Document OEr2RpzLd8OYMjGmz0pZ0jONX

E. I. DU PONT DE NEMOURS &. COMPANY KREBS PIGMENTS DEPARTMENT 256 VANDERPOOL STREET NEWARK, NEW JERSEY Serial No. Copy No. / ? -P/- "V r^ 'I Period Covered; NEWARK PLANT PIGMENT COLOR RESEARCH REPORT Final Beport . Miniature Panel Series 65* 67* 6$, 70* 72 nwmUP-.fttaiw* f X90 + swlwr 1W FILE: DATE, l mm ,,u i lists: N37940 Copy to* * I 12 - Extra Serial So* 139-44-61 Copy So* f 0J SEWAES. PLAHT PXGMIBT COLOR RESEARCH REPORT Pinal Report Titles Miniature Panel Series 65. 67, 69, 70, 72 SIMPEDEX Primers* t Period Covered* February 1943 - Sovember 1943. t APPROVED Bis DUP050149742 2 ISTROBOCTIOIH r The miniature panel series reported here ere concerned with the effect of wet grinding on flake pigments. The primary Interest la the effebt of degree of dispersion on the performance of flIMPEDEXw in metal primers, 'fhe effect o# ferric iron contamination in "B4PIDEX", and the performance of materiad. WHjufaotured from ammonium sulfate and ' iSiMiam:|to!^hate.,inie ragortad#: : v T" ; ' Tv' T !.;5 . '; :; : .. T'... in attempt was made to coat steel with a film of ammonium ferrous phosphate similar to the phosphatized steel coatings commonly used, -The results of moisture condensation exposure of tte'trsated steel specimens arereporbed* aaBcmiiQiifr 1 ':*ThQ' perforaaBce of well dispersed (severe paint grind) "IMPEDES" - -.-was-.superior to mix-in or light grinding, The- indication was: "Uiat the wetting accomplished by severe grinding was more ; effective than large flake -else in determining moisture impedance. The same trend was noted for Aratone and aluminum hut the effect was not as marked. 2 - hump "IMPEDES" returned approximately the same performance as did micropulverlsdd material, 3 - "HPED1X" manufactured from ammonium sulfate and sodium phosphate was equal to that manufactured from ammonium phosphate. Thus the source of ammonia sod phosphate would be dictated by economic considerations# 4 - The treatment of steel with "IMPEDES" holds no interest at this time since no improvement has been effected over the phosphoric acid dip. However, it should be noted that an ammonium fhosphate dip or a copperas dip followed by ammonium phosphate reataent showed some promise. SHMMARVt MPB #65 lafogjarag Btaiahata Hone of the "IMPEDE!" primers was better than the zinc yellow/ FegC^/Josp. control. The deleterious effect of high amounts of ferric iron was demonstrated. When the ferric iron content was over 1G$ the presence of "IMPEDE!" was detrimental to the performance of the primer. DUP050149743 3 ........SEX" manufactured from ammonium sulfate and sodium phosphate, substituted for pjiospfcate in' ` 1-0 was found to be equal to the material turn phosphate. w #67 - .^Xstuye condensation exposure patats demanatrst................. ground ground' material. Immersion panels of single pigment *IIP10X`! paints indicated that light grinding was preferable to severe grinding. #69 - .in.,a..F,alni..CAS!i) IS^EBEX*, Aratone and Huminum were compared in single pigment primers and in combination with zinc yellow/FeoCH, in which the flake pigments were subjected to several degrees or grinding as well as having been added as mix-in pigments. HI single pigment primers failed rapidly on moisture con densation exposure. The effect of dispersion on the performance of *J$f,lSgg was noted, in that the well ground pigment showed definitely better performance compared with the mix-in paint. Aratone and aluminum were inferior to BIMPIDBXH. The latter two showed no effect of the degree of dispersion. In combination with zinc ysllow/Fe23# the performance of ^IMPEDIX* primers was superior to Aratone primers and equal to the aluminum paints. Here again *HII>EC1XB was improved by the better dispersion as was aluxainum; degree of grinding had no effect on Araione. The flake pigment combinations with zinc yellow/Fe^O? showed no improvement over the zinc yellow/F203 control. mps #70 - i,igiMi!;,i,Txts^dLSls.eI An attempt was made by two methods to coat steel with ammonium ferrous phosphate crystals, to function similar to the phosphate films in common use: 1 - Crystallize ammonium ferrous phosphate crystals on a steel surface by successive immersions in reactant solutions. 2 - Apply a film of a.f.p. crystals to a steel surface by Immersion in an ^IMPEDE! dispersion (water or other volatile medium)* DU P050149744 4 In no case was steel treated In this manner superior to a phosphoric sold dip (no ammonia present). v. two procedures were equal to the phosphoric acid control e*g*. mwmlxin phosphate dip, or copperas dip followed by an ammonium phosphate dip. Only in these two instances of method 1 were crystals (believed to be a.f.p.) observed on the steel when viewed under the microscope. #72 - ,,,ia, m the same single pigment comparisons were made in this series as in M.P.S.-69 except that the paints were pigmented at 30$ by volume. In this case as in the 40$ P.V. primers the better moisture condensation performance was noted for the well ground *BU?EBEtB. Paint grinding also improved the aluminum and Aretone primers. lump and micropulverised BBU?IDEXB were compared in this series, ho difference was noted; this was similar to the comparison in K.P.S. 6?. The plan of the miniature panel series 65, 67, 69, 72 has been tabulated at the and of this report, dll paints were ground in a ball mill except as indicated. The flake pigment dispersion studies were prepared by mixing a suitably ground flake pigment mill base with the zinc yellow control primer. 1H x 3" clear steel panels were sanded and solvent wiped then primed, using the 8Pry Brush Technique* (0.2 mil dry film). The exposure was made in the roof condensation box; sun and weather during the daylight hours with positive motatdre condensation at night. The &.P.5. 70 was prepared as follows. Previously cleared 1* x 3* steel panels were treated. 1 - Phosphoric Acid dip followed by ammonium hydroxide dip. 2 - Hydrochloric acid dip followed by ammonium phosphate dip. 3 - Ammonium phosphate dip. 4 - Phosphoric acid dip. 5 - Phosphoric acid- dip followed by ammonium phosphate dip. 6 - Copperas dip followed by ammonium phosphate dip. 7 - *liPEB13t* dispersed in water (1039-3A) 8- * " * mineral spirit 9- * B" * /alhyd resin 10 - * * * acetone 11 - /elkyd resin. DUP050149745 5 exposure was in the poof condensation box* sun and weather during the daylight hours with positive noisture condensation at night* For further details refer to notebook 958 experiments 68 and 71} notebook 1039 experiments 10, 11, 15, * r DUP050149746 DUP050149747 * 1 It Liisi I* * > * eAHhHH)M o DUP050149748