frea orifice opening, a second pilot test deck was sprayed. This particular spraying project, pro gressed with minor incidence of trouble or interruption. Oven Ary density of KX-4 sprayed in this second test was 20.1 lbs/ft.3. Underwriters' laboratory minimum oven dry density specification is 18 lbs./ft.3, 1 understand no mhximum density has been set by g,L. for our HK products. pilot (steam sprayed) Deck No. 2 was fire tested during the first week of March 1972,' fire endurance time was one hour and twenty-two ainutes (1:22) ;v v ` '/ The longest time/JElre endurance^or wet hose applied MK-4 pilot deck to date -iaf5^ minutes t TR-0^^28). Walt Payment. tdid correlation raeSj^rch between fire endurance time and oven dry density* it was foooidt that pilot fire test decks invariably failed within the firsts 30 minutes, if the oven dry specimen density.ranged above 23.3 lbs./ft. . :'fl* Density of Wet Hose TR-8 was 20 TT lbs./ft.3. one of the main difficulties with the Meyers Bros, blower machine appears to be in the feed gate system. The revolving segmented air lock, is charged with material from the hopper by screw feed and gravity, it revolves 180 degrees to the inverted position and becomes discharged by gravity. The discharged material falls into an air Venturi and is carried by air down the dry hose. This particular system gives an irregular flow rate and causes problems with controlling hydration. A field trip was made to observe a competitor using a Universal machine for blowing Asbestospray. The Universal machine appears bo have a superior air lock arrangement. Each segment of the revolving air lock is positively discharged by air as it rotates 180 degrees to the inverted position. 25067034