MENZEL SYMPOSIUM ON
HIGH PRESSURE STEAM CURING
Compiled under the sponsorship of ACI Committee 516, High Pressure Steam Curing, and .the Autoclave Division Committee, National Concrete Masonry Association, the 10 papers in this volume are the proceedings of a symposium held at the 65th ACI Annual Convention, Chicago, April 1969. Ed'ted by W. H. Kuenning.
PUBLICATION SP-32
v
CTD000969
fr
* j
:ed in ; . io the ; s-iow.
;*US;i in ; .-is \ i
j '* 4
t <a
3t *- 1 !
* ts
-V
6 i t (
Ii
PREFACE
Commercial high pressure steam curing (autoclaving) of concrete block in significant volume began about 1944. about 10 years after Carl Menzel developed the comprehensive background of technical information that gave this portion of the autoclaved products industry its first real impetus. Other portions of the industry have also drawn heavily on the results of Menzel's work.
| Building products had been autoclaved as early as 1868 in Milwaukee by James Rowland. In Germany Michaelis initiated autoclaving as a method
' of testing of mortars in 1880. Interest in the autoclave process revived | briefly in the United States in 1911 with the publication of a paper by Wig. | In the 1920's and 1930's D. G. Miller published papers on high pressure steam
curing, and Thorvaldson and various Canadian coworkers wrote of their ini vestigations of several aspects of the subject during the same period. | Woodworth reported on the properties of block made in an early autoclave
plant in 1930, and Pearson and Brickett published the results of laboratory studies in 1932. These were the major autoclave forerunners of Carl Menzel.
High pressure steam curing is now applied to the manufacture of a number of products, each with their own special requirements. The most ; significant benefits that autoclaving contributes to the several major groups 1 are:
Concrete block and brick - early strength, and reduction of drying shrinkage
i Sand-lime brick - achievement of strength within a practical manu ti facturing period, and reduction of drying shrinkage I 1
Asbestos-cement products - sulfate resistance, and early strength
l j Cellular concrete - high strength-to-weight ratio, and reduction of iJ drying shrinkage ii Hydrous calcium silicate heat insulation products - high strength-
to-weight ratio.
t Only the first, third, and fourth of these are specifically discussed in papers contributed to this volume.
We are fortunate to have three Russian papers included in this volume, on diverse subjects. In Russian practice high pressure steam curing has made it possible to utilize materials that become effective binders only at auto clave temperatures. The Russian literature therefore deals with a wider va riety of raw materials than those used in the United States and Canada.
iii
CTD000970
PAPER SP 32-6
AUTOCLAVED ASBESTOS-CEMENT PRODUCTS
By JULIE C. YANG
Curing of asbestos-cement products by high-pressure autoclave, including saturated steam and superheated steam conditions is dis cussed and compared.
The binder produced under the various conditions were character ized by x-ray diffraction, DTA, microscopic point-count estimation of composition, pore spectra, uncombined Ca(OH>2 analysis, density, and strength determinations. The desired high-strength binder was essenti ally tobermorite and some CSHn geL Al-substituted tobermorite and CSHII) may be present in small amounts, but C2SH, AI2O3, Fe203, and SC>3-bearing hydrous phases were not detected.
Superheated steam conditions should be avoided at all time, and saturated steam autoclaving can be carried out usually at pressures around 100-110 psig (7.0 - 7.7 kgf/cm2) for times of about 16 hr Curing in saturated steam, utilizing a water spray technique, is recom mended because it permits the desired binders to be formed over a broad pressure range and also reduces significantly the autoclaving time.
An optimum autoclaving cycle is recommended that uses stepwise curing at two pressure levels in the presence of water spray: 5.5 hr at 115 psig (8.1 kgf/cm2) followed by a 3.0 hr at about 130 psig (9.1 kgf/cm^).
Keywords: asbestos-cement products; autoclaving; binders (materials); calcium silicate hydrates; chemical analysis; compressive strength; curing; differential thermal analysis; flexural strength; manufacturing; micro scopy; pipes (tubes); porosity; presteaming period; research; superheated steam; supersaturation; tobermorite; xonotlite; x-ray diffraction.
Autoclaved asbestos-cement products were introduced commercially in 1935. ^ adoption of autoclaving was the culmination of a search for a curing method
would effect rapid strength development and provide a binder with good -Ymical stability and required physical properties.
As the demand for various autoclaved asbestos-cement products grows, capayof the existing autoclaves, or the cost of installing new pressure vassels is '"ally the factor limiting increased rate of production. A significant improve~-cnt in production efficiency as well as reduction in cost will be achieved if Y autoclaving cycle is shortened, while the quality of the product is maintained.
In this study, the effects on the binder properties and product strength of nations of autoclaving conditions to reduce the. curing time are discussed.
117
CTD000971
t'ri'mm it it
TVMrtMMTi.ii T, in t YrPn**--
--
118 HIGH PRESSURE STEAM CUR|>,
ACI Member JULIE C. YANG has been associated with the Johns-
Manville Reasearch and Engineering Center, Manville, New Jersey I
since 1955 where she has been a research chemist, a senior research |
chemist, and a research associate. Her work has been concerned i
primarily with studies of the properties of inorganic silicates, asbes- !
tos-cement products, cements, and high-pressure synthesis of vari- i
ous systems containing silica.
j
1 i i *
\
Dr. Yang is a member of the American Chemical Society, the
<
American Ceramic Society, the American and British Mineralogi
es! Societies, Sigma Xi (Science), lota Sigma Pi (Chemistry), and
Pi Mu Epsilon (Mathematics). As a member of the American
Concrete Institute she currently serves on Committee 516, High
Pressure Steam Curing.
i
{
MANUFACTURING PROCESS
Asbestos-cement products can be formed by several processes, the choice of
which depends on the material being produced. Most large products such as
pipe, corrugated, and flat sheets are made by a wet process that is similar to
papermaking. A thin slurry containing about 10 percent thoroughly mixed
solids and 90 percent water is spread into thin layers and filtered on a screen
under vacuum, laminated, and compacted under pressure on a form until the
desired thickness is built up. Flat sheets are stripped immediately after form-
ation, cut, pressed, and stacked for a presteaming period,* whereas pipes are
left on the mandrel for 30 to 45 min prior to stripping.
_
More recently, the extrusion technique has been adapted to produce de sired shapes and intricate designs. In the extrusion technique a small amouiu of "hvdromodifier" is used, a material that regulates the amount of water and the consistency of the asbestos-cement mixture without the dewatering oper ation that is necessary in the filtration process.
j ; ! t
4
:
Materials
A typical formulation for autoclaved asbestos-cement products contains cemcr asbestos fiber, and finely divided silica. For example, autoclaved asbestos-cenirn; pipe contains about 20 percent clirysotile asbestos fiber, 30 to 35 percent of
* The term "presteaming period," defined in "Cement and Concrete Tern;ology, "ACI Publication SP-19, as" . . . the time between molding of a concrete product an ! shs-t of the temperature rise period," is used here in place of the term "precure", used m the asbestos-cement industry.
CTD000972
--SSURE STEAM CURlsc
nSBESTOS-CEMENT products
119
--sd with the Johnsrrville, New Jersey ^_st, a senior research s been concerned rranic silicates, asbesj synthesis of van
neal Society, the .rritish Mineralogi-
Chemistry), and -xhe American -=rittee 516, High
pound quartz flour with a Blaine surface area of about 2600 sq cm/g, and 45 u 50 percent of portland cement. The fine silica flour does not function as n aggregate, as in concrete, but ns a chemically reactive silica that will react ith the hydrolytic lime (formed during hydration of the cement) to provide jJditional binder material.
It is helpful to look upon the asbestos-cement system as a composite mater ial consisting of a matrix of cement binder reinforced with asbestos fibeT, in which the fiber component contributes to the high tensile, flexural, and impact .irength of the product.
Sample Preparation
For this study, data were compiled by testing both 3x8xl/4-in. cake speci mens and 6-in. diameter Class 150 (ASTM C 296) pressure pipe. The pipe was obtained from the production line immediately after stripping from the mandrel. A standard composition of 20 percent asbestos fiber blend, 30 percent New Jersey silex flour, and 50 percent Type I portland cement was employed. Thecomposition of the portland cement is shown in Table 6-1.
processes, the choice of ~ e products such as
.os that is similar to rr-snt thoroughly mixed _r_2nd filtered on a screen Tscire on a form until the immediately after form ^od,* whereas pipes are
- ^CT
^ipted to produce de_a;:hnique a small amount ire amount of water and . .Lzt the dewatering, oper-
t l j
? |
..Tat products contains cement {
_ autoclaved asbestos-cement j
. -i, 30 to 35 percent of
}
i
j --enient and Concrete Termn- )
- een molding of a concrete j r_ised here in place of the j
I
Laboratory specimens were prepared by mixing 150 g of premixed dry blend with 1000 ml of water for 1 min with a mechanical stirrer. The slurry was trans ferred to a 3x8-in. filter box ar.d the water removed by suction. The filter cake was then placed on a press with a confined mold and pressed at 320 psi (22.5 kgf/cin^) for 5 sec to remove excess water. The specimen was stored on a glass plate for the prcstcaming period. As based on previous testing results, the laboratory specimens prepared in this manner simulate the actual products formed by wet process in production.
Pipes obtained from production were selected randomly. A total of 12 sec tions of 10=ft (3.05 m) length was taken. Each pipe was cut into four 2-V4 ft (0.76 m) lengths and the group was divided into four parts.
Curing
It is standard practice to cure asbestos-cement products in a moist atmos phere at ambient temperature before autoclaving. The actual length of the presteaming period varies from 12 hr to a week, depending upon the specific! product. For example, autoclaved pipes and extruded products are given a prcstcaming period of about 1C to 24 hr, whereas the stacked Hat sheets are given 48 to 72 hr.
For this investigation, all samples (both laboratory specimens and pipe) had a presteaming period of 16 hr at approximately 90 percent relative humidity and 20-25 C.
CTD000973
mi.; nUMiWiiii i -I
120 HIGH PRESSURE STEAM CURING
The autoclaving process refers to the curing of articles for a predetermined time in a saturated steam atmosphere at a temperature above 100 C. The pro cess is generally carried out in the temperature range of 160-190 C (320-374 F). with corresponding pressure of about 75 to 180 psig (5.3 to 12.7 kgf/cm2) for 16 hr or more. Air was purged during heating according to normal practice, and heating was done at the rate of 80-100 psig (5.6 - 7.0 kgf/cm2) per hr.
ASBRSTG
thin sections nitric acid in on each sectit rographic mi; cutalions wer and chrysotil
Laboratory samples were hydrothermally treated in a small 36 in. high auto clave with cam automatic pressure controller and recorder. In some cases, the samples were stored under water while being autoclaved.
Three quarters of the 2'A-ft lengths of pipe'were cured under various exper imental autoclave conditions. The remaining specimens were used as controls and cured under conventionally accepted optimum conditions (16 hr at 100 psig in saturated steam).
One of the experimental modifications used for curing the pipe samples was the inclusion of a water spray in the autoclave ( Fig. 6-1). Spray nozzles were positioned at the top of the autoclave, and were fed with condensate water from the autoclave or service water distributed by a pump at a temperature of about 170 C under pressure. The spray nozzles were calibrated to Jeliver approximately 1 gal of water per minute for each foot of autoclave body length. 2
t i
tr
Porosity
Porosity d eury intrusio microns.
Strength
Mechanic made accord commercial! in accordant
Uncombinr.
Uncomb'
PROPERTY EVALUATIONS
In order to evaluate the effects of the various curing conditions, the samples were subjected to the following tests:
Phase Composition
Phase composition identifications were made on an x-ray diffractometer with filtered Cu radiation.
Differential Thermal Analysis (DTA)
! I
Effect of I
Physicoi products c microstruc
cimcn, usii morite (5C steam cc-r.1 strength r;
DTA diagrams were obtained with a differential thermal analy?.er using a 28-gage Pt-Pt, 13% relative humidity thermocouple and a corundum 1200 C( high temperature cell. Sensitivity of this instrument is 0.025 or 10-J cal.
Micrcsopic examination
Examinations were made on a polarizing microscope. Petrographic thin sec tions were prepared lor evaluation of hydrated protland cement pieducts.-3 Quantitive estimates of the amounts of gel and fiber, unhydrated cement, and silica present were made by a point-count method on polished sections. These
Friedlc of the aut moisture i hydration
Our fti tom pent! decrease: identifier expen'C < tion fro :
CTD000974
r.H PRESSURE STEAM ClTv
-- of articles for a predetcnr. - --^perature above 100 C. The : -2 range of 160-190 C (320-,v4
r.0 psig (5.3 to 12.7 kgf/cm'< .:r according to normal practi.t.
::;g (5.6 - 7.0 kgf/cm*) per hr
created in a small 36 in. high , . .--nil recorder. In some cases, ts autoclaved.
-- -were cured under various fxp:? -specimens were used as contt.. i cc^auro- conditions (i6 hr at 100 > ,
--d for curing the pipe samples ; : j* ( Fig. 6-1). Spray nozzles wrr ccrrre fed with condensate water ---d by a pump at a temperature n! .tcss were calibrated to deliver -.r.ach foot of autoclave body
S
~'-us curing conditions, the sampler
"oe on an x-ray diffractometer
~.iuial thermal analyzer using a .-couple and a coruiidum 1200 C(
mment is 0.025 or 10-^ cai.
'Microscope. Petrographic tiiin see-_-J protland cement products.-5 --. d fiber, unhydrated cement, and .cchod on polished sections. These
AASSBRtSmTOaS--C--E--M--E---N--T PRODUCTS
121
, 4 sections were impregnated with epoxy resin and etched with I percent
, acid in a)chol,3,4 Over 300 points at equal intervals were counted
, fjch section, using a point-counter attachment on the stage of the pet-
{tpluc microscope, The ensity factors applied for weight precentage cal-
. j'.ions were as follows: gel 2.2, quartz 2.65, unhydrated cement 3.15,
:tA 2..S6.
verity Porosity determinations were made on a 60,000 psi (4220 kgf/cm^) mer-
,-jty intrusion porosimetcr covering the pore diameter range of 100 to 0.003
-.icions. Suength
*
Mechanical strength determinations on laboratory "sag cake" specimens were cade according to ASTM C 459 for flexural strength. Crushing strength of the commercially produced 6-in. (IS-cm) Class 150 pressure pipe was determined
:n accordance with ASTM C 500.
Uncombined Ca(OH>2 lincombined Ca(OH)n was determined by ASTM Method C SQ0.
RESULTS AND DISCUSSION
Effect of Water-Spray Curing
Physicochemical and mechanical properties of the hardened asbestos-cement products depend on the degree of hydration, density, phase composition, and microstructure of the binder material In a well-autoclaved high-strength spe cimen, using proper proportions of raw materials, the principal binder is tobermorite (SCa0-6Si02-5H20). 4>5.6,7 Proper autoclaving requires that saturated ueam conditions be maintained. If superheated steam is used, there is a severe
strength reduction.
Priedtaender, and Friedlaender and Camarda^ related the strength reduction v of the autoclaved asbestos-cement product under superheated conditions to the moisture loss in the specimen. The loss of the water that is required for proper yrlration is directly proportional to the maximum superheat temperature.
Our findings (Tabic 6-2) showed that for a curing pressure of 100 psig and temperatures in the range 190-230 C (superheated steam conditions), marked decreases in strength and increases in porosity were obtained. X-ray diffraction identification of the binder phase showed the formation of xonotlite at the rvpensc of tobeemorite. In order to compensate for the rapiil moisture deple tion from the product while the hydration process proceeds, a technique
ps--
CTDQQ0975
122 HIGH PRESSURE STEAM (Vj.:
utilizing a water spray, which simulates underwater curing, was developr.t; ensure a saturated steam environment- in large production autoclaves,
Strengths of specimens cured under various experimental conditions an ,, in Table 6-2. The determinations demonstrate that with the aid of undo:, curing, autoclaving pressure can be raised from 100 psig (7.0 kgf/cm^) t,, . 135 psig (9.5 kgf/cm2), yet the strength can be maintained even though (>. autoclaving duration is reduced from 16 hr to 9 hr.
Effect of High Pressure and Temperature Conditions in Underwater Curing
Experiments designed to study the optimum combination' of presssurc F
up, duration of the underwater curing period, and binder characteristics i,: .
experimentally cured specimens were carried out. Samples used for
fraction studies, DTA, and uncombined Ca(OH)2 determinations were cpj-
immediately after autoclaving, ground, and stored in CO2 free desiccators
X-Ray Diffraction Data
Kalousek, et al,7 described the x-ray identification of tobermorite in a-A.cement products. Their method is based on the strong'diffiaction peaks ;>t [1.3, 3.07, and 2.97 ft- and it introduces also an intensity ratio measurer,of the w.97 and 3.07 a peaks to differentiate between tobermorite and 1j ,. CSH (1). Tobermorite has an intensity ratio of the 2.97 and 3.07 X peal-..
the range of 0.70 to 0.80. On the other hand, CSH (1), described by Tay can be identified by strong diffraction peaks at 12,5 and 3.07 ft but thru 1
no peak at 2.97 A so that the intensity ratio for CSH (1) should be 0.0. F fraction peaks at 3.02 to 3.03 ft and at 14 ft suggested to Kalousek ct*a!, r.
presence of CSH,,, a gel-like phase having the composition of (0.8 - 1.33) CaO'SiOynH jO.
Table 6-3 shows the 2.97/3.07 peak intensity ratios for the experimental;, cured asbestos-cement products in addition to the phase identification. A kx-ray diffraction patterns are shown in Fig. 6-2 and 6-3.
It has been found that the intensity ratios of the 2.97/3.07 lines for to!-.: morite can be applied only when no xonotlite or Ca(OH)o is present. V.'h;i: the product is cured, at a pressure higher than 135 psig (9.5 kgf/cm^), a pat: transformation from tobermorite to xonotlite takes place. The strong peak . 3.07 ft for xonotlite causes a reduction of the value of 2.97/3.07 intensity : to around 0.5 or less depending upon the amount of xonotlite present. Or. i'1
other hand, if the silica/cement ratio in the product is very low or the auto claving condition is not adequate, an appreciable amount of Ca(OH>2 if f: which in turn carbonates to form calcite. Calcite has a strong peak at 3a1- ' and also interferes with the 2.97/3.07 peak intensity computation. (Tin- be seen in the first two spectra of Fig. 6-2b which correspond to Samples 1 and 8 of Table 6-2.)
Taylor's CSH(l) may be present in very small amounts in these produrtv : Ct -CnSH, AHO3, FenO^, and SO3 bearing-hydrous phases were not detected.
. >***:
CTD000976
~: . ..ESSURE STEAM CURlSt.
ASBESTOS-CEMENT PRODUCTS
123
r curing," was developed to oduction autoclaves,
H is difficult to determine whether the binder phase is partially Al or FeMtituted, as described by Kalousek11 and Diamond,1^ since the tobermor-
--cr^pe.nmental conditions are ih.. 'ri^at .with the aid of undcrMjs-.
i
, fanned under these conditions is not sufficiently well-crystallized to give jip diffraction peaks in the 11.2 to 1 l.sX region. The appearance of new
TI'D psig(7.0 kgf/cm-) to :>.K. I Av described by Diamond12 at 2.67 to 2.79 A was found in most cases,
--rrtaintained even though the i
though 2.71 to 2.74X. peaks also represented the peaks of unhydrated
-errvarw in Underwater Curing
: IjnU cement. Other peaks that characterize the substitution at 4.20-4.25 1 3.60X are interfered with by the quartz line (4.25/i) and the chxysotile | . A (3.o5/\), the essential ingredients of the autoclaved asbestos-cement
-- -combination of presssure build J . ,jUct. It is, however, assumed that some substitution in the tobermorite ~-r_i't}inder characteristics of so.-, | cilice has taken place.
--. Samples used for X-ray dif-
-- 1 determinations were crushed
. iferential Thermal Analysis and Uncombined Co(OH)
--^2 in CO2 free desiccators.
DTA tracings of all the laboratory autoclaved specimens in Fig. 6-4 show a
.-ill sharp endothermic deflection at 573 to 574C whicn characterizes the 0-/3
-.mtion of tobermorite in asben., --: strong diffraction peaks at = intensity ratio measurement --=e- ween tobermorite and Taylor'i - 2.97 and 3.07 X peaks in
;jrtz inversion of the unreacted silica flour present. The small endothermic ;<ik at 823-825 C and the broad endotherm at around 650 C are due to the
.wince of chrysotile asbestos fibers. A small endotherm at 4] 0-420 C is due 1 the presence of Mg(OH)2, which occurs With asbestos fiber. Broad endot.crms around 200-280 C, 650-700 C, and a sharp and high exothermic peak
---:H (1), described by Taylor1 - I 2.5 and 3.07 A but there is _ -- CSH (1) should be 0.0. iin--c: sted to Kalousek et al, the -=ai- . usition of (0.8 - 1.33)
840-870 C indicate the presence of tobermorite and CSHn binder compounds.13
f f
1 .it the same curing duration a shift of the exotherm from 865 to 843 C was :al when the autoclaving pressure increased from 115 to 175 psig (8.0 to
i :2.3 kgf/cm^). The only samples showing uncombined Ca(OH>2 by DTA
1 jlvsis were Samples 7 and 8 (pressure increased stepwise up to 150 psig
!0.6 kgf/cm2 ), in which a distinctive endothermic response at 510-515 C
rr- ratios for the experimentally
--phase identification. A few . arjd 6-3.-
tad a small one at 480 C were exhibited (last two tracings of Fig. 6-3). it
The sensitivity of determining uncombined Ca(OH>2 by DTA, using the equip
ment constants of the present analyzer, is not as high as by ASTM Method C
--- -h<s 2.97/3.07 lines for tobercr Ca(OH)2 is present. When -23 psig (9.5 kgf/cm^), .3 partial
----*"es place. The strong peak Jt .. value of 2.97/3.07 intensity r.m
1 of xonotlite present. On the -act is very low _cr the auto-
30 (Table 6-4). A calibration curve was employed for semiqualitative estimai 'n of uncombined Ca(OH)2 in the specimens. It was based on the area under
:-e endotherm at 500-515 C versus percentage of Ca(OH)2 added to a ground ` hestos-cement sample with no detectable Ca(OH)2-
Quantitative Estimation of the Components by Microscopic Point-Count Methdd
amount of Ca(OH)2 if fornw>!. .... has a strong peak at 3.04 A
'rarity computation. (This nuy . ~ : h correspond to Samples 7
Point-count analysis was applied to a polished, etched asbestos-cement thin *vtion to determine the quantity of components. Unhydrated cement and -mcacted quartz giains are readily identifiable, whereas chrysotile asbestos may, `tpcar indistinguishable from the binder gel when viewed in polished sections.
' photomicrograph of a polished section of a typical autoclaved asbestos-cement
t.r amounts in these products, bat . :!'e is shown in Fig. 6-5. Therefore, gel and fiber were counted together in the
t- drous phases were not
--linen. For computations, the fiber component is assumed to.be 18 percent
\ ( the total sample* since under those autoclaving conditions employed, no
I i Fiber was 20 percent of the dry sample before hydration. I
CTD000977
124
HIGH PRESSURE STEAM CURINc,
Asm ST*
visual interfacial reaction between cementitious material and chrysotile fiber takes place. (Interfacial reaction between saturated Ca(OH)2 solution and asbestos was, however, detected by tracer technique in electron microscopic examinations of material autoclaved at 200 C for prolonged periods).
The results, listed in Table 6-5, show that the two-step autoclave curing with 5.5 hr at 115 psig (8.1 kgf/cm2) and then 3 hr at 127 psig (8.9 kgf/cm2) yielded the highest gel content and a low percentage of unhydrated cement. Other 8.5 hr underwater cured specimens showed a degree of hydration com parable with that of 100-psig (7.0 kgf/cm2) autoclaved standard.
uirngths j puy is t i
The v r.uing pnglh o , ,>nc end ( , ,m be s i tv rente 1 im-rcial vithin-r :
Porosity Measurement
I'rod
The permaebility of wet-process asbestocement products is generally very low since they have been formed under vacuum pressure, or both. Porosity is
(hose ci cement ,
one of the basic parameters that relates closely to mechanical and physical
properties, so it gives an indication of the effectiveness of any- experimental
autoclave condition.
Pore spectra and the relative percentage distribution of several experimen tally cured specimens are given in Fig. 6-6.
When the autoclaving pressure exceeds 135 psig (9.5 kgf/cm2) as for the top sample in Fig. 6-6 porosity increases despite the use of underwater curing
Underwater curing in the range 127 to 135 psig (8.9 to 9.5 kgf/cn>2) spectra 3 and 4 from top) yielded impermeable products compared with the control. The fifth spectrum from the top, which underwent 8.5 hr underwater twostep curing, showed the least poroxity and highest percentage of fine pores of all the specimens tested.
{ |
From the evaluation of binder material and strength of the underwater cured specimens, the optimum condition is 8.5 hr at a pressure of 100 to 130 psig. (7.0 to 9.1 kgf/cm2). A slow, stepwise pressure buildup using two steps, or pressure levels, (Sample 5 in Table 6-3) is preferred, i.e., a 5.5 hr first step at 115 psig (8.1 kgf/cm2) followed by a 3 hr second step at 127 psig (8.9 kgf/ cm2). Properties of the binders are very similar and often superior to those of the control cured 16 hr at 100 psig (7.0 kgf/cm2).
I j ? !
APPLICATION TO COMMERCIAL PRODUCT
Water-spray autoclaving of 6-in (15-cm) Class 150 pipe with single step or two-step curing was tried under actual production conditions. The crushing strength of the pipe is plotted against single-step autoclaving time, as shown in Fig. 6-7. A strength increase of about 7 percent was achieved when singlestep water-spray curing was carried out 9 hr at 115 psig (8.1 kgf/cm2) which demonstrates the feasibility of employing water spray. A comparison of the
\ t
i
(both 1 ' cured i -1
liie | small a ton ml ; . hydrat ; detect. |
Sail ! irealm t at 10C : tcr.'pe ate toof sm .
Su; ditirr. ; porot:
Av yield l:i\. U. hi
CTD000978
ITRE STEAM CURING
and chrysotile fiber /H)2 solution and -ssctron microscopic iced periods).
-T3 autoclave curing 127 psig (8.9 kgf/cm2) -anhydrated cement. ,-ae of hydration comnandard.
ASBESTOS-CEMENT PRODUCTS
125
strengths obtained in single-step and two-step curing with and without water spray is shown in Table 6-6.
The values shown are considered to give a reliable comparison between curing combinations because comparative pieces were taken from the same length of pipe. Experience has shown individual pipes to be uniform form one end to the other. Although a larger variation than might be expected can be seen between standard-cured pipes No. 2 and 3, for example, it must be remembered that the individual pipes were selected at random from com mercial production, where the between-pipe variation is much larger than the within-pipe variation.
vaucts is generally very -e, or both. Porosity is -nanical and physical - of any experimental
' of several experimen-
Products employing water-spray curing have consistently higher strength than those cured in the absence of water spray. The density change of asbestoscement pipe is negligible.
SUMMARY
Mechanical, physical, and chemical properties of asbestos-cement products (both laboratory-prepared specimens and commercial asbestos-cement pipe) cured under various autoclaving conditions were evaluated.
i kgf/cm2) as for the -i underwater curing, o . .j kgf/cm2) spectra -oared with the control. 5 hr underwater tworssntage of fine pores of
f
' ci of the underwater cured rare of 100 to 130 psig. 'iap using two steps, or
a 5.5 hr first step at .p at 127 psig. (8.9 kgf/ often superior to those
-DDUCT
pipe with single step or -editions. The crushing jdaving time, as shown -ea-as achieved when singleosig (8.1 kgf/cm2) which v. A comparison of the
{
j | ? ; \ |
The desired binder was essentially tobermorite and some C$Hn geL Very small amounts of uncombined Ca(OH)2 (usually less than 0.2 percent) were found in satisfactory autoclaved products. a-2SH, dicalcium-silicate alpha hydrate, and hydrated phases containing AI2O3, Fe2C>3, and SO3 were not detected.
Saturated steam-curing conditions were compared with superheated steam treatments. In regular saturated steam curing, long durations of about 16 hr it 100 to 110 psig (7.0 to 7.7 kgf/cm2) are preferred. With increasing curing temperature and pressure, products formed under high saturated steam pressure ar are found to be more porous lower in strength, and to have an increasing amount of xonotlite..
Superheated steam environments should be avoided. Curing under such con ditions produces binder that contains xonotlite, and has low strength and high porosity.
Autoclaving procedures that employ water spray to ensure saturated steam yield superior products in both strength development and reduced permeabi lity. Meanwhile, the total autoclaving time can be reduced significantly from 16 hr to about 9 hr.
Underwater curing was used in the laboratory to achieve such conditions; but for commercial operation, a water-spray technique was developed to assure saturation.
CTD000979
. it r iiSH rit <t -
126 HIGH PRESSURE STEAM CURING
In underwater curing, or in the presence of water spray, the workable prey sure range seems to be broader. Products can be cured at elevated pressures up to 135 psig (9.5 kgf/cm2) with a slow rate of pressure buildup. The opti mum conditions comprises two-step pressure curing with water spray: 5.5 hr at 115 psig (8.1 kgf/cm2) followed by 3.0 hr at about 130 psig (9.1 kgf/cm2). Binder characterization indicates the abundance of tobermorite and CSHn gel. which is quite dense and impermeable, with 80 percent or more of the pore size diameters less than 0.04 microns.
ACKNOWLEDGMENT
The author wishes to thank Mr. R. Zukoski for his assistance in making many of the measurements reported here, Mr. D. Bailey for the point-count determinations and microscopic examinations, Mr. T. Sopoci for the uncom bined Ca(OH)2 analysis by ASTM C 500, and Mr. R. H.-Adams for the pilot plant evaluation of pipe.
REFERENCES
1. Redican, F. W.; Blair, L. R.; Yang, J. C.; and Gorman. R. J.. "Manufacure of Asbestos-Cement Products," U. S. Patent 3,219,467, Nov. 28, 1965 (Assignors to Johns-Manville Corporation)
2. Adams, R. H., "Method for Steam Curing of Articles Comprising Fiber, Hydraulic Cement and Silica," U. S. Patent 3,327,032, June 20, 1967. (Assignor to JohnsrManville Corporation)
3. Bailey, D., "Microscopy of Steam-Cured Asbestos-Portalnd Cement Products," Joutnal of the American Ceramic Society, V. 46, 1963, pp. 34835L
4. Chayes, F. A., "A Simple Point-Count for Thin Section Analysis," American Mineralogist, V. 34, 1949, pp. 1-11.
5. Blair, L. R., and Yang, J. C,, "Hydration and Solubility Studies of Asbestos-Cement Products," Presented at Highway Research Board Meeting, Washington, D. C,, Jan. I960.
6. ACI Committee 516, "High Pressure Steatn Curing: Modern Practice and Properties of Autoclaved Products," ACI J.OURNAL, Proceedings V. 62, No. 8, Aug. 1965, pp. 869-908.
7. Kalousek, G. L.; Camarda, F. B.; Kopanda, J. E.; and Jugovic, Z. 1., "Analysis of Asbestos-Cement Binders," Materials Research and Standards, V. 6, No. 4, Apr. 1966, pp. 169-179.
CTD000980
1
itofeai
1V^SSURE STEAM CURING
ASBESTOS-CEMENT PRODUCTS
127
~^cr spray, the workable prcs--aired at elevated pressures ^pressure buildup. The opli'~-g with water spray: 5.5 hr -lout 130 psig(9.1 kgf/cm2). ~r tobermorite and CSHn gel, sxcent or more of the pore
I
v Tor his assistance in making - -Bailey for the point-count
- T. Sopoci for the uncom-- R. H. Adams for the pilot
^and Gorman. R. J.; "Manu-u 3,219,467, Nov, 28, 1965
~r Articles Comprising Fiber, --, -, June 20, 1967. (Assignor
8. Friedlacnder, W. V., "Effect of Superheated Steam on Autoclaved Products," Presented before the National Concrete Masonry Association, New York, Jan. 1968.
9. Friedlaendcr, W. V., and Camarda, F. V., "Influence of Superheated Steam on the Autoclave-Cure Strengths of Cement and Concrete Compositions." Menzel Symposium on High Pressure Steam Curing, SP-32, American Concrete Institute, Detroit, 1972, pp. 99-115.
10. Taylor, H. F. \V., The Chemistry of Cement, Academic Press, New York, 1964, V. 1, 194 pp., and V. 2, 372 pp.
11. Kalousek, G. L., "Crystal Chemistry of Hydrous Calcium Silicates: I. Substitution of Aluminum in Lattice of Tobermorite," Journal of the American Ceramic Society, V. 43, 1957, pp. 74-80.
12. Diamond, S. , "Tobermorite and Tobermorite-Like Calcium Silicate Hydrates: Their Properties and Relationships to Clay Minerals," PhD Thesis, 1963, pp. 106-112.
13. Kalousek, G. L., and Prebus, A. F., "Crystal Chemistry of Hydrous Calcium Silicates: 111. Morphology and Other Properties of Tobermorite and Related Phases," Journal of the American Ceramic Society, V. 41, 1958, pp. 124-132.
Asbestos-Portalnd Cement =ery, V. 46, 1963, pp. 348-
=>r Thin Section Analysis,"
-oi and Solubility Studies of Research Board Meeting,
iram Curing: Modern Practice -URNAL, Proceedings V. 62,
--da, J. E.; and Jugovic, Z. T., --s Research and Standards,
[
sj
t !
CTD000981
128 HIGH PRESSURE STEAM CURlv
TABLE 6-1--CHEMICAL ANALYSIS OF PORTLAND CEMENT NATIONAL PIONEER, TYPE 1 CEMENT*
Components
Amount, %
Loss on ignition (1800 F) Si02 Fe203 AI2O3 Ti02 Mn203 CaO MgO Na20 k2o so3
Probable composition
0.4 21.1
2.8 5.0 0.19 0.005 64.7 3.2 0:18 0.67 1.92 100.22
Amount, %
C3S c2s c3a c4af
60.0 15.0 8.5 9.0
* In addition to the ASTM C 150 requirements, the cement meets the following lohns-Manville requirements:
Fineness, specific surface (Blaine), cm^/g .......... 3600
Sulfur trioxide (SO3), max., percent ....................
2.0
n;1
Vl! i'r
lit
vtl V tl ct Ul '
CTD000982
%
PRESSURE STEAM CURING
"vND CEMENT \~T*
Amount, %
0.4
21.1
2.8
5.0 0.19
*
0.005
64.7
3.2
0.18
J.67
1.92
- 100.22 --- --- -----------
- Amount, %
60.0 15.0 8.5 9.0
cement
3600 2.0
ASBESTOS-CEMENT PRODUCTS
129
TABLE 6-2-EFFECT OF HIGH PRESSURE AUTOCLAVING. SUPERHEATED STEAM AND UNDERWATER CURING ON FLEXURAL STRENGTH OF ASBESTOS-CEMENT 3 x 8 x 1/8-IN. "SAG CAKE" SPECIMENS
Experimental Conditions
Description
Temp., C
Saturated steam pressure,
psig
Time hr
Product identified besides asbestos*
Flexural strength. psi
Change fr control strength,?
Saturated steam cure
160 75 16.0 (T) + Q
3320
, 32.7
170 100 16.0 T + (Q)
4940 (Control)
181 135 8.5 T + (X) + (Q) 4620
6.5
190
175
5.0 (T) + X + (Q)
2970
40.0
200 210 16.0 (T) + X + (Q) 2930 - 40.7
230 385 7.0 Tt + X + Q
3050 . 38.2
Superheated steam cure
190 200 230
100 16.0 ' (T) + (Q) + (X) 2500 . 49.4
100 7.0 T + (Q) + X
3860
- 21.8
100 7.0 T + Q + (X)
3360 - 30.9
Saturated steam cure under water
170 175 175 179 181 186 186 192
100 16.0 T+ (Q) 115 5.5 T + Q 115 8.0 T + (Q) 127 8.5 T+(Q) 135 8.5 T + (Q) 150 5.5 (T) + (X) + (Q) 150 8.5 T + (X) + (Q) 175 5.5 (T) + (X) + Q
* symbols:
T = tobermorite gel binder Q = quartz X = xonotlite () denotes minor quantity t denotes trace quantity
(Strength determinations made on 4 to 6 samples of each.)
5080 4600 4860 4910 5020 4750 4620 4590
+ 2.8 - 6.8 - 1.6 - 0.6 + 1.6 - 3i8 - 6.4 - 7.1
CTD000983
ii ~i arii Jjiiitf li'iii'
4
130 HIGH PRESSURE STEAM CURING
TABLE 6-3-BINDER PHASE IDENTIFICATION OF ASBESTOS-CEMENT PRODUCTS BY X-RAY DIFFRACTION METHOD* AND STRENGTH PROPERTIES
Autoclaving Sample conditions, No. psig-hr
Change
Under Flexural from
Hydration
water strength, control product
curing psi
Strength % identified3
Peak intensity ratio 2.97/3.07 A
1 100-16
No 4940 -- T + G
0.77
(control
9 100-16 2 115-5.5
Yes 5080 + 2.8 Yes 4600 - 6.9
T+ G (T) + G
0.81 0.93
10 115-8.0
Yes 4860 - 1.6
T + (G)
0.77
11 '27-8.5
Yes 4910 + 0.6
T+ G
0.88
12 135-8.5
Yes 5020 + 1.6
T + G + (X)
0.68
3 150r5.5 13 150-8.5
Yes 4750 - 3.8 Yes 4620 - 6.5
(T) + G + X 0.58 (T) + (G) + X 0.50
4 175-5.5
Yes 4590 - 7.1
X + (T) + G* 0.47
5 115-5.5, 127-3& Yes 5200 + 5.2 T + G
0.76
6 115-5.5, 150-3b Yes 5090 + 3.0 T + G
0.77.
.14 100^ 127-8.5 Yes 5090 + 3.0 T + G
1.09
(100-2, 110-2,
120-2, 127-2.5)c
15 100-* 135-8.5 Yes 4750 - 3.8 (T) + G
0.92
(100-2, 110-2,
120-1.5, 130-1.5,
13501.5)c
7 100-> 150-5.5 Yes 3870 - 21.6 T* + (G) + C 0.93
(100-1, 110-1,
120-1, 130-1,
140-1, 150-0.5)c
8 100-> 150-8.5 Yes 4550 - 7.9 T* + G + (C) 0.83
(100-1, 110-1,
120-1, 130-1,
140-1, 150-3.5)c
8 Symbols:
T = tobermorite X * xonotlite G = CSlln gel C = CaC03 (Calcite) 0 0 = denotes minor quantity * denotes tTace quantity
k Stepwise curing, 5.5 hr at 115 psig, followed by 3 hr at the higher pressure indicated.
c Stepwise curing, Data may be read as follows, c.g., for Sample 14: Pressure steps from 100 to 127 psig for a total of 8.5 hr, made up of individual steps of 100 psig for 2 hr, and finally 127 psig for 2.5 hr.
ASBESTO:
1
Sample No. Ti
1 1C 9u 2 ii 10 r 11 i: 12 l 3 i ' 13 i 4l 5 l. 6j
1. 14 i; 15
! 7
r
8 ii
8 Stepw._ indica"
k Step" arrow
details, s
!
I
\I
l
CTD000984
"3SURE STEAM CURING
~_SBESTOS-CEMENT JETHOD'
r.'dration nduct -ratified3
+G
Peak intensity ratio 2.97/3.07 X
0.77
+G i+G + (G) -r G -r G + (X) )+G+X 1 + (G) + X - + (T) + G* -+ G -r G
+ G
0.81 0.93 0.77 0.88 0.68 0.58 0.50 0.47 0.76 0.77 1.09
-) + G
0.92
* t(G) + C 0.93
* + G + (C) 0.83
at the higher pressure
--r Sample 14: Pressure steps ^-individual steps of 100 psig
ASBESTOS CEMENT PRODUCTS
131
TABLE 6-4-ANALYSIS OF UNCOMBINED Ca(OH)2
Sample
Autoclaving conditions
Uncombined Ca(OH)2
No. Psig- hr
Under water DTA method ASTM method C 500
1 100-16
No
0
0.2
9 100-16
Yes
0
0.2
2 115-5.5
Yes
0
0.2
10 115-8.0
Yes
0
0.2
11 127-8.5
Yes
0
0.2
12 135-8.5
Yes
0
0.2
3 150-5.5
Yes
0
0.2
13 150-8.5
Yes 0
0.1
4 175-5.5
Yes
0
0.1
5 115-5.5, 127-33 Yes
0
0.2
6 115-5.5, 150-33 Yes
0
0.2
o0
to 1
00
a*
14
Yes 0
0.2
15 100--135-8.5^ Yes
0
0.1
7 100--*4 50--5.5^ Yes
1.5
1.7
8 100--ISO--8.5l> Yes
0.5
0.8
a Stepwise curing, 5.S hr at 115 psig, followed by 3 hr at the higher pressure indicated.
^ Stepwise curing at various pressures from 100 psig to pressure at right of arrow for period of time indicated by number after dash. (For further
details, see Table 6-3.)
j
CTD000985
iiaiiar 132
um *s*
HIGH PRESSURE STEAM CURING
ASBESTOS-CEME>
TABLE 6-5--MICROSCOPIC POINT-COUNT DETERMINATION OF THE COMPOSITION OF ASBESTOS-CEMENT PRODUCTS
Autoclaving conditions (psig - hr) 100-16 100-16 115-5.5 127-8.5 135-8.5 150-8.5 115-5.5, 127-3 100-> 150-8.5 hr
Stepwise*
Underwater curing
Unhydrated cement, %
Composition silica, % Gel and fibe
Nol 2.8 7.4 89.8
Yes 0.9 8.1
91.0
Yes 3.0 7.8 89.2
Yes 2.6 8.3 89.0
Yes 3.2 8.8 88.0
Yes 2.6 6.8 90.6
Yes 1.7 5.1 93.2
Yes 3.2 6.0 90.6
* For details see Table 6-3, Sample 8.
Z c. r-i r> r. <;
U. d. -- -- ~ ;
\
"3 o tr, v
CTD000986
'-{ PRESSURE STEAM CURING
ASBESTOS-CEMENT products
~ DETERMINATION OE ZZMENT PRODUCTS
Composition
133
Cincd as in columns 4 ami 5
vC>
=1
f*t
)I 5r
r
CTD000987
. 134
Yr - ii iJkrn rln .1.-1 8,-ajtagj
(
HIGH PRESSURE STEAM CL'klV, 1 aSBESTOS-I
Steam Inlet
1 i
s ?
! :
f \I
i
CTD000988
CTD000989
2 6 , DEGREES
Fig. 6-2-X -ray diffraction patterns of some autoclaved asbestos-cement products: in 2 0 = 4 to 56 deg range; Q-quartz, A-chrysotile asbestos, G-CSUn, T-tobermorite, X-xonolite, P-unhydrated Portland cement, U.W.-underwater curing
136 WAVELENGTH, H
i
HIGH-PRESSURE STEAM CURING WAVELENGTH, &.
ASRCSTC
I
CURiN CPS IG -1
I03- i
1U0.w0-lt 000.12 Uw
(ioo-i: uW
i
s 11*- s
i 127-3
iti
U V.S-*.
135-7
U H.
!
i 1U1 5H->
Fig. 6-3-X-ray diffraction patterns of some autoclaved asbestos-
cement products: in 2 0 - 6 to 9 deg and.28 to 31 deg range;
U.W. - underwater cunr.g
\
15C-C . UW 175*! U *
nuo.wo-; i
i i t
j : p, r
CTD000990
ASBESTOS CEMENT PRODUCTS
137
ff*
Fig. 6-4--DTA tracings of asbcstos-ceenmt compositions: U'W. underwater curing
CTD000991
m i i MimjaaatmaAOfai
138 HIGH PRESSURE STEAM CURING
I
t I t I 1I
}
\ tv/ V;
* V/.
f t* Fig. 6-5-FoiisheJ section of autoclaved asbestos-cement pipe as viewed by in
flected light; crystals which show cross hatching are C2S; smooth guvco'stals are C3S; "Q" (iconics quartz grains; "C", chi ysotile; marr." tion, 800 X
CTD000992
ressure steam curing
m, tupwmg1 i I < I
s-cement pipe as viewed by rehatchirr. are CnS; smooth gray rains, "C", clLrys'tiie'; magniti-'a-
ASBESTOS CEMENT PRODUCTS
CURING (PSIG-HR) (100-150) -8.5
uw
^ Cl -- (i00-127) - 8.5 U.W.
1
135-8.5 U.W.
n
139
-100
-00 60 40
f -20 nn
___
n_ _ _
-60 -
-40 -20
_n
-
-
127 -8.5
O U.W. H 3 CO tr hCO
11 5-5.5,127-3 U.W.
n
n
n n
-20 -
-
60
-40 -20 -
-
-
-
-
100-16 >10 10- 1
-
-60
-40
i -0 l 0. i -O.CS 0 OS* 0 0 2 0 02 -001
P0RF DIAMETER,^
<001
-20 -
6'6--l'o:c spectra of autoclaved asbestos-cement products; U.W. -under water curing.
CTD000993
.^Tl
140
, ---- ---------------
HIGH PRESSURE STEAM CURING
CRUSHING STRENGTH IN FLEXU R E,PSI
Fig. 6-7 --Effect of curing conditions on crushing strength of asbestos-cement pipe (6-m. Class 150)
CTD000994