Document MM8OQ7RR51bJqz66p1M1oa5Gk

ASBESTOS J.>* . -JW nj, UNION CARBIDE HIGH-PURITY ASBESTOS A UNIQUE FIBROUS SOFTENING AGENT AND RETENTION AID FOR TISSUE AND TOWELS PROVIDES FEXIBILITY; DRAPE; VELVET SURFACE FEEL CLARK SOFTNESS VALUES : BLEACHED SULFITE UNFILLED-----------9.5 SAME WITH 5% ASBESTOS--14.1 IMPROVED RETENTION OF CELLULOSE FINES AND FILLERS SEE ATTACHED GRAPHS AND MILL TRIAL DATA APPLICATION SOFTNESS FOR FACIAL TISSUE Purpose of Trial: Improve overall softness and reduce raw material costs. Type of Paper Machine: Yankee -- 120" Trim with 75/58 mesh wire Machine Speed: 1000 ft./min. with 10% Crepe Production Rate: 20 tons/day Furnish (in use): 10% Kraft Bleached Hardwood ($90 per ton) 66% Spruce Sulfite ($150 per ton) 24% Broke ($130 per ton) Furnish Possible Using 4% High Purity Asbestos: 29% Kraft Bleached Hardwood ($90 per ton) 43% Kraft Bleached Pine ($110 per ton) 24% Broke ($102 per ton) 4% Asbestos ($150/ton) Furnish Cost... $139 per ton paper $110 per ton paper Savings to paper company per year (300 days) ........................................................................................................ $174,000 Economic Gain and Quality Improvement: This trial indicated that this paper company can save $174,000 per year in their facial operation alone. High Purity Asbestos was evaluated at the 2%, 4%, and 6% level. A panel of people experienced in evaluating facial tissue handfeel judged the 4 and 6% asbestos content paper the best they had felt for handfeel. A side benefit was noted by the paper company people--that the asbestos contributed to more uniform formation. Physical Characteristics of the Facial Tissue: Percent Asbestos: Basis Weight (Lbs./3000 ft.2) Bulk or Caliper (Std. Test) Machine Direction Tensile (oz./15 mm strip) Cross Direction Tensile (oz./15 mm strip) Tensile Ratio (M.D./C.D.) Absorption (seconds/.01 ml) 0% 11.53 32 9.3 4.8 2.0 5 2% 10.96 31 8.6 3.8 2.2 5 4% 10.66 30.9 7.1 3.4 2.1 5 4-6% 10.94 31.2 5.1 2.6 2.0 5 RESULT OF THIS WORK WITH THIS PAPER COMPANY: This company now uses asbestos in all products: tissue, towels, and facial tissue. A 17058 SOFTNESS AND FORMATION Another example of pape* properties experienced with High Purity Asbestos additions is illustrated in Table 1. High Purity Asbestos was added to a 30 lh. wet creped towel and softness was found to improve over 20C7-. Additional benefit' included improvements in wet tear. % stretch, and an obvious reduction of solids in the clarified water at the effluent of the saveall. TABLE I TRIAL DATA Basis Weight (Ibs./24' x3fi"x48' ) Softness (Crush Test) Bulk (4 ply cap.) % Stretch Wet Tensile Aged (one inch strip aged in oven at 108eC for 10 min.) Machine Direction Cross Direction Dry Tensile (one inch strip) Machine Direction Cross Direction Wet Tear Machine Direction Cross Direction Absorbency (1/1Occ) Seconds No Ashmtn* 30.0 2200 0.267 6.5 With Aikntot in Piprf 2% 3% 4% 30.1 29.8 30.4 1700 1680 1680 0.268 0.266 0.274 7.4 7.2 7.1 2.7 2.8 2.7 1.7 -- 1.5 1.6 9.6 ' --- 9.3 8.6 5.7 -- 5.5 5.5 30 -- 36 42 34 -- 42 52 35 -- 33 35 Formation improvements are often dramatic with High Purify Asbestos addition. ^7059 Asbestos softening of a 40-lb. towel. ^17060 TEAR FACTOR SOFTNESS UNITS 150 % ASBESTOS IN HANDSHEET % CHEMICAL SOFTENER x 10"' Effects of asbestos on paper softness and tear (kraft pulp,standard weight). A17061 Asbestos improving aged towel absorbency. A 17062