Document MX3kEj6dv4Zdnzbv8ZEpEryk

E. I. DU PONT DE NEMOURS & COMPANY KREBS PIGMENTS DEPARTMENT 256 VANDERPOOL STREET NEWARK. NEW JERSEY Serial No. Copy No. l Numerical File I 4 No NEWARK PLANT PIGMENT COLOR RESEARCH REPORT Final Report CPC LAKES FOR Vim* BP-23?~D and BL-2?6D PLANT DEVELOPMENT AND STANDARD 13AT ION Period Covered: j u l i *. mcsmm-, 194?. , .* 4 V FILE, n*TE. 223 p 4 10/6/48 N42169 Copy to* 1 - Numerical Pile 2 Research Offloo (223.4) 3 * Library file <223.4) 4 - #10 Building Pilo 5 - V. Chalupski, Plant Files 6 - W. P. Spengeman, Hewark 7 * Extra. KJJ--48--16 Copy Ho, 1 HEWARK PUSS nmm c o l o r r e s e a r c h r e p o r t Pinal Report CPC LAKES FOR VIHYL, BP-237-U and BL-276-D PMSf DEVELOPMEHT AHD STANDARD IZATIOH JULY - DECEMBER, 194?, CHARGE: 1100-12-21 (AIC-21) SUBMITTED BY: B. J. HESS DATE SUBMITTED: 7-7-48 DUP050067024 mmmmL BP-237-D Bad been obsoleted as a linoleum color in September, 1946, with tha advent of BP-263-D which gava improved dispersion. However, the failure of BP-263-D to give satisfactory performance in vinyl plastic made it necessary to return to the manufacture of a BP-237-D type product for vinyl use# SUMMARY & 1MlilORSi S' In order to me*t a specified cost figure it was first decided to set up the new CPC lake for vinyl at the sane toner content as BP-263-D or about 10# lower in CPC content than BP-237-0 (17.5# instead of 19.1# CPC). Plant manufacture of this modified BP-237-D, now designated BB-276-D, ground oat equal in strength to the BP-237-0 standard, lot 40008. A blend of this material adjusted to strength with Whiting, lot 82176, was proposed as a standard for BB-276-D and gave satisfactory results by vinyl test. Meanwhile, however, the Sales Division had reconsidered their decision to set up e weak product and requested that material equal to BP-237-D be made. As the BP-237-D standard, lot 40000, had been consumed, a proposed replacement standard, lot 82271, was blended from the BL-276-D manufacture (no additional extender added), lot 82271 was set up as the BP-237-D standard in Jfoveaber, 1947. She new BP-237-D standard formula, S-2505, based on the revised process differed from the previous procedure. K-1901, only in the doubling of the batch size. It was decided to retain the original 19.1# CPC in the formula until more experience was gained with the lower toner amount# K-2505 was later designated BP-237-C(A), Subsequent experience with the *Aa process showed that pro duction was averaging about 10# stronger than standard and a new formula, BP-237-IKB), was issued adjusting the CPC content to about 17.5# (the amount used in the standard, lot 82271). the Production Division assumed supervision of 1P-237-B massifactors in December, 1947# DUP050067025 2 c^y8M,M,.,yfc8jL Because of the failure of BP-263~B to glue satisfactory dispersion to vinyl plastic, toe Sales Division requested that a product similar to BP-237-D be included to toe standard line because of toe better performance of the "Bamapow type lake to vinyl. BP-237-D had been replaced in September, 1946. for linoleum composition by 3P-263-D which showed improved disper sion for this use* It toe same tine, however. Sales wished to take advantage of toe lower cost of toe BP-263-D type product which shewed s cost advantage to the order of ten cents a pound over BP-237-D, mainly due to a decrease to toner content of approximately 10# (17* 5# SBC instead of 19.1#). Accordingly, a series of tores batches were made to July, 1947, using a formula which differed as follows from most recent BP-237-D formula, K-190Is 1. The batch else was doubled. 2. The "Monastral* Blue BE standardized 10# paste was decreased 10# from 5000 pounds to 4500 pounds. All three batches ground out about 5# strong versus the 1B-237-D standard, lot 40008, although the formula used has been designed to give a 10# weaker product. A blend of tola material adjusted downward in strength by dry mixing with whiting to give the desired 10# weak product versus toe BP-237-D standard, lot 40008, was submitted for evaluation as the proposed BB-276-D standard, lot 82176. Because of the small amount of experience with the formula, it was decided to issue the Bh-276-0 standard, K-2500, at the 17.5# CPC level (although the standard, lot 82176, eOnt&fned only 14.9# CPC). Meanwhile, toe Bales Division decided to set up a product equal to BP-237-D in strength for vinyl and BD-276-D was obsoleted in July, 1947, before samples had baen submitted or sales made. As the BP-237-D standard, lot 40008, had baen consumed, a replacement standard was needed. A blend of the tores BL-276-D batches was found to give a close match to lot 40008 and this mix, lot 82271, was set up as the 8P-237-D standard in JJovember, 1947. Comparisons of the new versus toe old standard by varnish dryer muboat and to vinyl follows 1 ygitiulffk flawJMtaa* Dot 82271 vs lot 400081 dark, green, intense - OE - 5# strong-trace intense IterMSMfc .twtrMttitBt&l Dot 82271 vs lot 40008j trace dark - 5# strong - y# green. DUP050067026 3* As la the esse of BL-276-D, although the standard lot contained only 17.5# CPC, the new BP-237-D standard formula K-2505 (subsequently the MAH process), was issued at a CPC content of 19.1% differing from the previous standard formula, -1901, only in the fact that the batch size was doubled* Manufacture on the K-2505 formula during November and December, 1947, averaged 10# strong versus lot 82271, and on this basis it was decided to reformulate at the 17*5$ CPC content* The new formula, BP237**D(B) differs from -2505 (the *A" process) in that the whiting extender amount is increased by 12%* Operating acceptad supervision of manufacture of BP-237-D to December, 1947* There is no patent restriction to the manufacture of BP-237-D* It is not believed that this study has resulted to any patentable developments. GLOSSARY: is232si* Originally an approximate 19% extension of CPC on barium rosinate (6%) and whiting 75%)I now consists of 17*5% CPC, 5*5% barium rosinate and 77% whiting* bl -276-Di An extended CPC similar to the present BP-232-D and now obsolete. BP-26VDt An approxtoate 17*5% extension of CPC on Resinous oil (5%) and Siting 77*5%). CPC Copper pbthalocyantoe <lBamano a treatment for improved texture which consists of boiling the pigment with an ammonium rosinate emulsion and striking with barium chloride* DSS-48-11. DUP050067027