Document OEB1YyYwvN5QGONKErE1azXgp
Environmental Health Pertpeetires VoL 9, tip. M-ft I97i
^Electron Microscopical Investigation of Asbestos fibers
Arthur M. Unger,* Anne D. Mackler,* and Fred D. Pooley t
Exuobi&ttea of Mbwtoa fibars by otoctMa akrotcoplcal teebalgw* subleo tbesbumr to wn( tb fiber Qfw by nrpbologin! ud ttnctml ftmubrioUwi
ChoyielleMbotaofilwrreBieiieofbMril>fabtflo.Kb--to<toeawnlHeeriibh pteyW emit. twfMdttai BUM oMsiat of a eaten] oayUlaiy 4efiaofi by ao i>wtw> Ooaaa tcyrtaflbte woU.ffHhlnerbNtbaoof oloetroaboaborbi-->, tbooaylUaiy wU Jaeraa--ota tbickmaa.dBfawaataadlaciiiayaiilalafiraaiMtortaeatraaahioatmrorlal Tbaebawf baton* tram oyanity b emUtrai to baa yaodaet of rtraeUnraUbmytiaa bn--kt about by bbybwytatiaa daa fa aiactea* raMaUea. Awoll raoagteted a-otto] dafeamtlaa.patten my ba wad
Anyblbala flban laud to bo atiraltfat, aplfa--y, aafi elaettaa-Mpapaa, allbomb oamd flban an oooaaiaaally ohaaraart. Diftnctten caotnat flfuraa are vMMa aa dark baada awbf pataUol and at right a--laa to the ar aafa. CmMaltte fbnaa tba ifcarteat aad (biaaaat flban, ftllawad la liaa by amaite aad aatkopkyUite. Sba dbtrtfwlloa cbwactexiatka of(ba amyUbato fiber typaa ara dlflanat.
Tbe tainted ana (tectra* dlifraettoa patters ter ctoyeotito ia uaiq--. Raflacdoaw raaga ia form from atraaked to unatt. BaOaetfca fcitemky aad ebape an tahtad to the decree ef apaaaaaa aftfct fiber bundle aad Che axteat ofpbyafaai decredatiaa ofthe fiber. Tbe anphtbote aabeatee fihen paaaaaa dkfractfo* pattens havf-- ahaliar ohanetoriattes yraUbiti-- !mdMtet Ideatifioatfoo. MJcroebanJaal aaalyide is r--abrad (hr kkatfficatkte ia such caaaa.
AdiaeeaeieaefthsMeetrialbjclaaatbreahoMlbwitTalanaraateBibibalaaibeateeWbara ia kmated. The dteoiwaiae la baaed ea tbafcr dttrl-- else dlatelbatioa ckanctarhtica.
g'Thc biological effects of asbestos in tbe lace Have been defined fl). In occupational , where indirect fiber exposure is com* in shipyards,, an over-increasing body of indicates that hazards exist, albeit to a degree than in direct occupational contact
The most intriguing; if not the moat imporasbestos problem deals with the families of workmen, populations living around inters of asbestos mining, milling, and
yfamnumtal Sekneai laboratory, Tha Mount Sinai of Medicint of tb City University of Hear York,
f York, 10029.
talent of Minora] Exploitation, University College i Wales and Monmootbshire. Cardiff, Wales.
manufacturing operations, and the use of asbestos products by the general population. Scientific inquiry is now focusing on how far into the general population the disease hazard is manifest (8). This latter question may be answered, in part, with proper epidemiological study. However, in such circumstances, the definition of fiber exposure is crucial.
The monitoring of working environments presents few problems in terms of defining the nature of the fiber used. That is, the working en vironment provides sufficient material for .analysis and latitude in the selection of analytical technique. Fiber characterization is readily achieved (iJ. In those areas removed from defined fiber exposure, the problem con nected with dust characterization may be enor-
1974 S3
1
mouA. Removed from the occupational setting, sublight microscopic fibers, often few in number, predominate. In these instances iden tification of single fibers may be required. It is the purpose of this paper to describe briefly some of the characteristics of sublight microscopic asbestos fibers which may be used for identification and characterisation of small numbers of or even single asbestos fibers.
Asbestof Mifltrait
The asbestos minerals are naturally occurring hydrated silicates which form fibers on com minution. Their commercial properties are many and have been described in detail (5). Asbestos fibers belong to two mineral groups both of which possess molecular configurations and structures predetermining the development of fiber morphology. Chrysotile, the serpentine rolled sheet silicate, forms cylindrical fibrils because of the structural mismatch between the component brucite and silica sheets (6).
The asbestos types amosite, anthophyllite, crocidolite, and tremolile belong to the amphibole mineral class in which cations link SUOidOHh groups to form an infinite chain which constitutes the fiber axis. The chemistry and structure of these mineral forms has been described elsewhere (7).
As a point of caution, mineral names 'themselves are misleading. Any one mineral species may vary in both chemical and physical properties. Therefore, the asbestos names cited in the literature may represent a wide range of materials (8). This paper will describe die morphology and selected area electron diffrac tion characteristics of selected asbestos fibers.
Experimental
Materials
The UICC standard reference asbestos minerals were used to provide specimens of anthophyllite, amosite, and crocidolite (9). Tremolite was obtained from the verxniculite pit mining operation at Libby, Montana {sample provided by W. Bank, U.S. Bureau of Mines, Denver, Colo.). Chrysotile samples from the Jef frey mine. Asbestos, Quebec, were obtained and used as the principal representative of this fiber
type {sample provided by 8. aped, Johns. Manviile Corp., Denver Research Centor, Denver, Colo.).
Preparation
The different amphibole asbestos minerals (0.1 mg) were placed in glass tubes and im mersed in distilled water (5.0 ml). This material was manually agitated for 30 sec. The suspen sions were further dispersed with ultrasonic ac tivity for 60 sec (Sonifier Cell Disrupter, Heat Systema-Ultrasonies Inc. Model W185D),
A I pi aliquot, withdrawn from the bottom of' each suspension was pipetted onto carboncoated Formvar grids and allowed to evaporate to dryness. The grids were carbon-coated again to form a Bandwich around the particles. Chrysotile asbestos was prepared from an opes,: triple air-jet milled sample in a similar manner, l The samples were examined by transmission-, electron microscopy with accelerating voltage set at 120 kV and 100 kV. Two instruments were used: Hitachi HU UE-125; and a JEOL JEM ; 120U. Scan magnification varied from 1504X to j 40.000X in each case. At least 60 areas on } several grids were inspected to assure.; homogeneity of sample preparation. Represen-.'S tative areas of each preparation were! photographed.
Usutts and Dfoamwn
Morphology of Amphibole Asbestos Fihsrs
Examination of amphibole asbestos fibertg demonstrates one morphological characteristic* that is common to all at low magnification. In-| dividual fibers tend to form straight, electron*! dense to opaque fibers. At magnifications lest* than 3000X, the population of each fiber tn*?1 displays remarkably different fiber lengths widths (Fig. 1). In addition to straight fiberit.}' curved fibers are occasionally observed (Fig. Crocidolite appears to form curved fibers morii often than the other amphibole asbestos typ*i?; In all cases, the thinnest fibers predominate *> the curved population. Amphibole fibers tendte| form morphologically straight edges parallel the fiber axis but irregular edges are observe^} as well (Fig. 3). These irregularities may related to both cleavage and fracture. Ends m:
64 Environmental Health Psrapectfrsf
xul, Johns^rch Center,
cstos minerals tubes and im ). This material sc. The suspenh ultrasonic acJisrupter, Heat W185D). m the hottom of I onto carbon.ed to evaporate on-coated again the particles. ;-d from an open, similar manner, by transmission lerating voltage instruments wen d a JEOL JEM >d from 1500X to
50 areas on :ted to assure ntion. Represen-
iration ware
-sbeatoe Fibers '3
e asbestos fibep*:| leal characteristic;! magnification, in-;! straight, eicctroa-;[i agniflcations le:i| of each fiber type;!;! t fiber lengths aM;:|| to straight fibeni$f y observed (Fig. curved fibers mom| ole asbestos type*|| ers predominate ip iboie fibers tend # ht edges parallel lip edges are observed1? egularitica may bej; d fracture. Ends f|
saltb Perapecti^;
65
*
-M
Picnw 2. Transmission electron micrographs of amphibole asbestos shoving prcnence of curved fibers (trrovf) in crocidolite, !8> amoaite, (O snthopbyllite. and (l>) rremolite. Bar marks equal l iim.
66 Environmental Health Pepectiv<$|
Morphological variation of ampbibole asbestos fibers at illustrated by (At amotite and (B) treindite, range from straightedge, right-angle fiber-axis terminations (amoaite) to irregular (cleavage and fracture led) edges and termination* (tremolite). Arrow >B) shows be planar view of (001) cleavage. Bar marks equal 1 ia.
3
fibers range from straight (right-angle termina tion across fiber axis) to irregular. Some irregular ends are controlled by cleavage planes parallel to the ab plane (Fig. SB). There appears to be no general relationship between amphibole fiber type and fiber edges and cleavage. However, amosite tends to present more rightangle truncations across the fiber axis, com pared to tremolite, which tends toward more prismatic forms. Anthophyllite tends to form electron translucent fibers whereas amosite tends to be more electron opaque. Thie latter feature is related to a number of factors in cluding composition, density and cleavage. Internal structures, such as fine lamellae parallel to fiber axes, are common in anthophyllite but may occur in other fibers as well. Some of these features have been reported previously (8,10).
Previous work concerning transmission elec tron microscopic examination of amphibole asbestos fibers indicated that a light and dark banding appeared to cross tho fiber axis at right angles (8). This banding is visible only on the electron translucent fibers. Some workers have called these bands decoration patterns in reference to similar diffraction contrast features observed on sheet silicates, especially talc (11). Diffraction contrast figures have been observed on all amphibole fiber types. They tendto form continuous, curved bands' across the fiber axis (Fig. 4). The nature of diffraction con trast figures in bright field imaging is well un derstood. Apparently, the energy absorption in the fiber is converted to heat which produces some distortion in the structure within the fibor. The result is a change in the electron dif fraction path (beam to crystal plane angle) producing changes in contrast Chrysolite, which has not been observed to flex in this manner, appears to dehydroxyiate rather than deform. This is common for hydrous minerals
(12). -
Size Distribution Characteristics of the Amphibole Fibers
The width distribution for each amphibole asbestos type was measured directly from photographic enlargements of EM plates with a resultant magnification of 700QX. Four to six plates, at the same magnification, were used to
obtain values for each fiber type. Numerical
data are given in Table 1. Measurements from
each photographic plate were obtained with a
millimeter rule which was adequate for diatinc.
tion of fiber widths to 0.1 jim. Interobserver error, previously determined in another study,
is small (13). The heaping phenomenon was negated by interval selection at the 0.1 divi
sion (13).
The size distribution of the amphibole
asbestos minerals forms a log-normal curve
strongly skewed toward the small size widths. -
The skewing is more marked for crocidolite and
amosite than for anthophyllite and tremolite, as previously reported Hi). Thus, more than 50%
of the crocidolite fibers are less than 0.16 urn in ,..
width, whereas only 40% of the amosite, 29% of. |
the tremolite, and 20% of the anthophyllite...... fibers fall below this size range. The next most iji
abundant size class for crocidolite and amosite :J
lies on tite smaller-size aide of their modal class: ^
whereas the next most abundant size class for/?!
anthophyllite and tremolite lies on the next;!
coarae-aize side of their modes. Polymodal size
distributions are common for these latter tWi|i| fibers suggesting that more complex cleavagii.v|
has produced more possible orientations, am|;|
concomitant viewing aspects. These variations??!
in croea-aectional aspects have been reported?!
previously (10). Width distribution trend*;;!
described here have been reported In the?
literature (11). The data presented herein reprd;|
sent smaller dimensional characteristics o'
amphibole fiber populations than has bee*;?;;;
previously described.
Amphibole fiber lengths were measured its;
the same way from selected photographs (actud??
magnification 4,000x). Tremolite fiber wiiiif
eliminated from this analysis because of it*?; close similarity to anibuphyilite with respect &|
length. Results are presented in Table 2.
'
The amphibole asbestos fibers display a rang*.??
of length distribution characteristics mod?!
remarkable than their width distribution;!
characteristics. Almost 98% of the crocidolite^:
fibers were measured at less than 5 teji
length; amosite 84% of the fibers were less lh*J(g
5 jam in length; anthophyllite, 51% of the fibed|.
were less than 5pm in len.-ir ?'early two-third*;?
of the crocidolite fibers length (Table 2).
' 1 m $
C4. Difi
... |*ftber *-u3
Bel to fig i vsriee.1
68
Environmental Health Perspective
4
numerical merits from
ined with a ? for diatincnterobaerver .other study, omenon was j 0.1 jam divl-
: amphibole . *;*ii lOrmal curve . I size widths, iocidolite and ... ; tremolite, as ore than 50% '.* an 0.16 in i:| nosite, 29% of anthophyllitaV';:] me next most;::| e and amoBit:;| dr modal cla**;;|| aixe class fot:-:!:^ . on the next;i$ 'olymodal siaij| .cse latter lW?5| nplex cleavagaill "ntations, sod-
e variations;.-| oeen reportedl;|| button trendiitij| ported in th<ij:| d herein repr^;:;| s-acteriatics ui^. .ban has beenj|j
. e measured tafi:| iOgraphs (actus|s| .lite fiber wa*|jj
because of . with respectW|j| ,, Table 2. :|| - display a ran^| cteristics th distribatid|| f the crocidol^l
: than 5 fitn rs were less thste| 01% of the fibe^l : surly two-thirok|;
a- i Ktn
tj:.
te,:
1
'
is; % i*. & m
i
Table 1. WWm4leCrlbWkaecfeMgMboka.lM.to.flbm.
Wo. of fibers <S of total)
Tot*l_
0.U- 0.21- 0.31- 0.41- 0.51- 0.81- 0.71- 0.81- 0.91-
MO, MED,
Fiber tyye .V* <0.1>un O.2*mO8*O.4)im0,5*niO.6Mra0.T/niO.8*imO.9|iM l.Qm >l,0Hm #mb
Crocidotite 552 146 224 90 39 19 16 5 5 126) (41) (15) (5) (5)
Aratolte
192 54 74 32 19 16 S 2 9 <1S) (38) (12) (10) (13)
AntbophyWte 261 16 62 10 33 21 31 14 16 (> (24) (15) (12) (9)
TrcmoUte 144 2S 38 29 9 12 7 12 9 (18) (23) 120) (6) (9)
*Ar.- total otinbcr of aiaeoramtsta far the population.
* WO: Modal alia determined by geometrical analjntia of hittograma. * MED: Mediae lit* determined from cumulativi frequency curvet
5 (8)
1 (9)
7 (33)
4 (24)
6 1 6 1
3 018 0.16 5 0.14 0.19 17 0.18 0.34 2 0.17 0.25
4 MB: Mean ebo calculated on the baaii of central claaa average: x * `Zfx/N. Valuae greater than 1.0 m were not indtufeil \ the austyaia. The calculated value far antbophyllita la therofare very atucb lew than real value.
Fiber type Crocidolite Amoalte Aocbopbygit*
Table 2. Leegth dlatribwMon of fleeted atapUbole aabaatoe Bberv. No. of fiber* n of total!
S Clara 1.1-28pin 2.1-00 pm
4,1-5.0
m 243
85' 30
u
;
(63) .
122)
(8)
(3)
(2)
202 46 57 44 14 8 (28) (28) (22) (7) (4)
212 29
43
28 '
17
(14) (20) (13) - (8)
12 (6)
mi >5.1 KM
10-11.8 l2i
33-1.4 (16)
83-5.) (89)
Morphology af Chryaotile Aabeatoe Fiber*
There have been numerous studies concerning the morphology of chryaotile' asbestos utilising the electron microecope. These ,, have been reviewed (IS). Most of these studies have centered on the appearance of the fiber bundle and to some extent the nature of the fibril unit The fibril has been described as possessing an internal capillary surrounded by an electron dense wall. Several of these references have shown figures of prepared ehrysotile which did not possess the characteristic morphological appearance. One such study showed a ball-
milled asbestos fiber which appeared to | none of the characteristic features (18). We 1 prepared and examined a number of ch samples: (a) air-jet milled sample, sonified 1 preparation; (b> air-jet milled, heated at 10 for 2 hr; (c) air-jet milled, heated at 460 hr, (d) air-jet milled, beaten in a Waring' dor for 30 min; (e) air-jet milled, beaten ballmill for 10 min. Each of these fibers' prepared in an identical manner for exan tion by electron microscopy. Chrysotilc : tend to consist of bundles of fibrils which i often curvilinear with splayed ends, features have been reported in the lit
70 Environmental Health Perse
USD,
HBle
0.18
0.19
OM
0.25
Mm*
o*!;
oat-1 Mr|
f). The individual unit fibrils which make up fiber bundles are normally composed of a al capillary surrounded by an electron
use wall. Fibril dimensions range in the iwing manner the central capillary, if pre ranges from 20 to 46 A ; capillary walls from 130 to 210 A; total fibril diameter 250 to 465 A (IT). Average fibril diameters from 300 to 360 A . Occasionally these
isions are exceeded, but not by more than a of two. Characteristic chryaotile fibrils
be seen in Figure 5/1. |fho central capillary of chrysotile fibrils may
within the same fibril, likely a function of in viewing aspect of noncyiindrical
Wanes as described by Yada (18). 0cmally, no central capillary is observed in jji fibril, again reflecting conditions of growth
tc tun. indiMied
MO,: i >5.1 fim pm :
33--5.1 139)
peared to possea| re# (iff). We b*t*| her of chrysotafe; pie, sonified fid* , heated at 100*6;' ted at 460*0 tori a Waring BIm* ilied, beaten in fi these fibers wof tner tor examinSS Chryaotile fibs*.; ' fibrils which W| tycd ends. Thif| : in the iiteratatfa
normal morphology which has been
ribed to chrysotile is rarely seen when ob-
such material under the electron proecope. For example, we have observed that
ala prepared by Waring Blendor prepara-
|| and ball milling, bear little resemblance,
" than overall fibril dimension, to the
rial in its natural state (Fig. SR.C). Also,
chrysotile is observed for prolonged
i of time it appears to undergo deforma-
| yielding an entirety new set of morpho-
' characteristics.
.
tile fibrils normally consist of a central
and electron opaque walls. As time of
pervation increases the following
photogical changes take place, in sequence:
pthe electron-dense wall decreases in width, iiii the outside of the fibril toward the internal
f, yielding an electron translucent layer;
||te the capillary wall width decreases with
the wall and capillary bend and become
(c) the central capillary may dfe-
- (apparently collapse) yielding a oon-
much-thinned, electron dense core en-
ated in an electron translucent material
i still possesses the outer fibril dimension,
es of this sequence are illustrated in 6. This identical deformational series,
ved with fibers prepared by heating at
and 450*0, is shown in Figures 7 and 8.
Hiddition to the alterations produced on un-
J I and heated chrysotile fibrils, size reduc-
tion by some vigorous mechanical methods further increases sensitivity to beam damage. For example, fiber bundle opening of chrysotile in a Waring Blendor produces irregular fibril edges (compare edges Fig. 5A, 5B). Magnesium is leached from the fiber during this process (A. M. Langer, unpublished data), which pro duces a weakened surface. These fibrils are readily damaged under the electron beam in ex tremely short time periods and display a highly deformed central capillary wail. The deforma tional sequence for chrysotiic is such that it may be used for identification purposes.
Selected Are* Electron Diffraction Characteristics of Amphibok Fibers
The electron beam interacts with atoms pre sent in the specimen resulting in different inten sities of the electron beam incident on the fluorescent viewing screen. The image of the scattered electrons is mainly related to diffrac tion effects and follows the Bragg geometry. Crystalline materials scatter electrons in regular patterns related to their crystal struc ture, atomic species present and their interplanar spacings. This image, in the back focal plane of the objective lens, may be focused on the viewing screen by defocusing the in termediate lens. The pattern obtained from an isolated particle is theoretically that of a single crystal. The reflection geometry obtained is similar to that of the Laue x-ray method (fixed crystal and film). This enables the microscopiat to measure directly the d spacing dimensions and their angular relationships (12).
One of us (FDP) has completed x-ray diffrac tion analyses of scores of amosite and croddolite samples from South Africa. These minerals are difficult to distinguish from each other on the basis of x-ray data. These fibers are very similar in structural aspect and therefore were expected to yield similar selected area diffraction patterns. Also, because of the multiple scatter ing phenomenon associated with electron in teraction in solids, small differences in reflec tion intensities disappear.
We have obtained selected area electron dif fraction patterns for each of the amphibole asbestos fibers. Two representative patterns are 3hown in Figure 9. The normal to the horizontal
;lth Perspectb*^
1974
71
m
:iS:
Fiona: 5. Morphology of chryuntil* asbestoe: (A) with no prior manipulation; t&t after heating in a Waring Blender for*;!
min: id ulcer ball millipg in a Spex Mill for 10 mb. Normal morphology a viewed under the electron microscope after treatment. Fiber bundle* are opened, reduced in length, and individual fibrils are highly sensitive to election beM|f
damage. Arrow in (B) shows electron translucent fibril with deformed and collapsed central capillary, u cnmp*|||
to normal fibril (arrow in (A)], flail milling tends to produce crushed fibrils [arrow in tCi\ Bar maria tVV.|
0.5 pm for all photos.
' ''
ft:.
Environmental Health Peripeoti^l
:
.. i
-t
?:
m .` : H.**
Ftr.inaJ7. -JK*4S=KS^^ 0.25 fim.
74
Environmental Health Perr
FtOl'RE 9. Characteristic selected area diffraction patterns obtained on (A). (Ci amosite and (B). (Dl crocldolitc. Fa LA; and (K were obtained on single fibers (single crystal pattern), whereas patterns (C'l and (Dl were obtained on a many fibers (polycrystalline pattern with bebye-Seherrer rings). The horizontal arrays (A. B) represent layer lines sSii. the fiber reciprocal * axis (5.3 A for each fiber type). The spacing repeat along these rows was measured:^ 18.1 A tor anionite and 1S.2 A tor croeidolit*. These represent b * axis spacing*. Their patterns are indistinguishable. Wjg polycrystalline arrays iC. Ih may be indexed a* x-ray powder patterns with the precaution that both intensities < ` occurrence of additional reflections may confound the analysts. All patterns obtained at 75 kV.
Environmental Health Persi
')) croeidoUte. F*
..obtained on at
,*nt layer
ow was : mdistinKoiihaU^S tt both inteaiti**`<5
lines represents the spacing along the c*
gjjjlof the reciprocal lattice. The c-axia dimen-
|jj. measured for both Fiber types yielded a
of 5.3 A . The spacings along the layer
^ indicate a repeat on the order of 18.1 A for
it* and 18.2 A for crocidolite. These
are indistinguishable and represent a
be plane projection for amphiboles.
jning diffraction patterns for accurate
_ measurements is very difficult Clear
crystal patterns are very rare, in that the
Ions tend to be multiple (double diffrac-
iitod occasionally streaked. Quite often
appear that occur at fractional dia-
B rather than in any periodicity
tic for the amphibole space group,
features may indicate translation of
y elements within the structure,
twinning. Further complicating the
diffraction picture, many fibers are too
i-'to permit the transmission of electrons
^Others are too thin to yield sufficient
in reinforcement. More important, for*
freflections tend to occur in selected area
diffraction. That is, the amosite and
to c*-layer lines should repeat 6-plane
. only at 020, 040, 060, etc. However,
|ire reflections present also at 010, 090,
... For the space group
(symmetry
jKfbr amosite and crocidolite) only k + k Inflections should occur. However, both
'to and h+k odd occur. There are also
of reflections which occur with un
great intensities. Those bright spots are
It about by a multiple elastic scattering of
beam (12). Also, the problem of par-
Hieatation gives rise to multiple patterns
.. mineral species.
Ilptedinique of selected area electron difcannot be used to uniquely distinguish
^single amphibole fibers. The diffraction
.. produces an array of spot reflections jlJuay be called amphibolejmly. 'flic fiber
loditity, along c*, may be cahftilated
i from the plate utilizing the instrument
constant Once the c* direction is es>
the reflection array along the layer
Ptiiay be measured as well. Still, even in the
|:%ases, results are equivocal, and
lemical characterization is required for
[identification.
Occasionally, where many fibers are in a single field a largo selected area aperture may be Inserted, and a polycrystalline pattern, similar in many respects to toe Debye-Scherrer powder pattern, may be obtained. This has been accomplished for amosite and crocidolite (Fig. 9). Utilizing the camera constant of the instru ment these rings may be measured and assigned a d spacing from within the structure. Their in terpretation is again hampered by the fact that the intensities are not the same as observed for x-ray powder patterns. Although chances of identification of fibers are best in this latter case, the occurrence of so many small fibers in an area suitable for diffraction is slim.
Selected Area Electro* Diffraction Charac teristics of Chrysotile Fibers
Chrysotile asbestos yields a unique selected area electron diffraction pattern (Fig. 10). Layer lines which denote the periodicity of the fiber axis n yield measurements of 5.3 A. Reflections on these lines tend to streak parallel to the layer line which has been interpreted in x-ray diffrac tion studies as progressive c-axis fanning and displacement brought about by the warping of the sheet structure (19). As the fiber bundles are opened, the reflections spots tend to be arcuate. These may be compared with mosaic disorienta tion in powder preparations in which DebyeScherrer rings are formed. These features are relatively well defined and have been cited in the literature previously (3, 17, 20). As chrysotile asbistos is progressively deformed by electron bombardment, its characteristic elec tron diffraction pattern changes. After 3 min a selected area diffraction pattern is observed which is markedly different from its initial character (Fig. 10).
Discussion
Identical comminution treatment of large UICC amphibole asbestos fibers produces marked differences in their size distribution characteristics. Crocidolite has a size distribu tion with a significant proportion of the fibers less than 1 pm in length and almost all of the fibers less than 5 pm in length. Also, over 90% of the fibers are less than 0.5 pm in width. Amosite fibers are longer and wider on the average.
eaith Persi
1974
77
Figure 10. Characteristic selected arc* electron diffraction patterns obtain*! on chryoneiie fibers. Pattern fA) rep a pattern obtained on a fiber with well ordered fibrils. The reflections in (A) are streaked only parallel to the layer !ia axis! related only to reflection* obtained from the Dormal cylindrical structure. The paturn nn 'B' i$ made up of arcs f-TM, than streaked spots, indicating fUiril dworientarion (characteristic of Debye-Scherrer r;ngi. This pattern is cosmsbjg:| obtained on fibers which have undergone physical manipulation during separation. Pattrras .r> >', and fOi represent ajgl fibers sfter tC) .10 sec and Hi) 180 sec under the electron beam. The visible pattern become* generally lest intense, high-order reflections being the first to disappear.
78 Environmental Health Pars]
Patter* (At rop vsl to the layer l
mad* upof arcs* patten to cos
-n4 (Dj represent
.,iHy ]eiw intense. <
jthophyllite fibers tend to be the longest sod value for alt fibers is based on limited data.
it of the amphibole types. All other Although the absolute carcinogenicity of the
photogicd and structural characteristics, ' various asbestos fibers is unknown, the present
selected area electron diffraction patterns, emphasis on crocidolite appears premature. For
to overlap.
. example, exposure to 5 fibers/ml level results in
i implications of these observations are im- a range of mass exposures which may vary
atr For' example, for a given industrial almost a magnitude for the different amphibole
of milling or mining, each fiber type types. The reduction of the crocidolite exposure
Id yield a physically different dust, in Great Britain to 0.1 fibers/ml corresponds to
phyllite would yield 39 countable fibers an equivalent moss exposure for.anthophyllite
|the NIOSH standards (a very dirty environ of 2.0 fibers/ml (based on a computation of an
, in violation of the law), whereas the same average particle size in which the decrease in
of erocjdolite would yield only two count* large fibers is carried throughout the entire size
pfiberafwell within the `W*". limits) (22). In range equally). The present disease patterns
of industrial hygiene, if a given may result from the doses associated with each
apbjrlUte process yields 39 fibers greater liber type. This must be carefully studied.
j 6 fita in length, measures taken to reduce Within each of the amphibole asbestos types
jjjjjte'to the 5 fibers/m! level would significant* there may be a range of size distributions
Indues the total mass of dust. No such dust related to a particular mine or a particular
tion would occur in the crocidolite environ- horizon within a mine which is being worked for
fi-The mass of respirable duat for each of the ore. Cleavage parallel lo the fiber axis is con
liiaccupational circumstances would be vast- trolled by cation forces which occupy the M* and
Tarent.
Mi sites of the crystal lattice. These cation sites
)haa been suggested that the greater disease occur at the margins of adjacent opposite facing
in crocidolite miners and millers in chains and provide the attractive forces which
tiweatern Cape Province, as compared to bind the chains together. A wide variety of ca
svaal, is related to the fineness of the tion species may be substituted within these
'). Hence, the concept of masB, surface sites which could change the cleavage properties
particle size, and dose response is indirect- of the mineral. It is important, therefore, that
plicated in its biological importance. Also the various asbestos mines and mills which pro
<t.of the small fiber--fleeter hinfogtoal duce and use amphibole fibers be thoroughly
"Saory is the observation that the studied to determine the influence of chemistry
fibers tend to accumulate in tfie on the physical comminution of fibers. These
iial tree, whereas the smallest nDcrs~ factors may reflect the relative dust hazard.
alveolar sacs and become lodged m
JWalternativc "long" asbestos fiber theory lining to carcinogenic effects) would
most disease in workmen exposed to hyllito dust, followed by amosite dust, |ftrocidolite dust Also longer, thicker fibers ' the Transvaal crocidolite fields should I'more disease stigma than that from the
stem Cape. The oppositeris true, $pd no it to support this theory. If indeed the rs were the most important biologicalsince fewer long fibers exist in an
1 *
Whereas the ,amphibole asbestos minerals tend to deform mechanically when bombarded
with a 100 keV electron beam, chrysotile fibers are altered markedly through dehydroxylation.
With a normal beam current on the order of tens of microamperes, the energy absorption from the incident electron beam may produce signifi cant changes in the substance. Irreversible changes take place, including the production of crystal defects, atomic displacement, bond rear rangement, and all- accompanying manifesta tions of heating. Under almost all conditions, chrysotile asbestos possesses sufficient thick
4ite population, the carcinogenkity of the ness, collision cross section, and stopping power,
iual "long" crocidolite fiber would be to produce significant effects. Such isolated fi
. magnitudes greater than for any other bers may achieve the activation temperatures
Itype.
'
required for dehydroxvlation in short periods of
fe designation of the same threshold limit time. This is well documented (12, 22). In addi-
;alth Penrap
1974
79
tion to the thermal changes obeerved in more normally prepared apedmene, prior treatment of the aabestoa fiber leaves it even more suscep tible to electron beam damage. This sequela is known and may be used for identification pur poses. The selected area electron diffraction pat tern of chryiotllu is feiatiyeiy unique. If tl*e fiber is sufficiently thick, and has not suffered extreme electron beam damage, the selected area diffraction may be used for fiber identifica tion. More detailed characterisation of the se lected area diffraction patterns of amphibole fibers need* to be done. By UBing a goniometer stage and well known arid characterised fiber
samples, it may be possible to distinguish among the amphibole asbestos types.
Although not included la this study, obser
vations-have-been made that the Coalinm-type
chrytotiles tend to produce more fibril-sized
piPttcleg, is compared with Canadian fibers,
When reduced' under identical conditions. The
relative proportion nf rennirabte dust is thercEy
significantly grwafo-. This may be comparable
to the crocidolite fibers where disease associa
tion is most marked in areas where finer dusts
are generated. An investigation into this aspect
is warranted.
,
nCKIIOWitaffnWn
The authors (AML, ADM) wish to acknowledge support under as NIEHS Center Grant, ES 00928. One of us (AML) wishes to acknowledge support under an NIEHS Career Scientist Award, ES 44812.
UR81NCES
1. iiofovski, P,, Qihon, J. C., Timbrelt, V. ud Wagner, J. (!-., Eds., Proreedinjp of the Conference on Biological Effects of Atbentoe, Int. Assn. Re*. Can. Scientific
Pub. No. 8, Lyon, 972WHO (1973). 2. Harries, P. Q. Asbestos bixards In naval ihlpyards.
Ana..Oceup. Hyg. 11:13S (1068). 3. SeKkoff, L JH and Hammond. E. C. Environmental
cancer'in the year 8000. 7th Natl. Dancer Conf.
Proe., Araer. Cancer Soc. 1978, p. 68Tr
--
4. Ekrenrefch, T., ct al. Le* fibres '<famiante dani
. lea pennons hsmaiat: lour signification medico-
legala dan* lea- maladies de Peavironment. Arch.
SlaUd, Prof. Med. Travail M: 189 (19731.
5. Spell, S., and Lemowcber, J. P. Asbestos miosrali
in modem technology. Eavirrm. Km. 2:168(1969).
8. Whittaker, E. J. W,, and Zuseraan, J. The dbara.
terizatioa of serpentine minerals by x-ray diffraction
Mia. Hag. 81; ,107 (19661
'
7. Ernst, W. G. Amphibole*. In: Crystal Chemistry,
Phase Relations and Occurrence. Springer-Vert**'
New York; 1968.
^
8. Laager, A. M., and Paoley, F. D. Identlffcatim of.
single asbeitna fibers in human tissues. In; ProeeedJag*'
of the International Conference on Biological
:..
of Asbestos. P. Bogovaki, et at., Eds., (ARC. ivon vl
1974, p. 119.
'
9. Timbrel!. V. Characteristic* of the VICG standard:
reference samples of asbestos. In: Proceedings'::::
of the International Pneotnoconiosis Conferrem^l;
Johannesburg. H. Shapiro, Ed. Oxford I.'niv, Pre%i'!'
London, 1970.
10. Poaley, F. JD. AsbeatM bodies, their formation,:-;?
composition and charaecar. Environ. Res. S: Ml-::':
(1972).
!;|
11. Hendstwm, W., et aL Talc sad carcinoma o( the ovaiyi:?; and cervix. J. Oh*tot. Gynecol. Brit. 78: 266 (1971). li:|:
12. McConnell, J. D. C. Electron microscopy and eieetwsjxlj diffraction. In: Physical Method* in Determinativei;!
Mineralogy. J. Zunsman, Ed. Acadcmle Press, Nt*::
Yack, 1967.
.!;$
13. Longer, A. M., and Madder, A. D. Distribution ^ii:|
sabostos In fibers in tbe lung of an asbestos workan.::::|
la preparation. 14. Timbrel!, V.! et al. Characteristics of respirahfci|
asbestos fibres. Im Proceedings of the InternstioAih^j|
Pneumoconiosis Coaferesce, Johannesburg, H. 8baii:| pire, Ed., Oxford Uni?. Press, London, 1970, p. lagf
15. Madder, A. D. Morphological characteristic* <i!
chryaotile asbestos. M. 3. (hosts, New York Univoiftja
*ity, 1972.
-g
16. Huggins, C. S. Electron micrographs of some untaad:
inorganic fiber*. UA. Bur. Miass. Rept, lovesdjjili::
6020 (1962).
jgf
17. Poaley, F. D: 'Electron microscopic characteristics <i
inhaled ehrynotile ssbeetos fiber,' Brit J. Ind.
29: 148 (1972).
: ||
18. Yads, K. Study of chryaotile asbestos by a lrij!| resolution electron microscope. Acta Crytt. 22: mil
mam
J
19. Znssmsn, J., et al. Electron diffraction studies :$i
20.
serpentine minerals. Amor, Mineral. Zvyagin, B. B. Electron Diffraction
4A2n: a1ly38si(s1o95ff7<o)/|:||'|^
Minerals Structure* (translated by 3- Lyaei, Plertiti
Press, New York, 1967.
'.
21. Standard far exposure to asbestos dart. Title
Labor. Chap. XVII. Occup. Safety and Health Attajs;|"
U.S. Dopt. Labor. Federal Register 3Tr June 7,1972;:;^
22. Keindertreich, R. D. Fundamentals of Transmadii|S|
Electron Microscopy, Wiley, New York, 1964.
Iv;
rei
lely iofog iraa|
80
Environmental Health Perspo
4
I
ENVIRONMENTAL HEALTH PERSPECTIVES
David P. Rali, Director, National Inatitut* ofEnvironmental Health Sciaacee
'Gary E. R. Hook 'George W. Luder Robert L. Dixon HanaL. Falk Lawrence Fiehbein
'co-nanaginf diion
BOARD OF EDITORS
Robert Goyer David Hoei Larry Hart Heinrich Malting John A. Moon
!. EDITORIAL STAFF
|)
Ruth Krigman, Copy Editor
M. Kenneth Miller, Typographical
!|
Martha Dockary, Editorial Aerirtant
Consultant
J. Earl Linthicum, Art
Elizabeth Jamee, Information
Specialist
it
ENVIRONMENTAL HEALTH PERSPECTIVES
Murne 9, December 1974
a& DEPARTMENT OF HCM.TH, EOUCATtOM HHO WELFARE f*M* HmM Santo*
*ft<O-uT-j-N--v nnw o-*r nMM