Document OJRRmEndwZzJR9d0G2LwXreX
United States Patent U9]
Myers et al.
PLAINTIFF'S EXHIBIT
UC-205
in] 3,947,286
145] Mar. 30, 1976
[54] PIGMENTED ASBESTOS COATING SYSTEMS
[75] Inventors: John L. Myers, Lewiston, N.Y.; Richard W. Lasher, Palos Verdes
Peninsula; Russell D. James, La Mirada, both of Calif.
[73] Assignee: Union Carbide Corporation, New York, N.Y.
|22] Filed: July 26, 1974
[21] Appl. No.: 492,062
[60]
Related U.S. Application Data
Division of Ser. No. 300,193, Oct. 24. 1972, which is a continuation-in-part of Ser. No. 34,796, May S, 1970. abandoned.
[52] US. CL........... 106/286; 106/300; 260/29.6 R; 260/17.4 R
[51 ] Int. Cl.*.... C09K 3/00; C08K 3/34; C08K 7/12 [58] Field of Search........ 106/286, 300; 162/3, 255
[56]
3,062,701 3.409.499 3,547.669 3.652.382 3.838,085
References Cited
UNITED STATES PATENTS
11/1962 11/1968 12/1970 3/1972 .9/1974
Novak................................... 162/155 Drcther................................ 162/155 Battuta................................. 106/272 Ganey....................................... 162/3 Myen et al..................... 260/29.6 R
Primary Examiner--Theodore Morris Attorney, Agent, or Firm--Lindenberg, Freilich. Wasserman, Rosen & Fernandez
[57]
ABSTRACT
Premium latex paints are disclosed exhibiting superior opacity and brightness characteristics, including dispersed^and liberated short chrysolite asbestos fibers having anionic pigment particles electrostatically at
tached at discrete points along the length of the fibers.
13 Claims, 5 Drawing Figures
--octss til
BKUTt.Liat>ATto stos slu*t |
aaocusmi
* T.o.-timo
| t.o,-asbestos slurry | 0EWATER
| jSVth*h*T(C asarsros | orauor
PCLLfTS I
PT 7~ nuni l KILL
otv nata [
DEWATER + TUMBLE | DRY
[~<0*B0%A5BCST0S
I
HjO*-!, 0,BLE NO I
]THamaTEO ASBESTOS SLUR fir
blind
BLEND (~MpQTHtR PIGMENTS ]
[ h|q*\C^*0THIR PlGME NTS]
H,0 AT HIGH SMCA*
E
TlTANATtO ASBESTOS SLURRY
BLIND 1 QTHtB HCtNTSk-
MIGH SMEAR H,QQTHE* RiGMENTS j.
pigment dispersion
U.S. Patent March 30, 1976 Sheet 1 of 2 3,947,286 r\ 70'
NO
U.S. Patent March 30, 1976 Sheet 2 of 2 3,947,286
ro O
Li.
3,947,286
12
and does not suggest the aqueous latex emulsion paint
PIGMENTED ASBESTOS COATING SYSTEMS
composition of the present invention in which the high
This application is a division of application Ser. No. purity chrysotile asbestos fibers having certain physical
300,193, filed Oct. 24, 1972. which in turn is a con characteristics are predispersed in water to develop a tinuation-in-part of application Ser. No. 34,796, filed S cationic charge so as to electrostatically bond anionic
May 3, 1970, now abandoned.
pigments to the asbestos fibers, to form the pigmented
The present invention relates to pigment dispersions asbestos of the invention, as described in detail below.
and coating compositions and, more particularly, to
Trc above and many other attendant advantages of
latex paints including a dispersion of pigmented asbes the invention will become apparent as the invention
tos fibers.
10 becomes better understood by reference to the follow
High quality finish and the include hiding pigments ing detailed description when considered in conjunc
such as rutile titanium dioxide (TiO,) which have a tion with the accompanying drawings wherein:
high refractive index (2.7) compared to the other in
FIG. 1 is an illustration of the appearance of dry
gredients in the system. Opacity, or hide, is a function processed Calidria fibers, one form of high purity of the difference in refractive index between the TiO, 15 crysotile asbestos fibers, at 20,000 magnification;
and pigment binder, (1.5). The different refractive
FIG. 2 is an illustration of the appearance of wet
indices cause the incident light to be bent through a processed Calidria fibers;
succeeding series of angles within the coating by alter
F'lG. 3 is a flow chart illustrating alternative pro
nately striking pigment binder, then titanium dioxide. cesses for forming pigment dispersion; The ultimate result is to reflect the incident light ray. 20 FIG. 4 is an illustration of pigmented liberated fibers
To optimise this mechanism within a coating system, of FIG. 2; and
the titanium dioxide must be thoroughly dispersed.
FIG. 5 is a graph illustrating the relationship between
Presently, high speed dissolvers are employed to impart the solids content of refined asbestos filter cake and
extremely high rates of shear to disperse the titanium degree of pigment dispersion in terms of National Stan
dioxide. Surface active agents aid the process by lower 25 dard (N.S.) Grind Numbers.
ing the surface tension of the liquid medium in which
It has been discovered in accordance with the inven
the pigments are dispersed, and help keep the pigments tion that the above advantages are obtainable with
separated once the shear is stopped. However, it has particular forms of asbestos having certain surface
not been possible in practice to completely disperse the area, lengths, fiber availability, and very high cationic pigment particles which tend to agglomerate and re 30 charge density. The high charge density and liberated
duce the optical efficiency of the paint film.
form of the fibers allow the fibers to electrostatically
In accordance with the present invention, improved bond firmly to anionic pigment which satisfies the
pigment dispersions and paint compositions are pre charge to form a highly pigmented fibrous product. By
pared by dispersing and firmly holding the pigment the term "liberated" fibers or fibrils is meant that such
particles along the length of liberated, i.e. discrete, 35 fibers are in the form of discrete fibers or fibrils, rather
highly cationic, colloidal, short fiber, high purity asbes than in the form of fibril bundles. Without the electro
tos fibers. When aqueous pigment dispersions contain static bonding of the pigments to the fibers to satisfy
ing such pigmented asbestos are incorporated into the cationic charge on the fibers, the available cationic
paints, the resulting film exhibits an increased opacity charge on the fibrils reacts with and agglomerates an
and has several other unexpected effects.
40 ionic latex particles. Without the cationic fibers, the
Even though the asbestos itself is a gray dull material anionic pigments will tend to agglomerate, reducing
and has a fairly low brightness, unexpectedly the paints optical efficiency. When these materials are combined
incorporating the aqueous pigment dispersions accord according to the invention, the pigment is uniformly
ing to the invention have very high brightness levels. It distributed along the length of the fibers so that the has further been surprisingly discovered that although 45 final product resembles and performs like a fibrous
asbestos usually occurs as lumps which would prevent pigment. The uniform distribution of the pigmented
the dispersability and a fine grind, a very fine finished fibers results in a very high optical efficiency and there-
aqueous latex paint having dispersed solids of a grind or formless hiding pigment is needed to obtain a given
fineness below 2 mils, can readily be manufactured opacity.
from the aqueous pigment dispersions containing the 50 Pigment dispersions in accordance with the invention
pigmented asbestos fibrils in accordance with the in incorporate a particular type of high purity chrysotile
vention.
asbestos. Generally, chrysotile asbestos has a low index
The pigmented asbestos of the invention in addition of refraction of about 1.31 to 1.33, is the softest and
provides improved structural strength to the film and most flexible of the several types of asbestos. When
also can decrease or eliminate the necessity for the use 55 dispersed in water it exhibits a positive or cationic
of biodegradable thickeneers such as cellulose ethers. surface charge and a very high tensile strength. Chryso
Furthermore, since the pigmented asbestos is a less tile asbestos occurs only in serpentine, a fine grained
costly product than pure pigment, the cost of manufac rock composed entirely of hydrous magnesium silicate
ture of the paint can be significantly reduced.
minerals similar to chrysotile in composition. Most
U.S. Pat. No. 3,328,238 to Knowles et al discloses 60 deposits of serpentine contain chrysotile in cross-fiber
stable suspensions of organic or inorganic fibers, in veins, and the ore typically contains only 6 to 10 per
cluding asbestos fibers, in a hydrocarbon vehicle, for cent fiber of random lengths which are tightly bonded
use as propellant suspensions, agricultural composi together in a parallel configuration.
tions, oil base drilling fluids, and oil base paints, in the
The unique materials according to the invention bear
latter application the mictofibers act as a suspending 65 little resemblance to other serpentine bodies since most
matrix for the pigments in the paint, forming a fibre of the mass of fibers are highly sheared and pulverized
thickened vehicle or gel in which the pigment solids are and consist of soft, friable sheets and clumps of asbes
dispersed. However, this patent bears no relation to tos fiber. In contrast to the cross-fiber arrangement of
34
conventional Canadian ores, the high purity chrysotile
The individual asbestos fibers are in the form of
asbestos material, one form of which is marketed as slightly-curved, short tubes having an external diameter
Calidria asbestos fibers, and is preferred for use in the of about 260A and an internal diameter of about 110A.
present invention, is obtained from a deposit near Coa- The length of the fiber varies from about 100 to 1,000 linga, Calif., occurs as a twirling mesh of disoriented 5 times the diameter and the average L/D ratio is about
fibers.
200. Thus, the average fiber length is about 5 micron
Conventional asbestos processing methods include and it is estimated that there are about I014 fibrils in
blasting, crushing and grinding, and air classifying. one gram of the high purity chrysotile asbestos.
Even with the use of the very best dry method of pro
By virtue of their small diameters and high aspect
cessing high purity chrysotile asbestos ore, fiber bun 10 ratio, the high purity chrysotile asbestos fibrils form
dles are still very much in evidence as shown in FIG. 1. colloidal suspensions when suspended in water and
The high purity chrysotile asbestos utilized in the pre behave according to the classical electrokinetic rules of
sent invention is preferably refined in accordance with hydrophobic colloids. That is, the fibrils develop a
a hydraulic beneficiation process to provide substan surface charge when suspended in aqueous solution as tially separated fibrils 10 as shown in FIG. 2. In the 15 the result of adsorption of potential determining ions
hydraulic beneficiation process, the ore is treated by from the suspending medium. The potential determin
wet grinding and screening to separate rock from as ing ions are mainly hydrogen, and therefore, the fibers
bestos fiber, flakes and clumps. The asbestos is then display a positive charge in the basic ph range. Thus,
subjected to wet mechanical and/or chemical treat ment to liberate the fiber, that is, to separate the fibers
20
the term "cationic" asbestos as employed herein is intended to denote asbestos or asbestos fibers which
into discrete fibers, and separate out occluded non exhibit a cationic charge when dispersed in water under
asbestos minerals to form standard grads product. High the ph conditions, usually about 4 to about 9.5, gener
purity product is obtained by further wet grinding and ally used in the paint industry. Electrostatic attraction,
centrifugal processing of the standard grade product. This process results in separated, individual or discrete
25
however, is just one of the factors that influence the effectiveness of the fibers in cofloccing pigment parti
fibers of high purity, high liberation and uniform parti cle size. Thus, this asbestos is different from any other asbestos product available. The physical properties of
cles. Collision and coagulation rate in suspension are determined by the collision radius which varies as the longest dimension of the particle while diffusion con
average Canadian, standard grade Calidria purity Calidria asbestos are provided in the table.
and high following
30
stant varies as the main particle dimension. The net result for the rod-like, high purity chrysotile asbestos particles is a very large effective collision radius and a large diffusion constant. Furthermore, the high surface
PHYSICAL PROPERTIES OF CHRYSOTILE
area of the high purity asbestos fibers, ranging from
ASBESTOS-continued
about 60 to 80 meters'/gram, in.combination with the
PROPERTY
AVERAGE CANADIAN
CALIDRIA PRODUCTS 35 cationic charge provides a very high cationic charge
STD HIGH density for attracting and firmly holding the pigment
GRADE
PURITY
particles.
Surface Area M*/GReflectance 4
Magnetite %
10-30 54-70
3-4
50-60 62-72
2.0
40-80 72-76
<o.so
The high purity chrysotile asbestos can be provided
in several forms, particularly useful in forming the pig 40 ment dispersion in accordance with the invention. The
final form of the fiber in the pigment dispersion is pref
erably a totally liberated, colloidal form. This is usually
Specific surface area is calculated from adsorption data achieved with the particular high purity, short fiber
using the BET (Brunauer, Emmet, Teller) method as chrysotile asbestos of interest which has an ultimate described in Brunauer, "The Adsorption of Gases and 45 fiber yield of at least 85%, e.g. 85-95%. Canadian
Vapors", Princeton University Press (1945).
chrysotile asbestos fibers, as represented by Canadian
Magnetite content is measured by a permeametric 6-D-20 (see Example IX) is only liberated to an extent
device patterned after ASTM standard method D- of about 25-40% ultimate fiber yield under the same
1118-57, which has been improved with respect to conditions.
sensitivity to measure a limit of detection of 0.005% 50 Ultimate fiber yield is determined by pulping 3 grams
magnetite.
asbestos in 250 ml of tap water at high speed in a Wa
Reflectance is measured on a sample prepared ac ring Blender for 3 minutes. The pulp is washed into a
cording to TAPPI (Technical Association of the Pulp beaker to a final volume of 300 ml. The pulp is dis
and Paper Industry) standard T-452-m-58 and is re persed, decanted, flocculated, dried and weighed. Per
ported as percent of ultimate reflectance based on 55 cent ultimate fiber yield is the supernate chrysotile
magnesium oxide as the standard of 100% reflectance. asbestos filler cake weight times 3 divided by the total
The significantly greater purity of the high purity weight of the two cakes times 100.
chrysotile asbestos essential in this invention is demon
The filter cake of liberated asbestos fibers in accor
strated by its improved reflectance of at least 72% and dance with this invention is a lightly compacted, essen
its low magnetite content of less than 0.8% magnetite. 60 tially non-agglomerated product which is readily redis
The wet processing procedure gives rise to high purity persible in water with conventional mixers to form an
asbestos fibers that are essentially grit-free and of high aqueous dispersion containing liberated fibers.
brightness. The reduced magnetite content of the pure
In the first step of making a high quality paint formu
flake product is also a measure of absence of gray ap lation in accordance with the invention, a dispersion of
pearance that has been characteristic of prior asbestos 65 pigments is prepared. The pigment dispersion can con
products. The reduced grayness and absence of black tain varying amounts of the pigmented asbestos usually
specks is essential in the preparation of premium qual ranging from 1 to 25%, preferably 5 to 10%, of the total
ity finished paints.
solids of the dispersion, depending on the water de
5 3,947,286 6
mand of the various components of the tystem, the fibrils 10 having particles of titania 12 electrostatically
properties desired for the final paint composition and attached along the length of the fibers to form a predis
properties desired for the final paint film. The unpig- persed product. In the pellet, and open fiber process,
mented high purity chrysotile asbestos fibers have a the ratios of materials are adjusted to form a product water demand of about 480% while the pigmented 5 containing from I to 90% titania. suitably about 35%
fibers have a lower water demand depending on the titania, though the asbestos is capable of holding up to
quantity and type of pigment.
9 times or more, e.g. 9 to 10 times, its own weight of
The demand for pigment in terms of cationic charge pigment. The coflocced slurry is dewatered, extruded
is preferably completely or totally satisfied by anionic into pellets and dried in a rotary dryer. The dried pel pigments. The high purity chrysotile asbestos fibers 10 lets can be milled to form an open fiber form of the
develop a total positive charge which must be com product.
pletely balanced by combining with a total negative
The paint formulator may predisperse the pellets or
charge which is furnished by the anionic pigment, re open fiber in water with a high shear mixer to form a
sulting in electrostatic bonding of anionic pigment liberated slurry of the partially titanated asbestos. The along the length of ite fibers. It has been found that in 15 remaining pigments are then added, continuing the order to completely satisfy the cationic charge on the high shear mixing to form the final pigment dispersion.
asbestos fibrils, it is necessary to employ a ratio of at least nine times anionic pigment to asbestos, by weight.
The separate dispersion in water with high shear mixing better assures complete liberation of the fibers, to form
Thus, in totally liberated or discrete form, the asbestos a paint having a fine grind. Alternately, the remaining
fibers or fibrils can cofloc or satisfy about 9 to 10 times 20 pigments in water can be added directly to the pellet or
the weight thereof with anionic pigment.
open fiber, and mixed with high shear to form the pig
The fibers may be totally pigmented with a primary ment dispersion. The dispersion of the high purity
hiding pigment having high efficiency and providing chrysotile asbestos is materially-aided by reducing the
opacity such as rutile titanium dioxide. Anatase tita ph of the sluny to the acid range, preferably from
nium dioxide may be used where chalking is desired. 25 about 4-5. An electrostatic condition in the slurry
Other anionic hiding pigments comprise zinc sulfide, under these conditions prevents the fibers from reag
zinc oxide, basic silicate of white lead, lithopane, iron glomerating.
oxide or antimony oxide. Any combination of these
In the filter cake process, (II), the dilute liberated
hiding pigments may be utilized. In another procedure in accordance with the invention to be discussed below,
30
asbestos slurry is dewatered in a vacuum frame press to form a filter cake containing 40-60% asbestos fiber
the fibers may be pigmented with a mixture of anionic which may be optionally dried with tumbling in a rotary
hiding pigments or a mixture of anionic hiding and drier to a homogeneous product having a solids content
extender pigments. Typical extender pigments and the of 80-90% asbestos. Again, the pigment dispersion can
amounts in present are
percent by weight in which they may be provided below. These extender pigments
35
be formed by adding th*e total pigments at one time to the dispersion of fibers, with blending or separately
may be combined as desired for a particular end result. predispersing the hiding pigment such as rutile titania
1. Calcium carbonate (whiting) 0 to 25%
before adding the remaining pigments and blending to
2. Hydrated aluminum silicate (clay) 0 to 25% 3. Magnesium silicate (talc) 0 to 8.5% 4. Silicon dioxide and calcium silicate (silicas) 0 to
4.5% 5. Potassium aluminum silicate (micas) 0 to 6.5% 6. Other pigments including barium sulfide, benton
ite. magnesium aluminum silicate and various or ganic and inorganic and crystalline pigments. The hiding pigment such as titanium dioxide, and the extender pigments such as clay and calcium carbonate, exhibit an anionic or negative charge when dispersed in
40 45
form the pigment dispersion. A series of experiments were run to determine the
critical percent fiber that could be provided in a re duced water content chrysotile asbestos filler cake that is readily dispersible with conventional mixers available to most paint processors, rather than the high shear and high horsepower mixers necessary to completely dis perse the pre-litanated pellets. Standard interior latex paints were prepared according to the formulation of Example 4 with each of these filter cakes. The results
water as result of attachment of hydroxyl groups to the are tabulated in the following table and FIG. 5.
pigment, and hence are termed "anionic" pigments 50
TABLE II
herein. Total pigment present in the paint composition of the
LATEX PAINT CONTAINING FILTER CAKE
Filter Cake
Ulei Paint of
invention can range from about 4 to about 65% by
Eeample 4
weight. Anionic hiding pigments are present in an amount generally of about 4 to 25% by weight, or 55
Albertos Weight
National Standard Grind No.
higher. The preferred hiding pigment due to its effi ciency in providing opacity is rutile titanium dioxide. Other hiding pigments noted above may be present to replace a part or all of the rutile titanium dioxide.
41
SS 7S 91 96
6 56 4.5
4.5 4
Referring now to FIG. 3, several processes for form 60
ing pigment dispersion containing coflocced pigmented
asbestos are illustrated. In the pellet or open fiber pro
Wrinkling was evident at about 91% solids level in
cess (I), a dilute liberated asbestos slurTy such as a the filter cake, and above, indicating incomplete fiber
slurry containing 2.5% asbestos is blended with an liberation and therefore the presence of available cati
anionic hiding pigment such as rutile titanium dioxide. 65 onic charge which causes coagulation of the anionic
Oppositely charged asbestos fibers and titania particles latex.
are attracted and bond to each other to form a co
Unexpectedly, the filter cake can be dewatered to a
flocced product as illustrated in FIG. 4 which shows the level as high as about 91% by weight of asbestos and
A;370b
3,947,286
8
still maintain an adequate grind of 4.5, corresponding reaction product with maleic anhydride, and polysac
to less than 2 mils, in the resulting latex paint, indicat* charides. The expression "K.U." refers to Krebs units,
ing fairly good liberation and noncompaction of the a measure of viscosity which is conventionally used in
fibers into bundles. It is however, preferable to main the paint industry, and is determined with the Krebs-
tain the asbestos content of the filter cake from about 5 Stormer viscometer, as described in the brochure of the
80 to 90% to provide finer finish paint films. The 80 to Arthur Thomas. Co., Philadelphia, Pa., "Directions for
90% asbestos filter cake product afTords substantial Use of Stormer Viscosimeter," published 1948.
absence of wrinkling as well as adequate grind of less
Surface active agents which function as surfactants
than 2 mils for the latex paint in which such filter cake and dispersants can be present in the range of about 0.1
is incorporated, and is otherwise a very desirable com 1 to 4% by weight of this composition. These ingredients
mercial form of asbestos since the water content wet the surfaces of the particles and stabilize the emul
thereof is sufficiently low to minimize shipping costs sion or colloidal system. Usually only anionic and non
and it is a form readily available for dispersion.
ionic compounds are utilized in latex paints and prefer
The dispersion containing the dispersed pigmented ably a mixture of these types of surfactants is utilized. asbestos is incorporated into a latex paint which is 5 Many diverse types of surfactants which are commonly
defined as a paint in which water is the principal dilu ent. The nonvolatile portion of the paint is between 30 and 80% while the pigment volume concentration
used in the formulation of latex paints are suitable for use in forming the pigmented asbestos latex paints in accordance with the invention.
(PVC):
20 Exemplary anionic surfactants are saponified fats,
pigment
pigment volume volume + vehicle
volume
*
too
sulfonated materials such as fatty acid esters, monovalent alcohol esters of fatty acids, fatty acid amides, fatty acid nitriles, fatty aldehydes, secondary alcohols, or
. . aromatic hydrocarbons. Other suitable anionic surfac-
is between about 15 and 80%. The paint may optionally 25 tants are alkali sulfonates of alcohols having 6 or more
also contain binders, solvents, thickeners, surfactants carbon atoms, aminopolycarboxylic acids and the con
and various other additives. Exemplary materials for densation products of fatty acid chlorides and amines.
each component with a suggested percentage basis
There are fewer non-ionic compounds commercially
based on the total weight of the paint are provided available. Exemplary non-ionic surfactants are sapo-
below. These ingredients are understood to be exem 30 nines and their derivatives, the condensation products
plary and are not intended to any way limit the inven of ethylene oxide with fatty acids and their derivatives
tion, it being understood that alternate materials can or with phenolic compounds having a side chain.
readily be substituted for those suggested.
Coalescing agents can be provided in an amount of 0
A general procedure for formulating paint composi to 4.5% as needed. Coalescing a&ents aid in film forma-
tions according to the invention is to first charge all 33 tion during the drying cycle. They are solvents for the
liquid ingredients including optional thickeners, and vehicle and eventually evaporate from the paint film.
optionally including a portion of the vehicle, especially Typical coalescing agents include plasticizers such as
in the case of modifier vehicles. The charge is thor oughly mixed and the solids namely, the anionic pig
dibutyl phthalate, glycols like hexylene glycol, glycolethers, and certain alcohols.
ment and cationic asbestos fibers, are then added under 40 Freeze-thaw stability is an important property for
high shear dispersion. In the case of anionically paints stored in cold climates. Glycols such as ethylene
charged vehicles, such as anionic resins, the presence glycol, diethylene glycol and propylene glycol are
of the cationically charged asbestos renders it neces added in an amount of 0 to 4.5% to insure freeze-thaw
sary for prepigtnentization of the asbestos to com stability.
pletely satisfy this cationic charge, before addition of 45 Latex emulsions, e.g. an anionic, nonionic or cationic
the anionic vehicle; otherwise, coagulation of the an latex, and various modifiers therefore, can be provided
ionic resin will occur as result of the combination of in an amount providing about 5 to 50%, preferably
anionic resin with unsatisfied cationic charge on the about 5 to 25%. by weight of resin solids in the paint
asbestos. Nonionic vehicles, e.g. nonionic resins, can composition. Latex emulsions can be comprised of
be added at any stage of the manufacture.
30 many polymer types, and commercially available emul
The diluent concentration is preferably maintained sions contain 30 to 70% by weight resin solids in the
between about 20 to 70%. While water is the primary form of nonvolatile polymer. The polymer generally
and predominant diluent in a latex paint system, sol employed according to the invention contains an ethyl-
vents for modifying resin vehicle may also be present. enically unsaturated polymerizable vinyl group. The
The percentage range also includes the water present in 55 polymer functions to bind the pigment particles to-
such vehicle portion.
gether and to bind the paint film to the substrate. Ge
Substantial thickening of the paint is provided by the neric types of suitable latex emulsions and polymers are
fairly high water demand of the asbestos. In some cases, listed below:
secondary thickeners need not be present. However, in
1. Polyvinyl acetate homopolymer latexes.
most cases, the viscosity of the paint can be adjusted to 60 2. Vinyl Acetate -- acrylic copolymer latexes. The
the desired range of 60 to 125 KU, preferably 80 to 105
acrylic portion includes but is not limited to ethyl
KU, by including 0 to about 4% of conventional thick
acrylate, isobutyl acrylate, methyl methacrylate,
eners such as water soluble cellulose derivatives, e.g.
N-butyl acrylate, methacrylic acid, N-methylol
cellulose ethers or esters, for example, hydroxyethyl
acrylamide, acrylonitrile, 2-ethylhexyl acrylate,
cellulose, methyl cellulose, and carboxymethyl cellu- 65 and acrylic acid. Furthermore, these copolymers
lose. Other types of materials can also function as
may contain itaconic acid, styrene, butadiene, eth
thickeners such as carboxylated polyacrylic acids, so
ylene, vinyl chloride, maleates, and fumarates.
dium alginate, bentonite clays, a polymethylvinyl ether
Specific examples of such polymers are the copoiy-
A ; 3706
3,947,286
10
mer of vinyl acetate and butyl acrylate, vinyl ace*
Any of the above latexes may be modified with or
tate and 2-ethylhexyI acrylate, vinyl acetate and ganic solvent based binders or oils which may be of the
dibutyl maleate.
drying or non-drying type. These modifiers in turn may
3. Acrylate Latexes -- The acrylate latexes may con be emulsified. Modifiers may comprise from 0 to 70%
tain any combination of acrylate and acrylic mono 3 of the vehicle solids in a given paint in which water is
mers noted above in vinyl acetate-acrylic latexes, the principle diluent. Suitable modifiers are the oils
except for vinyl acetate. Specific examples of such such as linseed oil, tung oil, safflower oil, tall oil rosins
polymers are the copolymer of ethyl acrylate, or tall oil esters. Resin modifiers comprise alkyd resins,
methyl methacrylate and methacrylic acid, and the epoxy resins, vinyl resins, acrylic resins, silicone resins,
copolymer of butyl acrylate, methyl methacrylate 10 phenolic resins, ester gums and cellulose resins.
and acrylic acid.
Various miscellaneous ingredients may be present in
4. Other latexes include polymers of styrene-butadi an amount of 0 to 4% by weight. Included in this cate
ene, styrene-acrylic, acrylonitrile-butadiene rub gory are defoamers which may or may not contain
ber. butadiene rubber, and ethylene-vinyl acetate, silicones and fungicides, of the mercuric and non-mervinylidene-chloride, and acrylate-vinyl chloride 15 curie types. Driers for the solvent based modifier such
polymers.
as cobalt, zinc or magnesium naphthenates or phthal-
It will be understood that the proportions of comono ates may also be provided when needed. Other various
mers in the above described copolymers can be varied materials may be incorporated for special purposes as
as desired and as well understood in the art, to obtain are well known in the art.
the desired properties. Thus, for example in the copoly 20 Generally the paint composition of the invention
mer of vinyl acetate and butyl acrylate the monomer includes, in addition to the dispersion of the pigmented
proportions can range from 90 to 75% vinyl acetate asbestos and latex, additional optional components,
monomer and 10 to 25% butyl acrylate monomer; and particularly thickener, surfactant, e.g. anionic surfac
in the copolymer of ethyl acrylate, methyl methacrylate tant, and coalescing agent. and methacrylic acid, the proportions of monomers can 25 A series of paint formulations were prepared by first
range from 40 to 70% ethyl acrylate, 20 to 35% methyl charging in order, water, thickener, surfactant, fungi
methacrylate and 0.5 to 3% methacrylic acid.
cide, freeze-thaw additive, coalescing agent, and about
one-half of the defoamer, and mixing for 5 minutes at
Latexes containing combinations of the above resins low speed. Thereafter, the TiO, was added and dis-
can also be employed, such as a combination of vinyl 30 persed until a desired dispersion was achieved. Mixing
acetate homopolymer and copolymer of vinyl acetate speed was increased. The remaining pigments, includ
and butyl acrylate.
ing calcium carbonate, clay and the high purity chryso-
The resins in the above latexes in the presence of tile asbestos fibers, were then added and mixed at high
anionic surfactants generally achieve an anionic speed to form a pigment-asbestos fiber dispersion. The
charge. This is due to the polymerzation of the mono- 35 latex and remainder of the defoamer were then added
mers to form the resins, in the presence of such surfac to the pigment-asbestos fiber dispersion at low speed.
tants carrying an anionic charge. Polymerzation can Agitation should be continuous and each ingredient
also be achieved in the presence of nonionic and cati dispersed before the next is added.
onic surfactants, in which case the resulting resins are
The chemical identification of each ingredient by
either nonionic or cationic in nature. However, be- *0 type, formula and function is provided wherever possi-
cause of the cationic charge of the chrysotile asbestos ble. The asbestos utilized in each case, except for Ex
fibers, the anionic latexes generally employed to the ample 9, was high purity, short fiber chrysotile asbestos
major extent in latex paints, must be added to the dis in the form of Calidria asbestos as either dispersed
persion of the chrysotile asbestos fibers after addition unpigmented filter cake or in pretitanated pellet form,
thereto of the anionic pigment in order to completely 43 as indicated. The ingredients utilized in the formula
satisfy the cationic charge of the fibers with the anionic tions are provided in the following table, and the exam
charge of the pigment, prior to addition of the anionic ples follow thereafter.
latex, to avoid coagulation, as noted above.
TABLE III
FUNCTION
MATERIAL
GENERIC TYPE
Solvent Thickener
Anionic Surfecunt
Do. Nonionic Surfecunt Freeze-Thaw Coalcscent
Defoamer Fungicide
Hiding Figment Extender Pigment Do. Do-Asbestos Do-Tiuneied Asbestos Do-Filler Cake Do*Tt*nated Filter Cake Solvent
Water Bentone LT
TAMOL 731
VICTAWET 3SB ADVAWET 33 Ethylene Glycol Butyl Cerbitol Aceute NOPCO NXZ CMP Acetate
Ti Pure R-960 ASP 170 Clay VICRON 25-11 CC 100 CC 135
CC 100 CC 135
Water
H.O Organically modified bentonite Sodium salt of diisobutylene maleic anhydride Sodium octyl phosphate Polyglycol ester
Monoether of dieihyicnc glycol 0.1* Si Chloromeihosy-Acetoxy mercuripropane TiO, Kaolin Clay Calcium Carbonate High Purity Chrysotile Do 35* TiO,
40 lo 50* solids 40 to 55* solids
H.O
707
FUNCTION Defoamers Latex Emulsion
Do. Do.
0.1 Modifier Eposy Modified Thickener
3,947,286 11
TABLE Ill-continued
MATERIAL
GENERIC TYPE
NOPCO NXZ NAT-1 (55*) UCAR-130 (51*1 UCAR 370 (46*)
PVO-44 ( 65*) Polytex 61! O Ccllosize QP-4400
Copolymer of Vinyl Acetate
and Butyl Acrylate (anionic) Vinyl Acetate homopolymer < nonionic) Acrylic Emulsion containing copolymer of ethyl acrylate methyl methacrylate. and methactylic acid (anionic 1 Bodied Safflower emulsion Epoxy ester emulsion A hydroxy ethyl cellulose
12
EXAMPLE 1
MATERIAL
Water Bentone LT TAMOL 731 -- 25* Active VICTAWET 3SB ADVAWET 33 Ethylene Glycol Butyl Carbitol Acetate NOPCO NXZ CMP Acetate Ti Pure R-960 ASP 170 Clay VICRON 25-11 Water NOPCO NXZ NAT-1 (55*)
TOTAL -
POUNDS
225 5.5 3 5.7 4 IS IS 2 0.5
242.5 100 144.7 151
2 217
1202.9
EXAMPLE IV
MATERIAL
Water Bentone LT 20 TAMOL 731 -- 25* Active V1CTAWET 35B ADVAWET 33 Ethylene Glycol Butyl Carbiiol Acetate NOPCO NXZ CMP Acetate 2S Ti Pure R-960 ASP 170 Clay VICRON 25-11 CG 100 Water NOPCO NXZ NAT-1 (55*1 30 TOTAL -
ROUNDS
3 IS 4.3 3 5.7
4 15 15
2 0.5 242 5
100 112
70
<5 2
217
(465*1
1263
EXAMPLE II
MATERIAL
Water Bentone LT TAMOL 731 -- 25* Active VICTAWET 35B ADVAWET 33 Ethylene Glycol Butyl Carbitol Acetate NOPCO NXZ CMP Aceute Ti Pure R-960 ASP 170 Clay VICRON 25-11 CG 135 Water NOPCO NXZ NAT-1 (55*)
TOTAL -
POUNDS
306 4.3 3 5.7 4 15 15 2 05
225 100 112 50 131.5
2 267
1263
EXAMPLE III
MATERIAL
Water Bentone LT TAMOL 731 -- 25* Active VICTAWET 35B ADVAWET 33 Ethylene Glycol Butyl Carbitol Aceute NOPCO NXZ CMP Acetate Ti Pure R-960 ASP 170 Clay VICRON 25-11 CG 135 Water NOPCO NXZ NAT-1 (55*)
TOTAL -
POUNDS
306 4.3 3 5.7 4 15 IS 2 0.5
225 100 112 98 (51*> 13.5
2 287
1263
EXAMPLE IVA
35 MATERIAL
Water TAMOL 731-25* Active VICTAWET 35B ADVAWET 33 Ethylene Glycol 40 Butyl Carbitol Acetate NOPCO NXZ CMP Acetate Ti Pure R-960 ASP 170 Clay VICRON 25-11 CG 100 45 Water NOPCO NXZ NAT-1 (55*)
TOTAL -
POUNDS
243 3 69 4.1 15 IS 2 0.5
242.5 100 93 7 107.4 (46.5*) 40
2 285
1160 8
50 EXAMPLE V
MATERIAL
Water
Bentone LT 55 TAMOL 731-25* Active
VICTAWET 35B ADVAWET 33 Ethylene Glycol Butyl Carbitol Acetate
NOPCO NXZ CMP Acetate 60 Ti Pure R-960 ASP 170 Clay VICRON 25-11 CG 100
Water
NOPCO NXZ NAT-1 (55*1 65 PVO-44 (65*)
TOTAL-
POUNDS
315 4.3 3 5.7 4 IS IS 2 0.5
242.5 100 112 70.(46.5*1 *5
2 216.(55*) 61.(65*1
1263
A;3703
13
EXAMPLE VI
MATERIAL
Water Bentonc LT TAMOL 731-25* Active VICTAWET JSB ADVAWET 33 Ethylene GWcol Butyl Carbitol Acetate NOPCO NXZ CMP Acetate Ti Pure R-960 ASP 170 Cla> VICRON 25-11 CC 100 Uliti NOPCO SXZ NAT-1 t55* 1 Poiytex 6IIO
TOTAL -
EXAMPLE VII
material
Water Bemone LT TAMOL 731-234 Active VICTAWET 35B ADVAWET 33 Ethylene Glycol Butyl Carbiiol Acetate NOPCO NXZ CMP Acetate Ti Pure R-960 ASP 170 Clay VICRON 25-11 CO 100 Water NOPCO NXZ UCAR-130 <584 |
TOTAL
EXAMPLE Vlll
MATERIAL
Water Bentone LT TAMOL 731-234 Active VICTAWET 3SB ADVAWET 33 Ethylene Glycol Butyl Carbitol Acetate NOPCO NXZ CMP Acetate Ti Pure R-960 ASP 170 Clay VICRON 23-11 CC 100 Water NOPCO NXZ Ammonium Hydroside UCAR 370 <464 I
TOTAL -
EXAMPLE IX
MATERIAL
Water Bentone LT TAMOL 731-23* Active VICTAWET 3SB ADVAWET 33 Ethylene Glycol Butyl Carbitol Acetate NOPCO NXZ CMP Acetate Ti Purr R-960 ASP 170 VICRON 25-11 Canadian Atbettoa 6-D-20
3,947,286
14
EXAMPLE IX-continued
POUNDS
MATERIAL
POUNDS
313 4.3 3 5.7 4 13 15 2 0.5
242.3 100 112 70 <46.5* I 90
2 216 (334)
66 <6041
1263
(Canadian No. 6 ahorta) Water NOPCO NXZ NAT-1
O
TOTAL -
326.0 9.0
215.0
1393.7
The properties and characteristics of the latex paints and dried films are listed in the following table.
TABLE
EXAMPLE
1 II III IV IVA
Viacoaity (XU) Reflectance PVC,<*> Contrast Ratio Solidt <*)
Yield (Gallons)
N.S Gttnd No
110
91 33.04
0 967 54 87
100 7
102-3 91 33.04
.973 32 43
101 4-5
96-7
91 33 04
0 978 5243 101 6
97-S 91 53.04
0.978 3245
I0S 5-6
66 SB 52 45
0983 36.3
96 5-6
POUNDS
315 4.3 3 5.7 4 15 15 2 05
242.5 100 112 70. <46.5*1 100
2 272. <3*41
1263
POUNDS
315 4.3 3 5.7 4 15 15 2 0.5
242.5 100 112 70 <46.5*1 29
2 2 343. <46*)
1265
POUNDS
225.0 4.3 3.0 12 7 9.0 13.0 ISO 2.0 0.S
242.5 100.0 112.2 32.5
EXAMPLE
Viacoaity (XU) Reflectance PVC <* 1 Contrast Ratio Solidt (*) Yield (Gallons) N.S Grind No.
V
103 90 33 04 0967 52 43 I0S 5-6
VI
107 90 3304 0 967 32 45 101 5-6
VII
112 91 53.04 0 9S9 5243 101 5-6
VIII
S2 90 53.04 0 978 32 43 108 5-6
IX
150 Bt 53.04 0.994 48.23 123.6 0
30 DISCUSSION
Example 1 is a typical interior latex paint formulation (53.0% PVC, 54.9% Solids) which provides a standard measure of reflectance (91) and opacity (contrast ratio 35 0.967) for a 242.5 pound level of rutile titanium diox ide. The pigments in this system require 1 SO pounds of water to be properly dispersed leaving 226 pounds of free water. Since the asbestos has a water sorption of about 480%, the quantity that can be added is a func40 tion of the difference in water demand between the asbestos and the pigment it is replacing as well as the free water available. The lowered amount of free water lowers the amount of thickener required and this im. proves the flow and leveling rheology of the paint. 45 Usually around 1-25%. preferably 7-20%, of total pig ments can be replaced with the high purity type chrysotile asbestos (HPTCA).
The water demand of the asbestos and therefore the level at which it could be incorporated into latex paints 50 could be modified by treating the product with agents, which induces hydrophobicity, such as fatty acids and their derivatives, silicones, silanes and various other materials.
A dry titanated asbestos (35% TiO,) in pellet form 55 was predispersed and then incorporated into the for
mulation of Example 2 at a 50 pound level, replacing 32.5 pounds of calcium carbonate and 17.5 pounds of the original charge of TiO, which is now contained on the titanated fibers. The reflectance remains at 91 and the contrast ratio was 0.973.
The asbestos has in effect predispersed the TiO, elec trostatically along the fibers, thereby increasing its opacity when incorporated into a coating. The high brightness is quite unexpected. Asbestos has a 72% 63 G.E. brightness and with replacement of a portion of a high brightness pigment this lower brightness material would be expected to substantially lower the reflec tance of the resulting paints. The maintena
A ; 3709
3,947,286
15 16
brightness is further indication that the asbestos fibers reflectance readings staled in this application are tested
are electrostatically coated with the high brightness over a white substrate. Therefore, paints with a lower
anionic pigments which hide the grayness of the fibers. reflectance will be grayer and have a higher contrast
There were several indications that the fibers were ratio although the opacity may actually decrease as is
not completely liberated. The grind reading decreased 5 the case in Example 4A.
from 7 to 4-5 indicating the presence of some fiber
The pigmented asbestos is compatible with diverse
bundles. The film was slightly grayer indicating some of types of latex systems as well as oil and epoxy modified
the fibers are not completely pigmented and the sur- emulsions as shown in Examples S to 8. In each case,
face wrinkled slightly indicating that cationic charge stable paints were prepared having acceptable applies-
was available to coagulate the latex. Both of these latter >0 tion and working properties.
effects could be due to compaction which prevents
Example ^ is an attempt to prepare a similar latex
pigment deposition to satisfy the cationic surface paint utilizing Canadian Grade No. 6-D-20 shorts as-
charge of the fibers.
bestos. It failed in every possible desired criteria. The
Example 3 is identical to Example 2, except titanated Canadian asbestos could not be dispersed and gave a
filter cake (51% solids) was substituted for the predis- 15 grind reading of 0 which is equivalent to a grind of no
persed pellet and the water adjusted for the filter cake less than 4 mils, whereas the paints of the invention
water component. The film had a reflectance of 91 and have grinds between 0.5 and 2.0 mils, equivalent to a
a contrast ratio of 0.978. The grind reading improved grind Number of 4 to 7. and preferably less than 2 mils
to 6 and no wrinkling was evident. Thus, the filter cake
The Canadian asbestos could not be liberated or
product is in a more available form, can be dispersed 20 pigmented since the film was very gray and the surface
with conventional equipment and provides a finer grind wrinkled indicating remaining available cationic
surface.
charge. The high viscosity is also indicative of available
In Example 4, the filter cake (untitanated 46.5% cationic charge. The water content was substantially
solids), and the titanium dioxide are added separately increased and the solids dropped to 48.3%, yet the
to the pigment dispersion. The reflectance is again 91 25 viscosity was still 150 K.U. A premium quality finish
and the contrast ratio is 0.978. This demonstrates that paint must have a viscosity between about 70 to 125
the asbestos fibers are in fact coflocculating with the preferably 80 to 115 K.U. The random length Canadian
anionic pigments during paint manufacture.
No. 6-D-20 asbestos fibers are incapable of complete
The fibers are coflocculating with more than the liberation and do not cofloc with anionic pigments to
titanium dioxide and the extender pigments are filling 50 form totally pigmented products in which the cationic
in the available spaces on the fibers. The pigment de- charge of the fibers is satisfied,
mand of the totally liberated fibers is about 900 to
The following are additional examples illustrating the
1000% by weight. In Example 4 A, the amount of filter invention.
EXAMPLE X
EXAMPLE XI
EXAMPLE Xll
Ingredients
9 Pans TiO, 1 Pan Asbestos
13 Pans TiO, 1 Pan Asbesto*
10 Pam TiO( 1 Pan Asbestos
Water
CELLOSIZE OP-4400
Tamol 731 Victawet 35-B Ad<tl 33 Nopco NXZ Ti Pure R-960 Asbestos CO 100 Filter Cake <44* solids) Ethylene Glycol Butyl Carbitot Acetate
UCAR-130
630 0.3 6.0 11.4 1.0 4.0
376.0
143.3 30.0
30.0 463.3
630 0.3 6.0 114 10 40
3760
154 0 30.0
300 463.8
630 05 60 II 4 80 40
316.0
131 0 30.0
30 0 460 7
Viscosity (KU) Reflectance P.V.C. (*) Contrast Ratio Total Solid* (*) Yield < Gallons) N.S. Grind No.
Physical Properties
63
93 43.04
0.9783 49.06 161
6
78
92.5 43.16
0.9730 48.94
162 6
74
93 4274
0 9783 49 20 160
6
cake was increased to 50 pounds. The resultant paint
Referring to Examples X. XI and XII the viscosity of
gave a grayish appearance when compared to the paint 60 65-78 for all of these compositions is within the usable
of Example 4. Only 342 pounds of the preferred an range. As to reflectance, however, it is noted that Ex
ionic pigments are available (680% ). Consequently, a amples X and Xll with ratios of pigment to asbestos of
portion of the asbestos fiber remained uncoated giving 9 to 1 and 10 to 1 respectively have the same high
a discolored film.
reflectance values of 93, whereas Example XI. with a
The reflectance decreased to 88 as compared to 91 65 ratio of 8.5 pigment to 1 part asbestos, and below the 9
for Example 4. The contrast ratio was 0.983. Contrast to 1 lower limit of the invention paint composition, has
ratio is defined as reflectance over a black substrate a lower reflectance of 92.5, and hence a lower bright
divided by the reflectance over a white substrate. The ness as compared to the paints of Examples X and Xll
A ; 37 ; C
3,947,286
17
Also, it is noted that Examples X and XII have a
18
3. A pigment dispersion according to claim 2 in
contrast ratio of 0.9785 whereas Example XI, having a which said anionic pigments comprise a mixture of
pigment to asbestos ratio of 8.5 to I, has a reduced hiding and extender pigments.
contrast ratio of 0.9730, indicating that opacity and
.4 A pigment dispersion according to claim 3 in
hiding power at a pigment to asbestos ratio of 9 to I or 5 which the hiding pigment comprises rutile titanium
greater, are at a maximum for a given quantity of hiding dioxide.
pigment to asbestos, and such contrast ratio remains at
5. A pigment dispersion according to claim 4 in'
such maximum with increase in the ratio of pigment to which the extender pigments are selected from the
asbestos above 9 to I, whereas such opacity and hiding group consisting of calcium carbonate, silica, clay, talc,
power undesirably decreases at a ratio of pigment to 10 mica and mixtures thereof.
asbestos below 9 to I.
6. A method of preparing a pigment dispersion com
In summary, the particular high purity chrysotile prising the steps of:
asbestos in accordance with the invention can be com
dispersing in water a predetermined quantity of short
pletely liberated and can in this form completely cofloc with at least 9 times its weight of anionic pigment, 15
fiber, high purity, chrysotile asbestos having a sur face area of about 60-80 meters'/gram, a reflec
usually 900 to 1000% by weight of anionic pigments.
tance of at least 72%. and a magnetite content of
The pigments are dispersed along the length of the
below 0.8%, by weight to form a colloidal slurry of
asbestos fibers and hide the relative grayness of the
cationically charged, liberated fibers;
fibers, increasing opacity. The opacity difference is quite dramatically displayed when 1.5 mil films are 20
adding anionic pigments to said slurry to electrostati cally cofloc said pigments along the length of said
observed on a hide chart.
fibers, the ratio of pigment to asbestos being at
The physical nature of the colloidal fibers with an
least 9:1 by weight; and
average L/D ratio of 200 provides reinforcement by the
blending said pigmented asbestos fibers to form a
whisker effect and improves the structural integrity of the paint film. The film has a high tensile strength and can experience large changes in substrate dimensions before the film cracks or fails. The durability, scrubbability and service life of the film are considerably en hanced.
Another desirable result is the degree of pigment dispersion attainable when the asbestos in filter cake form is incorporated into latex paints. The prior avail
25 30
uniform dispersion thereof. 7. A method according to claim 6 in which said pig ments comprise a mixture of hiding and extender pig ments. 8. A method according to claim 7 in which at least a portion of said hiding pigment is first combined with said fiber sluiry. 9. A high efficiency hiding pigment for coating com
able dry Canadian fibers were limited to a maximum dispersion or grind of 3.5 mils while the filter cake
positions comprising: high purity, uniform, short length chrysotile asbestos
yields a dispersion or grind of 1.2 mils. This is the first 35
fibers having a surface area of from about 60-80
material which allows the use of asbestos in premium
meters'/gram, a reflectance of at least 72%-, a mag
interior and exterior paints.
netite content below 0.8% by weight and an aver
It is to be understood that only preferred illustrative
age L/D ratio of about 200; and
embodiments of the invention have been disclosed and
said fibers being electrostatically combined with ru
that numerous substitutions, alterations and modifica 40 tile titanium dioxide pigment particles to form a
tions can readily be practiced by those skilled in the art
titanated asbestos product redispersible in water to
without departing from the spirit and scope of the in-
form liberated, separated, pigmented asbestos fi
ventiop as defined in the following claims.
bers, containing a ratio of at least 9 times said
We daintT'-
pigment to asbestos.
1. A pigment dispersion for a coating composition in 45 10. A pigment according to claim 9 in which said
which the pigment solids consist essentially of anionic titanated fibers are in the form of a pellet having a
pigmented,-liberated, colloidal, high purity chrysotile water content below about 2% by weight.
asbestos fibers having a surface area of about 60-80
11. A pigment according to claim 9 in which said
melers'/gram. a reflectance of at least 72% and a mag fibers are in the form of milled, dry, titanated fibers netite content of below 0.8%, an amount of anionic 50 having a water content below 2% by weight.
pigment being present sufficient to completely satisfy
12. A pigment dispersion accroding to claim 2, said
the cationic charge on said asbestos fibers.
high purity asbestos fibers having a surface area rang
2. A pigment dispersion according to claim I in ing from about 60-80 meters'/gram.
which the pigment solids are dispersed in water, the
13. A method according to claim 6, in which said
pigments being anionic pigments and the chrysotile 55 dispersion has a grind of less than 2 mils and wherein
asbestos fibers being cationic liberated asbestos fibers, the asbestos added to the slurry is in the form of a
the ratio of pigments to asbestos is at least 9:1 and in lightly compacted redispersible product containing less
which the grind of the dispersion is no more than 2.0 than 60% by weight of water.
mils.
60
65