Document NEg1zRG3mXy6ewaxMnoGQ1m6g

Manufacturing 3p#eificatlona - Lookland Dacaabar 1Zt 1968 3up* rsading iasua of November 29, 1963 Star* denote changes sine* lssu* of 11/29/68 MIXIHO PBQCEDmc CABgYTSMP - STARCH FORMULA Batch Formula Matarial P*rllt* Bentonite Vo* 90 Starch* Mirafilm 40 / Lytron MS $700 COM 4S Aabaato* Fiber // 1/2* Ola*I Fiber Silicon* R-20 1300 oo Arwonla . 700 ae Pound* Solid* 191.50 22.91 11.44 3*56 12.00 3.00 1.11 sit 215.70 ?rcent 74.85 * 10.62 * 5.30 * 1.57 5.56 1.39 .51 __ 31 100.00 / U* Kofila 50 a* an alternate aouree for atareh and us* th* starch with th* lowest coat, if then la car ohana* la th* prle* relation* * ship. 7a* pound for pound substitution. // KB-41 may be used a* an alternate fiber. Water* Binder Batch: #300 lb*, equal* epproxlnately 140JS of th* dry material*. 44.0 gallon* at approxlnataly 6.1 lb*, per gallon. MOTE*. Silicon* is 50% aollda, apecifie gravity la 1.22* Ammonia 26-29% NHj, specific* gravity is 0.9. PLAINTIFF'S EXHIBIT