Document MM7pM3wgN7VX4N3qvRRRre2jV
AROCIOFT PLASTICIZERS
A series of inert, chemically-resistant, fire-retarding plasticizers compatible with wide variety of resins. TECHNICAL BULLETIN O/PL-306
PLASTICIZERS
The htormalion contained in this beUelin U. I* ow but knowledi*. tiu* and accurate. bvt l> recommendatwne or tuiMdioni in nM< without luannte*. tine* In* condition* el u* in bayend ou< contnl. The Monaanto Company ditelilmt eny liability incurred m connection with th* mm el lh*i* data ei luitettiont. Furlheimon. nelnini contained herein ihailb* conitrued at * ncemmtndMien to um my product In conflict with eiiMiny patenti covermi any material or it* me. Organic Chemicals Division / 800 N. Lindbergh Blvd. / St. Louis. Missouri 63168
0509867
TOWOLDMONOQ35134
Table ol Contents '
s.
INTRODUCTION............................................................................. 4
DESCRIPTION.................................................................................. 4
COMPATIBILITY...........................
6
AROCLOR IN SYNTHETIC RESINS........................................ 6
Polyvinylchloride....................................................
6
Polyvinyl Acetate......................................................................13
Ethylene/Vinyl Acetate........................................................... 14
Epoxies...................................................................................... 15
Polyesters.................................................................................. 18
Polyethylene.................................
19
Polystyrene............................................................................... 19
Polyurethanes........................................................................... 20
Phenolics................................................................................... 21
AROCLOR IN RUBBERS............................................................... 21 Chlorinated Rubber and Polypropylene..................................21 Styrene-Butadiene Copolymers............................................... 23 Synthetic and Natural Rubbers...............................................24 Polysulfide Sealants..................................................................26
AROCLOR IN CELLULOSIC RESINS......................................... 27 Ethyl Cellulose......................................................................... 27 Nitrocellulose............................................................................ 28 Cellulose Acetate-Butyrate...................................................... 31
AROCLOR IN PAINT, VARNISH, WAX, AND ASPHALT...82 Paint and Varnish.....................................................................32 Wax........................................................................................... 34 Asphalt...................................................................................... 35 Allyl Starch...............................................................................35
AROCLOR IN MISCELLANEOUS APPLICATIONS................. 36 Dust Prevention and Dust Catching....................................... 36 Vapor Suppression (Longer-lasting Insecticides) Moisture Proofing.............................................. Pigment Dispersion............................................ Sealing and Impregnation..................................
^
0509868 2
TOWOLDMONOQ35135
>'
PROPERTIES OF THE AROCLOR PLASTICIZERS............... 39
Solubility.................................................................................. 39
Chemical & Physical Properties (Chart).......................... 42, 43
Monsanto Specifications'.................. ........................'......... .00
Density...................................................................................... 44
Specific Volume......... :............................................................. 44
Volatility............ .................
45
Vapor Pressure..........................................................................46
Viscosity.................................................................................... 47
Stability..................................................................................... 47
Nonflammability....................................................................... 48
Nondrying and Thermoplastic Properties............................... 48
Electrical Properties................................................................. 48
How to Emulsify Aroclor.........................................................49
TOXICITY & SAFE HANDLING.............................................. 50
SHIPPING.......................................................................................... 51
0509869
li n
3
TOWOLDMONOQ35136
Introduction Description 4
The unique Aroclor plasticizers are among the most versatile chemi cally produced materials available. One outstanding characteristic -- inertness -- makes Aroclor useful in many ways for many different applications. The major benefits offered by Aroclor include:
Chemical Resistance Fire Retardance Compatibility with most resins Nonoxidation Adhesivity Low Cost
This bulletin describes some of their many important plasticizing and related applications, including numerous suggested starting formula tions. Examination of their physical properties, also given in consider able detail, may suggest scores of new uses that could not be performed by any other known material.
Additional information about the Aroclor compounds is available from your nearest Monsanto district sales office in the following technical bulletins: PL-307...............Monsanto's Plasticizers in Synthetic-Resin Adhesives PL-311.............. Aroclor Plasticizers for Chlorinated Rubber PL-321.............. Aroclor 1221,1232. 1242 for Polyvinyl Acetate Emul
sion Adhesives PL-327.............. Monsanto's Plasticizers in Protective Coatings PL-331.............. Monsanto Modifiers for Poly-sulfides CS-14................ Aroclor Fire-Retarding Plasticizers and Modifiers in
Epoxy Resins CS-18.................Aroclor Compounds (performance with waxes)
__________________________________
Monsanto's Aroclor plasticizers comprise a series of chlorinated bi phenyls and chlorinated polyphenyls. They vary from mobile, oily liquids to white crystals and hard, transparent resins.
Twelve of the Aroclor plasticizers, each of which represents a series, are discussed in this bulletin. An understanding of the system for designation of each Aroclor should pro-re useful in the evaluation of the property gradations among them. The last two digits indicate the approximate weight percentage of chlorine in the product, and the first two digits indicate the type of material, as tallows:
12 -- chlorinated biphenyls 25 -- blend of chlorinated biphenyls and chlorinated triphenyls
(75:25) 44 -- blend of chlorinated binherrrls and chlorinated triphenyls
(60:40) 64 -- chlorinated triphenyls
For nearly every Aroclor mentioned, a dariar. less-pure grade exists, with about the same physical and hheumcal characteristics, but lower in price.
0509870
TOWOLDMONOQ35137
Aroclor compounds are nonoxidizing, inert, pi-minni'iilly thermoplastic, of low volatility, non-corrosive to metals, ami low cost. Aroclor com pounds are not hydrolyzed by water and ivi,i alkalies, acids, and corrosive chemicals. The viscous, more-highly chlorinated liquids and resins do not support combustion, and they impart, (ire retardance to other materials.
The crystalline Aroclor compounds are relatively insoluble, but the liquid and resinous compounds are soluble in m<nl of the common organic solvents, thinners, and oils. All Aroclor compounds are in soluble in water and glycerine. Aroclor 546b j;) insoluble in lowermolecular-weight alcohols; Aroclor 4465 is only partly soluble in the lower alcohols.
Aroclor compounds plasticize a great many r>aim without softening them unduly. The Aroclor compounds are unwrp;Hed for the plasti cizing of protective coatings, particularly for nw, in chemical plants and other facilities that require a tough, chemically resistant surface. Aroclor plasticizers can also be used to flexibiliw. scaling compounds, adhesives, lacquers, inks, varnishes, free film?, fabric coatings, and pigment dispersions. They are also used as components or extenders in elastomers and waxes. The properties of many end products can be improved -- yet at reduced overall cost -- by the u of an Aroclor as either a primary or a secondary plasticizer.
The properties imparted by Aroclor compound? b.r.d their usefulness in particular applications) vary in regular gradient over the series. Selection of the right Aroclor for a particular vie can generally be made by comparison of the properties, by "blending" two or more, and by adjusting the percentages used in the particular mixture in which the Aroclor compounds are formulated.
Monsanto's Plasticizer Council can provide specific formulation guidance that may help you improve your ;.rv: .,x or lower your processing cost. Processors are invited to ask v.e nearest Monsanto office for help on special problems.
Compatibility___________
-
----------- -------
The Aroclor plasticizers are compatible with materials; they are compatible to the extent following:
common plastic ical use with the
Asphalt Benzyl Cellulose Carnauba Wax Cellulose Acetate-Butyrate Chlorinated Rubber Coumarone-Indene Resins
Damar Resin Ester Gum Ethyl Cellulose Ethylene/Vinyl Acetate
Epoxy Resins Nitrocellulose Paraffin Phenolic Resins
Polyexb^erue Polyevv-r
Polysty-** -cesins Polyiy?-?,-. y,.-.ne
PolyE'-idev
Polyu.r^-.>./^
Poly*.;-- 'rotate Polyv-y u.,yral
. Polyv Rosin
Ruble-
vvoride Chloride
Styr^-Vv-^v.^iene Copolymers
0509871
5
TOWOLDMONOQ35138
Liquid Aroclor
Soft, Resinous Aroclor
Hard, Resinous Aroclor
Aroclor plasticizers are not compatible with phenolic resins in the final stage of condensation or with cellulose acetate. Aroclor plasticizers generally impart progressively increasing proper ties in the direction of the arrows in the following diagram:
Flame Hardness Flexibility Retardance Volatility Density Viscosity
Usually the desired balance between flexibility and hardness can be obtained either by selection of an Aroclor with the appropriate physical characteristics or by use of a blend of two or more Aroclor plasticizers. In evaluation of formulations that contain Aroclor plasticizers, the compounder should thoroughly test an experimental product for compatibility, heat and light stability, and other properties according to normal industry practices.
Aroclor Plasticizers In Synthetic Resins
Low-cost Aroclor plasticizers are valuable for a variety of applications. They improve chemical resistance, flame retardance, and oxidation resistance. Depending upon the use, the various Aroclor plasticizer offers a number of benefits to the user. In almost all formulations, the use of an Aroclor reduces the over-all cost per pound.
In Polyvinyl Chloride .
Aroclor is valuable in polyvinyl chloride and copolymers as a secondary plasticizer or as a plasticizer extender. The Aroclor plasticizers impart flame retardance and chemical resistance.
Selection of the proper Aroclor enables compounders to impart such special properties to their formulations as:
Resistance to migration to nitrocellulose lacquers (Aroclor 1260 and 1262).
Fine,uniform cell structure in vinyl foam (Aroclorl262and 1268).
Adhesion in vinyl coatings (Aroclor 1260 and 5460).
Viscosity stability in plastisols (Aroclor 1248 and 1254).
Compatibility
Aroclor plasticizers (except Aroclor 1268) are compatible to about 25 per cent of the total plasticizer content in polyvinyl chloride and usually somewhat greater in copolymer resins. At these levels, no exudation occurs in the loop-compatibility test, one of the most severe used by the industry.
050<8U
TOWOLDMONOQ35139
The control specimen burns rapidly; the one containing Aroclor does not even ignite.
Performance
As an illustration of the performance of Aroclor plasticizers, Table 1 shows evaluation of the five most commonly used in polyvinyl chloride.
TABLE 1
PERFORMANCE EVALUATION OF FIVE AROCLOR PLASTICIZERS IN POLYVINYL CHLORIDE
Vote- `
Low-Temp
Hard tilitf Kerosene-' Flexibility
Concern ness {Plasti Extraction (Clash Tensile
Elonga
tration (Shore cizer (Plasticizer & Berg) Strength Modulus tion
Aroclor (parts)
lost, %J lost, %) (Tf*C) (psi) fpsi) tw
1248 15 87 19 23 -26 2330 1320 342
1254 16 88 14 24 -24 2310 1360 334
1260 15 89 11 32 -22 2200 1330 315
4465 17.5 89
6
19
-19 - -- -
6442 17.5 87
6
16
-20 - - -
Ingredients
a) Opalon 660 PVC resin Dioctyl Phthalate Calcium Carbonate Stabilizer Aroclor
b) 24 hours at 87*C over activated carbon
c) 96 hours at 25*C
Parts by Weight
100 45 40 3 indicated
TOWOLDMONOQ35140
Heat and Light Stability
Aroclor compounds impart good heat stability but somewhat reduce the light stability of vinyl formulations, but no more so than do many other secondary plasticizers commonly used in the industry. Light stability of the system may be improved by incorporation of a small amount of light-screening agent, such as 0.1 per cent Tinnvin P.m
Chemical Resistance
For imparting resistivity to chemical attack, the Aroclor plasticizers are unsurpassed. Independent evaluations of the chemical resistance of vinyl chloride-vinyl acetate copolymer paint, modified by eight types of materials (alkyd resin, phenolic-chinawood oil varnish, ester gum-linseed oil varnish, Aroclor 1254, dioctyl phthalate, tricresyl phosphate, polymeric plasticizer, and acrylic polymer), showed that Aroclor 1254 has the "best all-around chemical resistance, failing badly only in the gasoline test."
Paints were sprayed onto solvent-cleaned, unprimed, cold-rolled-steel panels, which were then immersed in seven types of solutions until failure. The data in Table 2, excerpted from the November 1955 issue of Official Digest of the Federation of Paint and Varnish Production Clubs, compare the chemical resistance imparted by Aroclor 1254 and by dioctyl phthalate.
TABLE 2
COMPARATIVE CHEMICAL RESISTANCE OF PLASTICIZERS IN VINYL CHLORIDE-VINYL ACETATE COPOLYMER PAINT
Plasticizers
Dioctyl Phtha Aroclor late 1254 m <%!
10 ~ - 10 25 - 25 AO - 50
a) End of test
10% Sodium Hy'drox ide (days)
120'
120'
60
120*
60
120'
Time to Failure in Corrosive Media
10% Hydro chloric Acid Gasoline (hours) (days!
92 0.4
168' 5
24 0.4
120 0.4
24 0.4
96 0.4
5% Sodium Hypo chlorite (days)
4
13
4
14.5
4
ii
Linseed 10% Oil Acetic Fatty Acid Acids (hours) (days)
84 60
168' 90*
64 27
120 90'
48 22
100 60
1% Tide at WTF (days)
21
22 25
22 25
22
In other corrosion-resistance tests of polyvinyl chloride plastisols, containing 70 parts plasticizer per 100 parts resin a formulation that contained 1 part Aroclor 1254 to 3 parts dioctyl phthalate was much more resistant to 15 percent nitric acid at either 23 or 50C for six months than a compound plasticized with dioctyl phthalate alone.
The plastisol modified with both Aroclor 1254 and dioctyl phthalate was also more resistant to 25 percent chromic oxide at 50C for four weeks and was equivalent at 23C for six months in comparison with the dioctyl phthalate-modified vinyl plastisol.
*Tf4t<Mrk el C*f|y Ctiemleel Ce.
050`>87'i
TOWOLDMONOQ35141
Migration Resistance
The use of Aroclor 1262 as a coplasticizer with dioctyl phthalate greatly enhances the resistance of plasticizer migration to nitrocellulose lacquers and films. Table 3 compares this property for four formulations.
TABLE 3
PLASTICIZER MIGRATION TO NITROCELLULOSE LACQUERS AND FILMS
Plasticizer*
Dioctyl Phthalate Polymeric Plasticizer Aroclor 1262 Hardness, Shore "A"
Time (weeks) Boom Temperature
i 2 3
Aroclor and DOP (parts)
66 -- 20 72
No Change No Change No Change
4 No Change
6 No Change
10 No Change
60* C 1 No Change
2 No Change
3 No Change
4 No Change
6 No Change
10 No Change
General Motors Lacquer Indentation.
Test (158*F; 72 hr.; Very Slight
K-psi load)
Softening
Control OOP /parts)
71
-
-- 72
Aroclor. DOP, and Polymeric (parts)'
36
33
20
72
Polymeric and DOP (parts)
38 35
-
73
No Change No Change No Change
No Change
No Change
No Change
No Change
No Change
Very Slight Marking
Very Slight Marking
Very Slight Marking
Very Slight Marking
Slight Marking Slight Marking Slight Marking
Slight Marking
Slight Marking
Slight Marking
Slight Markins
Slight Marking
Slight Marking
Moderate Marking Moderate Marking Moderate Marking Extreme Softening
Moderate Marking
Severe Marking
Very Slight Softening
Slight Softening
Slight Softening
Slight Softening
Lifting
Very Slight Softening
Very Slight Softening
Slight Softening
Slight Softening
Slight Softening
Moderate Softening
Extreme Softening
a) Formulation Ingredients
Opalon 660 PVC Resin Epoxy Soybean Oil Barium-Cadmium Laurate Calcium Carbonate Plasticizer
Parts by Weight
100 3 3 25
as indicated
0509875
9
TOWOLDMONOQ35142
Plastisols
The use of an Aroclor as a coplasticizer with dioctyl phthalate in polyvinyl chloride plastisols or organosols contributes greatly to the viscosity stability of these materials, especially at elevated tempera tures. This benefit is especially important whenever shelf stability is required. Although the initial viscosity of the plastisol or organosol is increased by the use of an Aroclor in the formulation, the viscosity reduction upon temperature elevation (before the fusion temperature is reached) is much greater than when most other plasticizers are used.
A comparison of the viscosity stability of plastisol formulations with and without Aroclor is given in Table 4.
TABLE 4
VISCOSITY STABILITY OF PLASTISOLS
25'C Initial 1 Day 1 Week 2 Weeks 4 Weeks
Dioctyl Phthalate (80 phr) Viscosity* (poises)
36 65 97 116 132
Aroclor 1254 (20 phr) Dioctyl Phthalate (60 phr)
Viscosity* (poises)
49 63 78 76 148
40'C Initial 1 Day
1 Week 2 Weeks
4 Weeks
37 84 215 308 426
48 98 108 110 209
SO'C Initial 1 Day
1 Week 2 Weeks
4 Weeks
66 gel
94 660 980 gel
a) Brookfield LVF viscometer. No. 4 spindle, 12 rpm
Aroclor 5460 (20 phr) Dioctyl Phthalate (60 phr)
Viscosity* (poises)
92 154 161 178 252
68 136 139 164 274
100 470 900 gel
Dipping Plastisols. The chemical resistance of Aroclor compounds is used to good advantage in chrome-plating-bath coatings and in glove coatings, as illustrated by the following formulation for a clear glove dipping plastisol:
ingredients Opalon 440 PVC resin Aroclor 1254 Diisodecyl Phthalate Santicizer 160 HB-40 Secondary Plasticizer Liquid Barium-Cadmium Stabilizer Liquid Chelator-Stabilizer Santocel 54 Silica Aerogel
Parts by Weight 100 20 60 25 20 2 0.5 3
0509876
C
TOWOLDMONOQ35143
Sealers. The adhesion-imparting characteristics of Aroclor compounds, their oxidation stability, and their chemical resistance are utilized in the manufacture of automotive sealers, such as the following suggested starting formulations:
Ingredients
Parts by Weight
Opalon 440 PVC resin Vinyiite' VMCH resin Aroclor 1260 Diisodecyl Phthalate Santicizer 160 Calcium Carbonate Epoxy Soybean Oil Dibasic Lead Phosphite
96 4 50 100 28 125 5 3
Fabric-Coating Vinyl Dispersions. The use of Aroclor plasticizers in organosol or plastisol formulations enables the manufacture of fireretardant free films and coated fabrics with a high degree of hardness, yet flexibility. The following typical starting formulation for a vinyl organosol to be used for free film or coated fabric illustrates this effect:
. Ingredients
Parts by Weight
Opalon 440 PVC resin Dioctyl Phthalate Aroclor 1254 Liquid Barium-Cadmium Stabilizer Epoxy Soybean Oil Thinner Xylene
100 33 10 2.5 3 20-35 15-25
Rigid Plastisols. The viscosity characteristics of the Aroclor plasti cizers are utilized in the following formulation for rigid, rotationallycast objects. The formulation is very viscous when first made up, but when heat is applied, the viscosity decreases so that a smoothly-flowing plastisol is obtained. The finished object has a Shore "D" hardness of 63.
Ingredients
Parts by Weight
Opalon 440 PVC resin Geon"' 202 PVC resin Aroclor 1254 Santicizer 141 Epoxy Octyl Taliate Liquid Barium-Cadmium Stabilizer Liquid Zinc Stabilizer Polyethylene Glycol 400 Monolaurate
of Union CtrbMt Cwp. ol B. F. Goodrich Chm>e*1 Co.
55 45 35 10 5 2 0.5 1
0509827
TOWOLDMONOQ35144
Vinyl Foam
Aroclor 1262 and 1268 impart fine, uniform cell structure and flame resistance to chemically-blown vinyl foam, as shown by the following formulations:
Ingredients
Opalon 440 PVC resin Aroclor 1262 Aroclor 1268 Dioctyl Phthaiate Diisodecyl Phthaiate Di-(/?-0ctyl, /r-Decyl) Adipate Santicizer 214 Santicizer 409 Butyl Oleate Liquid Barium-Cadmium Stabilizer Epoxy Resin Neutral Calcium Petronate Calcium Oxide Sodium Lauryl Sulfate Nitrosan* Chemical blowing agent
Parts by Weight
100 100 100
- 20
-
20 - 10
40 - -
-- 50 30
- 10 30
-- 15
-
50 - -
5--
233
-2 2
3.6 3.6 3.6
-1
1
-- 1.6 1.6
10 10
5
Flame-Retardant Floor Tile
The nonflammability of the Aroclor compounds suggests their use in the manufacture of flame-retardant vinyl-asbestos floor tile for military applications. In Table 5 is presented an evaluation of three Aroclor plasticizers in typical vinyl-asbestos-tile formulations. Substitution of antimony oxide for part of the limestone is suggested for still greater fire retardance.
TABLE 5
EVALUATION OF AROCLOR IN FLAME-RETARDANT, VINYL-ASBESTOS FLOOR TILE
Santicizer 160 Aroclor 1254 Aroclor 1260 Aroclor 5460 McBurney Inden tation Hardness Banbury Time (to reach 280*F, sec.) Time to band on roll mill (sec.) Plasticity Tack Surface
a) Formulation
Control* (parts)
37
-- _
7.8
99
15
Excellent Excellent Excellent
Aroclor 1254 (parts) 30 15
-
9.6
96
10
Excellent Excellent
Fair
Aroclor 1260 (parts) 36
--
17
--
10.4
102
10
Excellent Excellent Excellent
Aroclor 5460 (parts) 40
_
20 11.2
115
5
Excellent Excellent Excellent
*Titdtmnk gI . I. do Pent da Htmoort t Ce., Inc.
TOWOLDMONOQ35145
In Polyvinyl Acetate
Ingredients
Opalon 506 PVC Resin Santicizer 160 Aroclor Asbestos Limestone Titanium Dioxide Stabilizer
Parts by Weight
100 As Indicated As Indicated
160 290 15
5
Aroclor compounds are excellent plasticizers for polyvinyl acetateemulsion adhesives and hot-melt adhesives. The excellent tack and strong bonding power they impart and their low cost contribute greatly to the performance and profitability of these adhesives.
Emulsion Adhesives
The liquid Aroclors -- such as Aroclor 1221, 1232, and 1242 -- blend readily by simple stirring with polyvinyl acetate emulsion at up to 11 parts per 100 parts of emulsion. They greatly improve the quick-tack and fiber-tear properties of the adhesive. The performance of Aroclor plasticizers in polyvinyl acetate-emulsion adhesives is compared with that imparted by dibutyl phthalate in Table 6. The following is suggested as a typical starting formulation for a low-cost, quick-tack adhesive:
Ingredients__________________________ Parts by Weight
Gehra $-55 PVAc Emulsion Aroclor 1232
100 11
TABLE 6
PERFORMANCE OF PLASTICIZERS IN POLYVINYL ACETATE-EMULSION ADHESIVES
Hardness (Shore "A")
Low-Temperature Flexibility (Clash & Berg, T/# *C)
Volatility (24 hr., 86*C over activated charcoal) (Plasticizer lost. %)
Dibutyl Phthalate (11 phr)
69
-10.2
4.0
Aroclor 1221
(11 phr) 66
-5.9
4.8
Aroclor 1232
(11 phr) 86
4.0
4.3
Aroclor 1242
(11 phr) 97
5.3
4.0
Kerosene Extraction (24 hr.. 25C)
(Plasticizer lost. %)
4.1 4.5 3.8 4.2
Formulation Viscosity (cp.) Initial*
2420
2240
1 Day
2460 _
3 Days
- 2200
4 Days
2520 -
5 Days
- 2200
7 Days
- 2180
10 Days
- 2260
a) Initial viscosity of unplasticized emulsion: 1500 centipoises
2160
-
2060
_
2040 2020 2060
-
--
--
-
0509879
13
TOWOLDMONOQ35146
In Ethylene Vinyl Acetate
When the slight odor of Aroclor is objectionable in an adhesive for certain applications, it can be easily masked, at negligible cost, by the addition of a small amount of Santomask II.
Hot-Melt Adhesives
Aroclor compounds are widely used as plasticizers in. polyvinyl acetate hot-melt adhesives for bookbinding and other applications. Four sug gested started formulations for evaluation are as follows:
Ingredient
Parts by Weight
Application
Temperature 165'-175*C
LowMelting
AlkaliDispersable
Polyvinyl Acetate Opalon 505 PVC resin
95' 100' 5--
50* --
38*
--
Modified Rosin Coumarone-lndene Resin (soft)
---
----
25
-
-
28.3
Aroclor 1254
- 55
12
27
Aroclor 1260
50-75 --
--
--
Dibutyl Phthalate
--~
13
7
Santicizer 160 (or dibutyl phthalate) 50-75 30
-
--
Clay
~ 25
--
-
Fluxing Resin (Filtros Resin WVV) - 75
--
Acrawax 0'
---
-
1
Sodium Benzoate
----
-
0.76
Viscosity (centipoises)
2000 (120aC) Non-blocking
3500 (175'C) Non-blocking
a) Gelva V-7 bj Gelva C-3 V-10 cj Gelva C-5 V-16
The Aroclor products are among the most compatible, effective, and versatile plasticizer/modifiers available for ethylene vinyl acetate. Both the liquid and solid Aroclor plasticizers are highly compatible with ethylene vinyl acetate and other ingredients commonly used in ethylene vinyl acetate, such as paraffin and microcrystalline waxes and other resin modifiers. Aroclor offers special functional properties and reduces formulation costs when used with ethylene vinyl acetate.
Hot-Melt Adhesives
Aroclor in ethylene vinyl acetate hot melts imparts excellent initial tack and high final bond strength. Aroclor is particularly useful in providing versatility of adhesive bond to various substrates such as aluminum foil, cellophane, polyethylene. Mylar** polyester film and paper. Liquid Aroclor, such as Aroclor 1254, provide greater flexibility and lower application viscosities. Solid Aroclor 5460 provides adhesive strength, permanence, and lowers the melt viscosity. Both liquid and solid Aroclor products are exceptionally heat stable, resistant to oxidation, moisture, and chemical attack and are, in general, very inert. Flexibility, specific adhesion, and melt viscosity may be adjusted by varying Aroclor concentration and by selection of solid and/or liquid Aroclor plasticizers.
Tdmrk cl Gifts Chcmitkli. *`Tcdimrk o* OuPonl Co.
0309880
c
c
c
TOWOLDMONOQ35147
In Epoxy Resins
Pressure-Sensitive Adhesives
Aroclor in ethylene vinyl acetate pressure-sensitive adhesives imparts excellent specific adhesion and tack. Liquid Aroclor, such as Aroclor 1248 or 1254, improve flexibility and adhesion while solid Aroclor 5460 or 5442 impart a high degree of tack and bond strength.
Suggested starting point formulations for evaluation using Aroclor in ethylene vinyl acetate hot-melt and pressure-sensitive adhesives are shown below:
Hot-Melt Adhesive
Pressure-Sensitive Adhesive
"Elvax"*
Ports by Weight
40
"Elvax" m
Ports by Weight
30
Aroclor 5460 40 Aroclor 5460
40
Microcrystalline Wax
20
Aroclor 1254
00
The Aroclor plasticizers probably have greater compatibility with epoxy resins than any other available nonreactive plasticizer-modifiers. The excellent chemical resistance, oxidation resistance, and adhesive qualities imparted by the Aroclor compounds reinforce these important beneficial properties of epoxies and thereby help the compounder reduce his formulation costs materially without significant adverse affect on performance.
The lower-molecular-weight, liquid Aroclor plasticizers (such as 1221 and 1232) have maximum plasticizing efficiency and impart the most flexibility to epoxy compounds. The more viscous, resinous Aroclor products have progressively less effect on epoxy flexibility: the highmolecular-weight, solid Aroclor plasticizers (1268, 2565, 4465, 5460, etc.), in fact, tend to reinforce the compound.
The effects of Aroclor 1221 and 1248 on the properties and performance of an epoxy resin are indicated by the data in Table 7.
TABLE 7
EFFECT OF AROCLOR 1221 AND 1248 ON PROPERTIES OF EPOXY RESINS
Formulation*
Viscosity*
Physical Properties
Physical Property* After Heat Aging
Aroclor Aroclor 1221 1248 --
28 - 28
Before Curing Agent
12,800 (30 rpm)
1880
7700
bod Clarity After Impact (Light Hardness Curing Resist Reflect Shore "D" Agent ance ed) (%) (10 sec.)
7900 0:2
3.0
76
1200 4300 0.6
3.0 3.0
8 40
Hardness Weight Shore "D" Loss (10 sec.) (%)
86 0.012
81 2.118 88 0.682
Trd*mirk el Do Pont Co.
oiosasi
15
TOWOLDMONOQ35148
c
Ingredients
Parts by Weight
a) Liquid Epoxy Resin
100
Tetraethylenepentamine
8
Aroclor 1221 or 1248
As Indicated
Cure: 30 minutes at 100*C
b) Brookfield LVF No. 4 spindle; 60 rpm unless otherwise specified
c) 24 hours at 86C in activated charcoal
Development of flame-retardant epoxy resins is of wide-spread interest. Aliphatic amine-cured epoxy-resin formulations are made self extinguishing by the use of 20 parts of liquid Aroclor per hundred parts of resin. The incorporation of antimony oxide at 5 phr, with 15 parts of Aroclor per hundred parts of resin, yields nonburning formulations (Table 8).
The use of liquid Aroclor in aliphatic amine-cured epoxies also improves flexural strength and compressive-yield strength, has little effect on tensile strength, and slightly lowers heat-distortion temperature and compressive ultimate strength.
The use of solid Aroclor in phthalic anh3rdride-cured epoxy systems also reduces flammability and, in combination with antimony oxide, produces nonburning formulations. The solid Aroclor products also greatly improve such important properties as compressive strength, flexural strength, compressive-yield strength, and tensile strength, although they slightly lower the heat-distortion temperature (Table 9.)
Extension of epoxy-resin adhesives with Aroclor greatly reduces the formulation cost, with minimum effect on the bonding characteristic of the adhesive or surface coating.
In epoxy-resin protective surface coatings, the use of Aroclor 1254, 1260, or 1262 economically imparts excellent chemical resistance, particularly to acids and alkalies. When resistance to solvents is de sired, however, Aroclors should not be used, since they are true plasti cizers and do not combine chemically with the epoxy resin. Frequently, about 10 to 15 per cent Aroclor 1260 or 1262 is added to increase the flexibility of the epoxy composition, with minimum effect on the corrosion resistance and adhesion of the film.
0509682 16
TOWOLDMONOQ35149
0509883
w
v,
V
TABLE 8
EFFECT OF AROCLOR 1242 AND 1260 ON FLAMMABILITY AND PHYSICAL PROPERTIES OF EPOXY RESINS
Aroc/or 1242 (phr) -
20 15 '-
Formulation * Aroclor Antimony 1260 Oxide (phr) (phr) ---
- -- ''
20 --
-5
15 5
Hardness (Rockwell "M")
104 108 103 107
100
Flammability (ASTM 635-5ST) inches Rate burned {in.jmin.)
4 0.82
2.125 b
1.125 b
0c
0c
HeatDistortion Temp. CC)
117.5
79.5 87 81
92
Flexural Strength
(psi) 20,100
21,800
23,800 22,200
22,100
Tensile Strength
(psi)
:
; '
11,400
10,700 : 13,000 ' 12,800 '
9,800 ' .
Compress/ye Yield Strength
(psi) 15,700
17,900
17,250
16,700
16,950
Ingredients
Parts by Weight
a) Liquid Epoxy Resin
100
Diethylenetriamine Aroclor 1242 or 1260
13 as indicated
i
Antimony oxide
as indicated
Cure: 16 hours at room temperature, plus 2 hours ar 100*C
bj Self extinguishing
c) Nonburning
TABLE 9
EFFECT OF SOLID AROCLOR ON FLAMMABILITY AND PHYSICAL PROPERTIES OF EPOXY RESINS .
Aroclor 1268 (phr)
--
20 15 -
Formulation *
Aroclor ' Antimony
5460 Oxide
Hardness
(phr} (phr) (Rockwell "M")
----
113
---
112
20 --
113
-5
112
15 5
111
Flammability (in.lmin.) 0.6 0.38 0.38 b b
HeatDistortion
Temp. ro
143
128
135.5
134
135
Flexural Strength
(psif
16,900
25,900
26,300
20,000
13,000
Tensile Strength
(psi) 11,000
13,500
11,500
11,100
10,200
: . Compres:'> sive Yield j\ Strength ! (psi) i 20,900
!> 22,300
i! 21,000
:; 20,500
r: 21,200
' Ingredients a) Liquid Epoxy Resin
Parts by Weight
T- loo
" Phllialic Anhydride
75
DMP-30* catalyst
0.1
Aroclor 1268 or 5460 Antimony Oxide
as indicated as indicated
'
Cure: 20 hours ar 15Q*C
'
b) Nonburning *T4mfk8l fehB&Xut 6*.
; .i
Compress/'ye
Strength (psi) 43,000 32.500 32.900 32,400 38,150
Compres sive
Strength (psi) 23,400 36,500 41,700 36,700 40,700
"4
TOWOLDMONOQ35150
TABLE 8
EFFECT OF AROCLOR 1242 AND 1260 ON FLAMMABILITY AND PHYSICAL PROPERTIES OF EPOXY RESINS
Aroclor 1742 (phr) ~
20
-- 15
Formulation Aroclor Antimony 1260 Oxide fphrj (phr)
--- ---- 20 --
-5
Hardness (Rockwell "M")
104
108 103
107
Flammability (ASTM 635-56T) inches Rate burned (injmin.)
4
2.125 b
1.125 b
0c
HeatDistortion Temp. ("Cj
117.5
73.5
87
81
- 15
5
106 0
c 92
Ingredients________________________________________________ Parts by Weight
a) Liquid Epoxy Resin________________________________________ __ _______ 1QQ
Diethylenetriamine___________________________________________________ 13
Aroclor 1242 or 1260_____________________________________________ as indicated
Antimony oxide
as indicated
Cure: 16 hours at room temperature, plus 2 hours ar 1Q0*C____________________________
b) Self extinguishing____________________ '____________________________________
c) Nonburning
Flexural Strength
(psi)
20,100
21.800
23,800 22.200
22.1QQ
Tensile Strength
(psi)
11,400
10,700
13.000
12,800
9,500
Compres sive Yield Strength
(psi)
15,700
17,900
17.250
16,700
16.950
TABLE 9
EFFECT OF SOLID AROCLOR ON FLAMMABILITY AND PHYSICAL PROPERTIES OF EPOXY RESINS
Aroclor 1268 (phr) --
20
15
-
Formulation * Aroclor 5460 (phr) _
-
20 -
15
Antimony Oxide (phr)
--
~ --
5
5
Hardness (Rockwell "M")
113 112 113 112 111
Flammability (in.lmin.)
0.6
0.38
0.38 b b
HeatDistortion
Temp. rc)
143
128
135.5
134
135
Flexural Strength
(psi)
16,900
25.900 26,300
20.000
19,000
Tensile Strength
(psi) 11,000
13,500 11,500
11,100
10.200
Compres sive Yield Strength
(psi)
20,900
22,300
21,000
20,500
21.200
Ingredients
a) Liquid Epoxy Resin Phthalic Anhydride DMP-30' catalyst Aroclor 1268 or 5460 Antimony Oxide Cure: 20 hours ar 150"C
b) Nonburning
Tr4tm*ffc of fiofitn & Hot Co.
Parts by Weight
100 75 0.1 as indicated as indicated
Compres sive
Strength (psi) 43.000 32.500 32.900 32.400 39.150
Compres sive
Strength (psi) 23.400 36.500 41,700 36,700 40,700
*886050
TOWOLDMONOQ35151
In Polyester Resins
The highly chlorinated, less-volatile Aroclor compounds such as Aroclor 1260, 4465, and 5460, are very effective and economical fire retardants for polyester resins, and they do not significantly affect the physical properties of the resin.
The Aroclor plasticizers are effectively used in combination with equal amounts of antimony oxide, since the two materials are synergistic: Aroclor imparts self-extinguishing properties to the resin, and antimony oxide reduces afterglow.
Table 10 indicates the degree of flame resistance imparted to a generalpurpose polyester resin (with a 35 percent styrene content) by various equal concentrations of antimony oxide and one of these three Aroclor plasticizers.
TABLE 10
FIRE RETARDANCE IMPARTED TO POLYESTER RESINS BY AROCLOR AND ANTIMONY OXIDE
Antimony Oxide and Aroclor
1250
2.5% --
4465 --
5460 flammable
a) Formulation
5% semiflammable
flammable
self extinguishing 60 seconds
7.5% :semiflammable
self extinguishing
5 seconds ~~
10%
self extinguishing 30 seconds
self extinguishing
5 seconds
self extinguishing
5 seconds
15%
self extinguishing immediate'
self extinguishing immediate
self extinguishing immediate
Ingredients Polyester Resin (general purpose)
Styrene Methyl Ethyl Ketone Peroxide
(60% in dibutyl phthaiate) Cobalt Naphthenate (1% solution) Aroclor and Antimony Oxide
Weight Percent 62 35
2 1 as indicated
Inclusion of an Aroclor increases the flexural strength of the naturally brittle polyester and makes addition of a more expensive plasticizing polyester unnecessary. At a concentration of 10 percent (enough for fire retardancy), none of the Aroclor plasticizers reduced the flexural strength of the cure resin significantly (Table 11), and their effect was comparable to that of a plasticizing polyester. At 20 percent addition, they improved the impact strength, whereas the plasticizing polyester reduced it. The solid Aroclor plasticizers are preferred for fire-resistant surface coatings.
0509883
TOWOLDMONOQ35152
In Polyethylene In Polystyrene
TABLE 11
EFFECT OF AROCLOR ON STRENGTH OF FIBER-GLASS-REINFORCED POLYESTER RESINS
Plasticizer
Flexural Strength <%) fpsij
None 0 47,210
Plasticizing Polyester
10 20
43.310 39,930
Aroclor 1260
10 45,600 20 33,880
Aroclor 4465
10 40,740 20 33.390
Aroclor 5460
10 37,400 20 35.890
Flexural Modulus
fpsij
2.190,000
2.000.000 1,560,000
2.090.000 1,690,000
2.190.000 1.290.000
1,700.000 1,550,000
Impact Strength fft.-lbjin.)
1.73
1.64 1.24
1.33 2.04
1.41 2.48
1.85 3.06
The need to make polyethylene and other polyolefins flame retardant is well recognized. The well-known flame retardancy of the Aroclor products suggests their evaluation for polyolefin applications such as molded products, coatings, and hot-melt adhesives.
Preliminary evaluation of Aroclor 5460 (20 percent) and antimony oxide (10 percent) showed good results in imparting flame retardancy to low-density, noncrystalline polyethylene. Compared to the use of chlorinated aliphatic hydrocarbons, the use of Aroclor greatly improved the heat stability and had considerably less effect on tensile strength, yield, and elongation of the formulation.
The Aroclor products are good plasticizers for polystyrene. The lowermolecular-weight Aroclor plasticizers have greater solvating power than the higher-molecular-weight Aroclor products. The gelling rate of various plasticizers in polystyrene resin is shown in Table 12, each plasticizer was added to the polystyrene resin at a concentration of 2 parts plasticizer per part of resin, and the time required for the material to gel was noted.
TABLE 12
GELLING RATE OF PLASTICIZERS IN POLYSTYRENE
Plasticizer (200 p,hr)
Aroclor 1221 Diethyl Phthalate Dimethyl Phthalate Aroclor 1242 Sant/cizer 141 Santicizer 160 Sant/cizer B-16
HB-m
Time to Gel (min.)
immediate 0.6 0.75 2 3 6 18 30
Q5G9tttt6
TOWOLDMONOQ35153
In Polyurethanes 20
Aroclor products are useful as plasticizers and flame retardants in polyurethane rubbers, foams, adhesives and coatings. Having extremely low moisture content (50 ppm or less), the Aroclor plasticizers are useful in applications where low moisture is required. Other advantages exhibited by Aroclor in polyurethanes include resistance to oxidation, resistance to alkali and acids, improved adhesion, and low cost. The following formulation illustrates the use of Aroclor 1254 in a polyure thane flocking adhesive:
Part A Part B
Ingredients Muitranir FLD Urethane Resin Mondur* C Isocyanate Aroclor 1254 Muitranii FLD Mondur C
Parts by Weight 100 5 20 100 5-10
Part A is applied to the fabric by knife coating and allowed to dry thoroughly. The fabric is then coated with Part B, and the material is flocked immediately.
Protective urethane coatings are unusually well suited for application to concrete and metal. Aroclor 1254 is incorporated to improve ad hesion and sealing. The first of the following formulations is the preferred prime coat for concrete storage tanks for gasoline and fuel oils. The second formulation is the base coat for a concrete wood-kiln coating, which remained in perfect condition after two-and-one-half-
years' continuous exposure to heat, moisture, and wood distillates. The other two formulations, for primer and intermediate light-metal coating, contain Aroclor 1254 for better adhesion to metal.
Ingredients
.
High-
Unsealed Temperature
Concrete Concrete
Prime Coat Primer
(parts)
(parts)
Mondur C
19.0 12.0
Multron R-4 Polyester Resin
-
-
Multron R-10
10.0 12.0
Aroclor 1254
5.0 2.9
Polyvinyl Acetate
0.2
Polyvinyl Butyrar
- 0.4
Methyl Glycol Acetate
8.7 9.0
Butyl Acetate
8.7 5.4
Ethyl Acetate
8.7 4.0
Toluene
8.7 6.9
Pigment (colored)
12.5 -
Zinc Chromate Titanium Dioxide (rutile)
-- 15.0
Talc (micronized)
12.5 13.9
*Moll'*<iiloft4 Mondm: Motwr Chmiea1 Comvnj trtfwntik*.
Light-Metal Coating
Primer Intermediate
(parts)
(parts)
21.0 25.1
2.6 7.2
10.5 7.2
2.7 1.8
0.3 0.3
--
8.0 7.5
8.0 7.5 15.1 14.2
6.7 21.0
7.9 -
-13.2 5.5
o^87
C
c.
c
TOWOLDMONOQ35154
c In Phenolic Resins
Considerable interest has been shown in the use of Aroclor plasticizers
to make phenolic laminating resins flame retardant. The higher-
molecular-weight Aroclor products (1262 and 5460) are usually evalu
ated for this purpose.
Aroclor 1268 and 2565 are useful in the manufacture of brake linings.
Aroclor In Rubbers In Chlorinated Rubber And Chlorinated Polypropylene
Protective coatings based on chlorinated rubber generally contain Aroclor plasticizers to enhance their chemical resistance (to water, alkali, and acid), corrosion resistance, and electrical insulating proper ties and to impart flame retardance. When properly pigmented, they are unusually weather resistant. Aroclor compounds strengthen the adhesive grip of chlorinated-rubber lacquers, varnishes, and paints to structural materials and improve the flexibility and life of the coating. Typical applications include protective and decorative coatings for swimming pools, stucco homes, steel structures, tank cars, and both wood and metal maritime equipment. Their outstanding chemical resistance qualifies these coatings for use in manufacturing plants where chemical attack is prevalent. Aroclor 1254 and 1260 are used in chlorinated-rubber coatings as flexibilizing plasticizers, commonly in combination with Aroclor 5460, which serves as a resin fortifier. A r variety of suggested starting formulations based on chlorinated rubber is given in the following table.
ibm 21
TOWOLDMONOQ35155
Paints for Alkaline Surfaces
Ingredients
Fed. Spec. TT-p-m
('parts)
Concrete Maximum Acid White
Swimming andAlkali Marine
Poo! Resistance Paint
(parts)
(parts) (parts)
Parlon* {20 cp.) Chlorinated Rubber 18
10.2 18
20
Aroclor 1254
10 5.1 8
6
Aroclor 1260
---- 6 -
Aroclor 5460
6-
---
Long-oil, oxidizing, alkyd resin
--
-
6
Medium-oil, drying, alkyd resin - 5.1
---
Carbon Black
0.5 --
--
Iron Oxide
----
18
-
Titanium Dioxide
16 11.4
-- 25
Zinc Oxide
2--
----
Asbestine** 3X (magnesium silicate) -
11.7
--
--
Bentona*** 34 gelling agent
- 1.3 - -
Epichlorohydrin
- 0.1
0.09 -
Stabilizer
--
0.9 --
Solvesso*** 150
42.75 --
--
Solvesso 100
-- 8.1 45
--
Turpentine
4.75 ~ 5 --
Xylene
- 45.7
-- 23
Hi-Flash Naphtha
--
" 20
Aroclor compounds are also incorporated in chlorinated-rubber for mulations used for heat-sealing adhesives, electrical coatings, paper and textile coatings, and printing inks. The following starting formula tion is for an acid- and flame-resistant adhesive:
Ingredients____________________________ Parts by Weight
Chlorinated Rubber (125-cp. type)
20
Aroclor 1254
6
Aroclor 5460
6
Toluene
68
Chlorinated polypropylene, a new film-forming resin, produces clear, colorless films, appears equal to chlorinated natural rubber in chemical resistance, and is noticeably more heat and light stable. Aroclor is very compatible with the resin and is recommended in the following start ing formulations:
Ingredients
_____ ______________ Composition fwt. %)
Chlorinated Polypropylene
50.0*
Aroclor 5460
15.0
Aroclor 1254
24.0
Dioctyl Sebacate
4.3
Epoxy stabilizer
1.7
Solids, wt. percent in toluene
50.0
55.0* 15.0 24.0 4.3 1.7 50.0
ol HmuiIm In*. **!rdmikel lMrnHoi#ITle C*. MIrdnnrli NtliontllM*
ol Sltndod Oil CoaipMjt (N. I.)
' 0509889
c
c
TOWOLDMONOQ35156
300fbeat stability 1 hour 2 hours 3 hours 5 hours 18 hours
Film Properties
v. si. yellow v. si. yellow si. yellow mod. yellow black
v. si. yellow si. yellow mod. yellow
_
--
Fade-Ometar" stability 24 hours 48 hours 96 hours 144 hours
si. yellow si. yellow mod. yellow mod. yellow
v. si. yellow si. yellow $1. yellow brown
Two-waak chemicalresistance water 10% hydrochloric acid 1% sodium hydroxide
excellent excellent excellent
excellent excellent exceliant
a) Parlon P {10-cp, 20% in toluene) -- Hercules Inc.
b) Parlon P (20-cp, 20% in toluene) -- Hercules Inc.
c) Lacquers were sprayed on "bonderized" steel panels. Films were 2.5- to 3.0-mils thick after 72-hours' air drying.
|n Styrene-Butadiene Copolymers
Aroclor plasticizers are very often incorporated in coatings based on styrene-butadiene copolymers to impart resistance to acids, alkalies, moisture, and corrosive chemicals. These coatings are suited for use on masonry, wood, and metal for such applications as concrete floors; architectural finishes; metal primers and finishes on maritime equip ment, structures, and tank cars; baking primers; corrosion-resistant industrial films; and oil- and grease-resistant coatings.
The following suggested formulations for typical applications of styrene - butadiene - copolymer coatings offer excellent performance:
Ingredient
Clear Wall Aluminum Vehicle Sealer Enamel Paint (wt. %) (Ib.HOOgal.) fwt.%) fib.)
Traffic Paint (parts)
Styrene-Butadiene Aroclor 1254
16.60' 8.39
123.2' 41.4
7.40' 147' 250* 6.00 -- 120'
Aroclor 1260
- -- -- 31 -
Aroclor 5460
9.11 41.4 13.40 - 130
Raw Tung Oil
1.655 -
-- ---
Hydrogenated Methyl Abietate -- -- -
8--
Troykyd* ABC
----
3-
Lecithin
0.545 -
-- --
Soya Lecithin
--
5.9 -
----
Petroleum Naphtha
62.70 246.4
--
---
Hi-Flash Naphtha
-- - - 395 -
Mineral Spirits No. 10
- 185.3 33.60 -- 340
Toluene
-- - -- -- 34Q
Xylene
- - 22.40 - -
`Tiidtmaili erf Aim Electric DevkwCo. el Trey Chrmcl Co.
0509890
23
TOWOLDMONOQ35157
Lithopone Titanium Dioxide Aluminum Stearate Aluminum Paste Zinc Oxide Barium Sulfate Asbestine 3X (magnesium silicate) Calcium Carbonate, ground Diatomaceous Earth Mica
-- -- -- -- -- -- -- -- -- --
339.3
-
-
59.2 ' -
179
5.9 _
--
-- 8.55 -
-- -- 60
-- -- 90
75.0 -
--
-- _ 236
- - 76
8.00 30
b) Marbon "9200" MV (Trademark of Marbon Chemical Div., Borg-Warner Carp.)
b) Pliolite S-5A (Trademark of Goodyear Tire and Rubber Company) c) Marbon "9200" LV (Marbon Chemical Div., Borg-Warner Corp.)
d) Raked Piccoflex 120 (Trademark of Pennsylvania Industrial Chemical Corp.)
e) Pliolite S-5B (Goodyear Tire and Rubber Company)
IJ or Aroclor 1248
-
-
-- -
-
-
Jn Synthetic And Natural Rubbers
________________________________________ _
The liquid Aroclor plasticizers -- 1221,1232,1242, and 1248 -- have a strong plasticizing action on both natural and synthetic rubbers. Solid Aroclor --1254 and 1260 -- imparts permanent tackiness and adhesion to the rubber composition.
Neoprene
Compositions containing up to 40 parts of Aroclor 5460, 2565, 4465, or 1268 in 100 parts of neoprene rubber are extremely fire retardant. About 1.5 parts of Aroclor 1268 per hundred parts of neoprene imparts excellent working qualities at 225 to 325 F for injection moldings. Neoprene modified with Aroclor compounds has proved extremely
useful as a wire and cable coating.
Aroclor 5460 imparts plasticization and adhesion to decorative and protective coatings that have been commercially used on rubber products for many years. Suggested starting formulations for a clear, dull coating and for three pigmented coatings are as follows:
Ingredients Aroclor 5460 Neoprene GRN-10 Chlorinated rubber (21 cps.) High-styrene resin Isobutyl methacrylate Toluene
Parts by Weight
dear, dull coating
base for
pigmented coatings
3.70 16.00
3.50 8.00
1.30 _
1.00 4.38
0.40 1.75
90.10 69.87
9
05Q9B91
TOWOLDMONOQ35158
Ingredients Paste:
Base Chromium Oxide Zinc Oxide No. 3 Titanium Oioxide Aluminum Hydrate Toiuene
green coating
20.0 ' 6.4
3.6 10.0
white /high gloss)
43.0 10.5 15.0 31.5
white fluster modifier)'
29.0 25.0 52.0
Resiy-to-Use Coating:
Base Paste
60.0 70.0 40.0 30.0
* *
*To modify the luster of the white, high-gloss coating, the selected amount of the modifier composition is in corporated into the high-gloss paste to achieve the desired degree of flatness.
Roiybutena
Aroclor plasticizers and Indopol* polybutenes are blended in various proportions to make permanently tacky coatings for fabric or paper. Insecticides, for example, can be blended into such coatings to make insect traps or barriers on tree trunks for foliage or fruit protection. Such coatings can also be used for tape and sign backing.
Excellent sealing and caulking compounds are made with blends of Aroclor and polybutenes with inorganic fillers, such as:
Ingredient Whiting Talc Lithopone Asbestos
Percent 50 30 10 10
By various combinations of selected Aroclor compounds and poly butenes, a wide range of hardness, viscosity, flow, and bonding charac teristics can be produced in durable sealing and caulking compounds.
Specialty mastics, too, are obtained by selective blends of Aroclor plasticizers with polybutenes. They have excellent adhesivity for such uses as automobile-body sealants.
*Tiidmrk ol Amoco Chemical* Carp.
OiO 98?g
25
TOWOLDMONOQ35159
Paper-transparentizing liquids (for making tracing paper, window envelopes, and special packaging) can be formulated with Aroclor 6460 and polybutenes. A typical economical formulation is as follows:
Ingredient
Percent
Aroclor 5460
30
Polybutene (//M/0/70/H-300)
25
Toluene
45
Butadiene-Acrylonitrile Rubber
The Aroclor plasticizers -- particularly Aroclor 5460 -- are useful as
softeners for Buna N rubber.
.
Silicone Rubber Aroclor is a very effective flame retardant for silicone rubbers.
Crepe Rubber (Natural)
Aroclor 1262 is used as a low-cost plasticizer for crepe rubber in paint
compositions. In concentrations of from 5 to 50 per cent of the weight
of the rubber, the Aroclor increases the films alkali resistance, and
adhesivity to steel.
-
Polysulfide Rubber
Aroclor plasticizers are widely used to flexibilize, improve the bond ing strength, increase the chemical resistance, and reduce the cost of Tkiokol* polysulfide liquid rubbers. Among the many uses of poly sulfide formulations are joint-sealant compounds used in construction, solvent-resistant gaskets, adhesives for concrete, potting and encap sulation, protective coatings, and binders.
Although the Aroclor plasticizers are highly compatible with poly sulfide rubbers -- up to 100 phr -- the concentration to be used depends on the handling and performance properties required in the finished compounds. Suggested concentrations of Aroclor range from about 15 phr for sealant compounds to about 40 phr for casting formulations.
Liquid Aroclor (such as Aroclor 1248) is used to reduce the viscosity and permit the use of higher filler concentration, whereas the solid Aroclor (such as Aroclor 5460) is useful where low volatility is desired.
The following suggested starting formulations illustrate the use of Aroclor 1232 in a joint sealant compound and of Aroclor 1248 in a polysulfide casting formulation:
*Tridtmrk d ThtoW Cixmtul Cmp.
0509893
TOWOLDMONOQ35160
Ingredient Thiokoi LP-32 polysulfide Thiokoi LP-2 polysulfide Aroclor 1232 Aroclor 1248 Calcium Carbonate Calcined Clay Titanium Dioxide Phenolic Resin Stearic Acid Zinc Sulfide Sulfur C-5 Paste'
Sealant (parts)
100 5-15
20 20 10 5 1 0.1 15
Casting Compound
(parts) 100
-
20 40
-
-
-
-
40 0.1 15
Property
Cast sheets, after cure of 7 days at room temperature:
Tensile strength, psi
150-200
Elongation, percent
500-700
Hardness, Shore "A"
30-40
150-200 300-400 25-35
a) lead peroxide, 50%; dibutyl phtbalate, 45%; stearic acid, 5%: passed three times through a tight paint mill.
Aroclor In Cellulosic Resins
In Ethyl Cellulose
Ethyl cellulose formulations plasticized with Aroclor are used as pro tective lacquers, adhesives, and strippable coatings. The solids, such as Aroclor 5460, are widely used with ethyl cellulose or cellulose acetate-butyrate resins in hot-melt applications for the protection of tools and metal parts.
The Aroclor plasticizers are highly compatible with ethyl cellulose: the liquid Aroclor imparts flexibility; the solids impart hardness. For example, 75 parts of Aroclor 1242 with 100 parts of ethyl cellulose produces a very flexible, slightly tacky material. Aroclor 5460 at the same concentration yields a very hard, somewhat brittle composition. Hard films that contain Aroclor 4465 are not brittle at ordinary temperatures.
For high-gloss coatings with exceptional weathering qualities to be applied to rigid surfaces, compositions containing equal parts by weight of Aroclor 5460 and ethyl cellulose are suggested. When a more flexible coating is required, a softer Aroclor should replace either all or part of the Aroclor 5460.
0309894
27
TOWOLDMONOQ35161
In Nitrocellulose
The following five typical formulations indicate the versatility of various Aroclor plasticizers in compounding for widely different types of applications. They are intended as guides to the use of Aroclor compounds with ethyl cellulose.
Ingredients
Lacquer (parts)
Ethyl Cellulose
50
Aroclor 1254
-
Aroclor 1260
60
Aroclor 5460
-
Dow 276, V-9
-
Octylphenol
-
Stearic Acid
Rutile Titanium Oxide
-
Epoxy Resin
-
Santonox Antioxidant
-
Mineral 0i)
-
Castor Oil
-
Epoxidized Soya Oil
-
Paraffin Wax (m.p. 135*F) -
White AlkaliResistant Lacquer (parts)
25 16
76
1
50 1
-
-
-
Liquid Adhesive (parts)
so 40 6 2
-
Strippabfe Coating (parts)
49 49 -
1 1 -
-
Hot-Melt Adhesive
(parts) 24
7 1 67 5 3 3
The first four of these formulations may be dissolved in suitable solvents, such as mixtures of about four parts of toluene to one part of butanol, to obtain the desired viscosity.
In nitrocellulose lacquers, the Aroclor compounds can function either as plasticizers to modify the properties of the film or as resin extenders to add film-forming body. They are highly compatible with nitro cellulose and with other resins and plasticizers commonly used in lacquer formulations. They impart weather resistance, luster, adhesion, and flame retardance. Their excellent electrical characteristics and their ability to retard the passage of moisture and gases through nitrocellulose films make the Aroclor compounds especially valuable in coatings for electric-insulating materials.
The following trilinear diagrams (Figure 1), show the limits of practical compatibility of Aroclor 1254, 1260, and 1262 when used in nitro cellulose lacquers in combination with some other resins or plasticizers. The less viscous Aroclor plasticizers (1242 and 1248) are more com patible than those shown; the more resinous Aroclor (1268, 2565, 4465, 5442, and 5460) is less compatible. In these trilinear diagrams, compositions represented by any point in an unshaded area produce homogenous nitrocellulose-lacquer films. On the other hand, compositions represented by points in the shaded areas produce impractical (segregated, brittle, or soft) films.
0509895
TOWOLDMONOQ35162
3 Fig. 1 -- Limits of Practical Compatibility of Aroclor in Nitrocellulose Lacquers
100 ->
NITROCELLULOSE, %
50 AROCLOR
1254 or 1262,% 60
100 90 80 70 60 50 40 30 20 10 0 ESTER GUM RESIN, %
NITROCELLULOSE, %
100 -*<
AROCLOR 1260 or 1262,%
NITROCELLULOSE, %
100 90 80 70 60 50 40 30 20 10 0 PHTHALIC ANHYDRIDE-GLYCEROL RESIN, %
3 100 90 80 70 60 50 40 30 20 10 0
PHTHALIC ANHYDRIDE-GLYCEROL RESIN, %
0509896
TOWOLDMONOQ35163
Fig. 1 (Continued)
Q
AROCLOR 1260 or 1262, %
The following formulations are given to illustrate modifications that can be obtained by variations in composition. They all have excellent durability, but the first two are much harder and less flexible than the third. The first two also have excellent sanding and polishing qualities, but No. 3 is too soft for sanding. The cable lacquer (No. 4) has ex tremely high flexibility, as required for high-tension automobile cables.
0509897
TOWOLDMONOQ35164
Ingredient Nitrocellulose (% sec.) (wet) Nitrocellulose (Vi sec.) (dry) Nitrocellulose (15-20 sec.) Aroelor 1242 Aroelor 1260 Aroelor 5460 Dibutyl Phthalate Tricresyl Phosphate Damar Resin Ester Gum
No. 1 (ports)
100 -
--
20-39
--
20-0 80
--
No. 2 (parts)
100
-- 20
--
20
-
--
80
No. 3 (ports)
~ 100 -- 80-70 --
-
39-70
--
--
No. 4 Cable Lacquer (parts)
-- 100
80 -- -- 120
--
--
No.S Chrome lacquer (parts)
100
-
--
-
47 32.5
-
In Cellulose Acetate-Butyrate
The high-chlorine-content Aroelor plasticizers are highly compatible with cellulose acetate-butyrate and are widely used in the manufacture of low-cost, flame-resistant lacquers. Typical uses for these products include paper coatings, lacquers for plastics, strippable coatings for paint booths, and hot-melt adhesives. Typical starting formulations, illustrative of these uses, are suggested as follows:
Ingredients
Paper Lacquers
Low-Cost
Flame
Cur!
Resistant Resistant
(wt. %)
(wt. %)
Clear Wood Filler (wt. %)
Half-Second Cellulose Acetate-Butyrate
20 20 7
Aroelor 1260
- 20 -
Aroelor 1262 Aroelor 5460
15 '_
--
-- 15
Diocty) Phthalate Epoxy Soybean oil
-_ --
Acrylic Resin
- ---
Dow 276. V9
- --
Socony Vacuum 200
- ---
"NewportW* pine resin Acetone
- -10 -
Methyl Ethyl Ketone
- ----
Methyl Osobutyl Ketone
- ---
Isobutyl Acetate
5 10 22
Ethanol
12 10 --
Butanol Isobutanol
---5 ~ --
Toluene Santonox Antioxidant Syn Fleur No. 6 odorant Asbestine X (magnesium silicate)
48 -- -
30 6 ---
- 45
a} Coatings for cellophane, cellulose acetate, and cellulose acetate-butyrate.
Plastics* Lacquer (wt. %)
6 1.5 -- --
-
-- 2.5 1.5 10 5 33.5 25 15 -- -
-
Paint-Booth Strippable
Coating (wt. %)
20
-
-
9 9 9.5
-
-
2.5 10 5 10
-- 25
-
.-
Hot-Melt Adhesive (wt. %)
35 -
-
30 15 19.89 0.1 0.01
-
Mudimtikol H*wpO(tlAdultrin Co.Dr*. ot K,dan NKpoflChniK1Cttp.
000<J<*98
31
TOWOLDMONOQ35165
Aroclor In Paint, Varnish, Wax, Asphalt In Paint And Varnish
Aroclor is soluble in paint and varnish oils and solvents and compatible with most film-forming coating resins. The Aroclor plasticizers improve adhesion to the substrate and impart to the film properties that correspond to the particular character of the Aroclor used: the hard, resinous Aroclor tends to give increased hardness; the viscous Aroclor imparts flexibility.
Aroclor 4465 and 5460 produce paints that are very quick drying and yet have excellent durability. The amount of Aroclor used may be from 30 to 50 percent of the weight of the oils.
Aroclor 1260 is best for short-oil varnishes that are required to be flexible. The Aroclor plasticizers impart water and alkali resistance and also enhance the value of the other resins used in the varnish. A sug gested starting formulation is two parts of oil, one part of Aroclor 1260, and one part of other resin. These proportions can be varied as required. The Aroclor may be considered to play the same role in the varnish formulation as oil, except that it does not oxidize and lose its flexibility on exposure.
The Aroclor plasticizers do not react chemically with oils, hence there is no advantage in heating together in making a varnish. They are best added as a "chill back" or as a cold cut in the thinning operation. The only reason to heat the Aroclor is to fluidize it so that it can be more readily mixed with the oils. Alkyd, phenolic, or ester gum resins, with a harder Aroclor such as 5460, may be used in making varnish formulations. To illustrate the use of Aroclor plasticizers in alkyd resins the following suggested starting formulation is shown.
' Ingredients Alkyd (60% Nonvolatile) Kettle Bodied Linseed Oil (Gardner-Hoidt Vise. Z-2) Raw Linseed Oil Aroclor 5460 Titanium Dioxide (Rutile) Titanium Dioxide (Anatase) Magnesium Silicate Mineral Spirits Drier-Absorption Agent Penyl Mercury Naphthenate (10% Mercury) Cobalt Naphthenate (6% cobalt) Lead Naphthenate (24% lead) Antiskinning Agent (Volatile type)
Parts by Weight 81 20 35 34 34 67 100 38 1.3 2.7 1.5 3.2 0.67
0509699
TOWOLDMONOQ35166
The following suggested starting formulation for a fire-retardant enamel illustrates use of the flame retardancy of an Aroclor in alkyds:
Ingredients
Parts by Weight
38% Phthalic Anhydride-Soya Alkyd
63
Aroclor 5460 Solution (Aroclor 5460, 53; Hi-Flash Naphtha, 22)
75
Whiting
84
Colloidal Grinding and Dispersing Agent
2.7
Antimony Oxide
. 42
Titanium Dioxide (Rutile)
33
Grind above ingredients, and thin with: 38% Phthalic Anhydride-Soya Alkyd Yylene Cobalt Naphthenate (6% cobalt) Manganese Naphthenate (6% manganese) Lead Naphthenate (24% lead)
96 38 1 1 2.3
Aroclor plasticizers are excellent grinding and dispersion media for pigments used in paints and varnishes. Aroclor 1254 is used to disperse aluminum powder in a paste form that can be incorporated easily into paints and varnishes. The Aroclor imparts excellent leafing qualities, brightness, or luster and does not tarnish the aluminum pigment on aging. Moreover, the composition does not support combustion.
Aroclor is an important ingredient of heat-resistant aluminum paints and enamels that contain silicone resins. For example, the following suggested formulation for a heat-resistant coating can withstand a maximum temperature of 800 F and continuous-service temperature of 400 F. The heat-resistant enamel can withstand temperatures of 900 to 1000 F in such applications as jet-engine components, exhaust manifolds, and incinerators. The heat-resistant paint has excellent resistance to a programmed heat test, including 8 hours at 1200 F, and to salt-water spray after programmed heating to 500, 600, and 900 F.
0509900
33
TOWOLDMONOQ35167
In Waxes
"Dow Corning 80S"* Resin (50% Nonvolatile)
G E Silicone Resin SR-82 (60% in xylene)
G E Silicone Resin SR-112 . (50% in xylene)
Styrene-Butadiene (50% in xylene) (PHoiite S-5B)
Aroclor 4465 (90% nonvolatile)
60% Aroclor Solution (Aroclor 4465, 36 wt. %) (Aroclor 1262, 24 wf. %) (StoAwso 100, 24 wt. %) (Xylene, 16 wt. %)
Aroclor 5460 (60% in xylene)
Aroclor 1254
Aluminum Paste (74% nonvolatile)
Cobalt Octoate (6% cobalt)
Xylene
Mineral Spirits
a) Meets Spec. TT-P-002S
Heat-Resistant Coating
(Ib.lJOO gal.) 220
.--
--
~ 332
-
-
384
--
114 -
Heat-Resistant Enamel
(ib.1100 gal.) --
174.2
313.3
--
--
435.6
-- -- 250.0 4.4 _
-
Heat-Resistant Paint*
(tb.ilOO gal.) -- 93.6
-- 207.9
-
93.6 47.8 240.0
_
140.8 113.1
The Aroclor plasticizers, especially 5460, are compatible with various natural waxes, and are blended with waxes for many uses, including "lost-wax" casting, impregnating compounds, and inexpensive sealers. Waxes formulated with Aroclor are nontacky and stable.
Much of the highest quality precision-casting wax used in the `lostwax" process is formulated with Aroclor, most frequently 5460, 4465, and 1254. Waxes containing Aroclor are widely used in making dental castings, costume jewelry, and precision-cast aircraft parts.
Usually from one-fourth to one-half the composition consists of Aroclor 5460, which contributes these desirable properties to the formulation: hardness without brittleness, shrinkage resistance, sharp definition, sharp melting point, fire resistance, low volatility, and volatilization without carbonization during final curing.
Excellent impregnating compounds to prevent sticking of furniture drawers, double-hung windows, etc. are made from selected Aroclor plasticizers, such as 5460, and various waxes. Combinations of resinous Aroclor with waxes make excellent and inexpensive sealers for masonry, wood, fiberboard, and paper.
Aroclor imparts moisture and gas resistance, adhesion, alkali and chemical resistance, flame resistance, lubricity, and insulation to impregnants for cloth, paper, wood, and asbestos. They are combined with such materials as waxes, asphalt, tars, sulfur, aluminum stearate, and inorganic pigments so as to provide exactly the physical charac teristics required for the specific purpose. Aroclor 1254, 4465, and 5460 are suggested as most applicable.
'Tftdtmi'k ol DowCwnkiiCorp.
'-
c c c
TOWOLDMONOQ35168
In Asphalt In Allyl Starch
Wood is decidedly toughened, hardened, and made more moistureresistant when impregnated by the vacuum-pressure method with the following mixture:
Ingredients Aroclor 4465 Microcrystalline Wax Sulfur
Per Cent 70 20 10
The coating is very resistant to acids and alkalies but can be attacked by aliphatic, aromatic, or chlorinated hydrocarbons. The paintable surface is not appreciably discolored. Various degrees of hardness and adhesion are obtained by variations in the proportions of the ingredients.
Blends of Aroclor 1268 and 1242 have the unusual capability to extend carnauba wax satisfactorily and at an attractive saving in cost:
Ingredients Aroclor 1268 Aroclor 1242 Carnauba Wax Ceresin Wax Paraffin Wax
10 5 S 20 60
Parts by Weight
19.6 30
35
4.9 5
5
6.6 10
30
19.6 20
20
49.0 35
10
36 5 50 10 -
Characteristics Color
Texture
Pale Yellow, White
Smooth, hard,
non-tacky
Softening point, *C Melting point, *C
60 78
Pale Yellow
Smooth, hard,
non-tacky
77 79
Pale Yellow
Smooth, hard, slightly brittle
78
78
Pale Cream
Slight surface crystallinity
79 86
Cream
Smooth; carnauba*
ringed surface
80.5 88
Self-extinguishing asphalt formulations for caulking, roof coatings, and sound-deadening coatings are obtained by incorporation of at least 30 percent Aroclor 5460 or other solid, resinous Aroclor.
Substitution of the hydroxy hydrogen atoms of the starch molecule by allyl groups produces allyl starch, which upon polymerization forms stable, cross-linked molecules. A minimum of 20 weight-percent plasticizer is required to make the film flexible. The aroclor plasticizers are highly compatible and very efficient plasticizers for allyl starch.
0309902
3? L
35
TOWOLDMONOQ35169
Miscellaneous Applications Of Aroclor
With their wide range of physical properties, their inertness, lubricity, - and low vapor pressures -- Aroclor plasticizers are valuable ingredients
in an incredible variety of formulated products. They are compatible with many solvents and oils and most resins. They are virtually non volatile and permanently thermoplastic; they do not react with other chemicals in the formulation. Finally, their low cost makes their use for special purposes eminently practical and economical.
Dust Prevention And Dust Catching
Aroclor 1254 is a low-cost dedusting agent that "holds down" the dusting of a variety of chemical materials. Since Aroclor 1254 resists both oxidation and combustion, it can even be used to control the dusting of highly reactive compounds. As a typical example, a few tenths of a percent controls the dusting of calcium hypochlorite.
Since Aroclor is non drying and tacky, it makes excellent coatings to capture dust, lint, and other fine, airborne particles. Glass fiber, metal mesh, and other materials used to filter air and gas streams are coated with Aroclor 1260 and 5460.
Vapor Suppression (For Longer Insecticide Kill-Life)
...... Moisture Proofing
The effective kill-life of expensive chlorinated insecticides is extended as much as ten-fold by the incorporation of equal parts of Aroclor 5460, which acts both as a vapor suppressant and as a sticking agent. Hard surfaces (painted or metallic) sprayed with lindane or benzene hexachloride fortified with Aroclor 5460 remain toxic to flies, ants, roaches, and silverfish for as long as three months, compared with one week for unfortified sprays.
The Aroclor retards the rapid evaporation of the volatile insecticides without adding odor or objectionable residue. Formulation into an insecticide is simple: a solution of the Aroclor in a suitable solvent is merely added and mixed into the other ingredients.
Aroclor 5460 is also recommended for noncrop insect formulations containing chlordane, aldrin, and dieldrin. The other resinous Aroclor products (1254, 1260, 1262, 4465, and 5442), also nonvolatile and sticky or tacky, likewise merit evaluation as insecticide extenders.
In moisture-proof coatings for wood, paper, concrete, or brick, Aroclor is best combined with waxes, especially paraffin or camauba; oils such as mineral oil or drying oils; or synthetic resins, including modified alkyds, phenolics, chlorinated rubber, polystyrene, styrene-butadiene copolymers, ethyl cellulose, cellulose acetobutyrate, benzyl cellulose, or vinyl resins. The material to be used with the Aroclor should be selected according to the end-use requirements of the specific ap plication.
Some very simple compositions contain only Aroclor and paraffin. One very efficient moisture-proofing compound, consisting of 96 weight percent Aroclor 5460 and 4 percent paraffin (melting point 54C), has
C
0*09903
TOWOLDMONOQ35170
an ASTM softening point of about 82C. A similar compound, based on Aroclor 4465, has a softening point of about 58C.
Softening point and viscosity when melted are further decreased by the use of mixtures of Aroclor. For example, a composition containing 40 percent Aroclor 1260, 56 percent Aroclor 5460, and 4 percent paraffin, is veiy soft at room temperature. A higher concentration of paraffin also produces softer compounds.
An excellent melt coating for paper and cloth, made according to the following suggested formulation, may be applied by knife or roller at 350F, requires no solvent, and provides an extremely flexible coating.
Ingredients Half-second Cellulose Acetate-Butyrate Dioctyl Phthalate Aroclor 1260 Santonox antioxidant
Percent 50 9.9 40 0.1
Pigment Dispersion
Aroclor 4465 is a useful resin in rotogravure and other printing inks. It is an important ingredient in the following mimeograph ink suitable for use on bond paper:
Ingredients
Aroclor 4465 Lubricating Oil (SUV 1200 @ 100'F) Paraffin Oil (SUV 76 @ 1007) Carbon Black Oil-Soluble Dye
Percent 40 35 20 4 1
Aroclor 4465 is also used in the preparation of imitation gold leaf. Bronze powder is spread upon a hot coating of Aroclor on one side of a sheet of paper. When the paper treated with Aroclor and bronze powder is placed on the object to be imprinted and a hot die is pressed against it, the Aroclor softens, sticks the bronze to the object, and coats the powder to prevent tarnishing.
Aroclor 1254 and 4465 serve as pigment vehicles for decoration of glass and ceramics. When the decorated object is fired, the Aroclor volatilizes without carbonization and thus avoids discoloration. Aroclor plasticizers are also valuable as grinding and dispersing mediums for pigments used in plastics.
Sealing And Impregnation
________
The liquid Aroclor plasticizers, 1221 and 1254, because of their low vapor pressures and fire resistance, are excellent sealants. These non evaporating fluids have good flow at slightly elevated temperatures and are chemically stable at elevated temperatures. These liquid Aroclor products therefore are excellent fluid seals wherever the use of oil would create a fire hazard. In the trough of annealing furnaces, for example, Aroclor plasticizers are dependable, fire-safe roof sealants.
050990*
TOWOLDMONOQ35171
Because of their nonflammability, high resistivity and dielectric strength, and low power factor, the liquid and resinous Aroclor plasti cizers are extremely valuable impregnants for many electrical applica tions. One important use of Aroclor 1260, 4465, and 5460 is in wire and cable coatings and as impregnants for braided cotton-asbestos insulation. Their high purity and excellent electrical resistance make Aroclor 1254, 5460, and 1268 excellent dielectric sealants: to close the pores of carbon resistors, and to seal electrical bushings and terminals.
Aroclor plasticizers are essential components of coatings for flame proofing cotton drill for outer garments and for rendering olive-drab canvas fire-retardant, water-repellent, and rot-proof for tents, tar paulins, etc., according to the following formulations:
Flameproofing Formula for Cotton Drill
Ingredients
Parts by Weight
(A) Urea-formaldehyde resin monomer . 9.62
Catalyst for resin
0.40
Water
22.26
(B) Oil-modified alkyd resin Aroclor 1254 Aroclor 5460 Stoddard solvent
3.89 12.00 14.40 25.15
(C} Antimony oxide, 300 mesh or finer
12.28
Dissolve the solids in the indicated solvents, add the aqueous solution (A) to the hydrocarbon solution (B) with stirring, and then disperse the antimony oxide in the emulsion.
Fire-Retardant, Water-Repellent, Rot-Proof Canvas Coating
Ingredients
Per Cent
Modified phenol-formaldehyde resin
4
Aroclor 1254
16
Aroclor 5460
4
Antimony Oxide
8
Tricresyl Phosphate
1.5
Aluminum Stearate
0.5
Copper Naphthenate (8% copper)
8
Mica, ground
3
Limestone, ground
6
Iron Oxide, yellow
7
Chrome Orange
2
V M & P Naphtha
40
C
c c
0509905
TOWOLDMONOQ35172
Properties Of The Aroclor Plasticizers Mobile Liquids Viscous Liquids Soft Resins Brittle Resins
Solubility
Numerous applications for the Aroclor plasticizers have been suggested and described in the preceding sections of this bulletin. Their success depends on the general Inertness of the compounds and on the range and gradation of their physical properties, including physical state, density, viscosity, melting and boiling points, volatility, and solubility. These and other properties, as well as handling and shipping informa tion, are presented in detail in the remainder of the bulletin.
The Aroclor liquids and resins are readily soluble in most common organic solvents and drying oils. Although all Aroclor plasticizers are insoluble in water, the hard, crystalline materials are generally less soluble than the liquids and softer resins. Solubilities of some Aroclor plasticizers are shown in Table 13.
050990b
39
TOWOLDMONOQ35173
fc.
o
TABLE 13
SOLUBILITIES OF AROCLOR PLASTICIZERS IN VARIOUS SOLVENTS
Solvent
Acid Acetic Acid Oleic Acid Benzoic Acid
Aroc/or 1242 25'C Hot
S S 10.031"c
s
s --
Arocfor 1248 25'C Hot
-- 10.032C
_ --
Aroclor 1254
. 25'C
Hot
ss
ss ----
Aroclor 1268 Cold Hot
__ ---- --_
Aldehyde 40% Formaldehyde Furfural
1 1 1 11 1ii VS vs VS vs vs vs ss ss
Amine Aniline Pyridine
ss
132.5"': 44Q99C
--
-s
s-
- 1143,c 425ioo*c -
--
Chioro derivatives
Amyl chlorides -- mixed S s s s s s -- . --
Carbon Tetrachloride
s
s
s
s
s
s ----
Chloroform
s s s s s sss
Dichlorethylene
-- --------------
Ethylene Dichioride s s s s s s s s
Monochlorobenzene
s
s
s
s
s
s
----
Orthodichlorobenzene
-
--
--
--
--
------
Tetrachlorethane
s s s s s s ----
Trichlorethane
s s s s s s ----
Trichlorethylene
s s s s s s ----
Drying Oil Tung Oil Linseed Oil
s s s s s s ---- ssssss 1s
Ester
Amyl Acetate
s ss sssss
Butyl Acetate
s ss ss sss
"Cellosolve"* Acetate
s
s
s
s
s
s
----
Cottonseed Oil
s s s s s s ----
Dibutyl Phthalate
s sssssss
Aroclor 4465 Aroclor 5460 Cold Hot 25'C
ss s s vs ----
-- --
1 1-- vs vs -
vs vs vs vs -
vs vs -
vs vs 156
vs vs
-
vs vs
--
vs vs --
vs vs --
vs vs --
vs vs
--
vs vs --
vs vs -
vs vs -- vs vs --
vs vs
--
vs vs --
vs vs -
s vs --
s vs -
0509907
TOWOLDMONOQ35174
o
TABLE 13
SOLUBILITIES OF AROCLOR PLASTICIZERS IN VARIOUS SOLVENTS
Solvent
Acid Acetic Acid Oleic Acid Benzoic Acid
Aroclor 1242 25'C Hot
s s
10.03,*c
s s
--
Aroclor 1248 25'C Hot
_
-- 10.0M'C
-- -
Aroclor 1254
t.l25'C
Hot
ss Ss
----
Aroclor 1288 Colt! Hot
__
---- ----
Aldehyde 40% Formaldehyde Furfural
1 1 1 1 i 1 i i vs vs vs vs VS vs ss ss
Amine
Aniline Pyridine
s
132.530"c
s
44039*C
--
-s s-- -- 114311 425iooc --
--
--
Chioro derivatives
_ _Amyl chlorides -- mixed
S
s
s
s
s
s
Carbon Tetrachloride
S
s
s
s
s
s ----
Chloroform
ssssssss
Dichi orethytene
---- --"--------
Ethylene Dichloride
s
s
s
s
s
s
s
s
Monochlorobenzene
s
s
s
s
s
s ----
Orthodichiorobenzene
--
--
--
--
--
--
--
--
Tetrachlorethane
s s s s s s ----
Trichlorethane
s s s s s s -- --
Trichlorethylene
s s s s s s ----
Drying Oil
Tung Oil
Linseed Oil
ssssss
_.
ssssss 1s
Ester
Amyl Acetate
s s s s s s s s
Butyl Acetate
ssssssss
"Cellosolve"* Acetate
s
s
s
s
s
s ----
Cottonseed Oil
s s s s s s ----
Dibutyl Pluhalate
ssssssss
Aroclor 4465 Cold Hot
ss s s vs
----
Aroclor 5460 25'C
'
--
-
11 vs vs -
vs vs vs vs -
vs vs _
vs vs 156 vs vs -- vs vs vs vs -- vs vs -- vs vs -- vs vs -- vs vs vs vs --
vs vs vs vs -
vs vs vs vs vs vs s vs s vs --
cs TOWOLDMONOQ35175
0066050
' i'r'
Diethyl Phthalate
s s s s s s -- -- s vs -
Ethyl Acetate
s s s s s s SS SS s vs -
Ethyl Lactate
, s. s s s s s 1 s vs vs -
sEthylene Glycol Diacctate s s s s s -- -- vs VS --
Methyl Acetate
S s s s s s SS SS s s --
Tricicsyl Phosphate
s
s
s
s
s
S -- -- SS s --
Ether: Ethyl Ether
s s s s 4: s s s s s -- --
Ether Alcohol Carbitor
2243rc
30799T
vs
VS
.1732G"
25998-c
1
s SS _ _
Cellosolve
S s s s s s 1 s s ----
Diethylene Glycol
s-- -- -- -- -- -- -- --
----
^.p'-Oihydroxy Ethyl Ether 16.923c
1939-C
SS
SS
g3Q*C
1qiqqc
--
--
SS
--
--
Hydrocarbon Benzene Gasoline Kerosene Mineral Spirits Paraffin Pine Oil Tofuene Turpentine Xylene
VS vs vs vs vs vs s
s VS vs 143
vs VS vs vs vs VS -- -- vs vs --
vs vs vs vs vs vs SS s vs vs -
vs vs vs vs vs vs s s vs vs -
s s s s2.0-5^
2.028-C
--
-- -- 5.0
-
S s vs vs s s s s s s -
VS vs vs vs vs VS s s vs vs 142
VS vs vs vs vs vs s s vs vs -
VS vs vs vs vs vs s s vs vs 178
Hydroxy derivatives Amyl Alcohol
ss
_ s s SS s s s _
/7-Butyl Alcohol
s s - - s s 1 SS SS s -
Ethyl Alcohol (3-A)
23.328*c
80.0*TM
--
--
10!rc
28-c
1
1 SS -- --
Glycerine Methyl Alcohol Phenol -- 90% Ketone: Acetone
1 1 1 1 1 1 1 1 1 1-
42.523c 88.5C<TM
--
--
15!6"C
22.265-c
--
--
SS
--
--
1943'c
s
-- -- SS s SS s
S
s-
s s -- -- s S 1 1 S s 260
Miscellaneous Carbon Disulfide
Nitrobenzene
ss
_ s s s s vs vs
s s -- -- s s -- -- vs -- --
Water
1 1 1 1 1 1 1 1 1 1-
I --Insoluble SS -- Slightly Soluble S --Soluble VS -- Very Soluble.
.
Figures show grams of Aroclor per 100 milliliters of solvent at 25*C unless otherwise indicated.
'T'ltfcfNifc*! Vnta Cl't'ticCo'p.
ObbOSO
4k
TOWOLDMONOQ35176
Q
Diethyl Phthalate
S s s s s s -- - s vs
Ethyl Acetate
s s s S s s SS SS S vs
Ethyl Lactate
S s s S s s 1 s vs VS
sEthylene Giycol Diacetate s S s s s -- -- vs vs
Methyl Acetate
s s s s S s SS SS s S
Tricrcsyl Phosphate
S
s
s
S
s
s -- -- SS s
Ether: Ethyl Ether
S
s
s
s
*'s ...
s
s
s
S
--
Ether Alcohol
Carbito!*
2243rc
30799"C
vs
vs
1732G-C
2S9S
1
S SS _
Cellosolve
s s s s s s 1 ss--
Diethylene Glycol
s-- -- -- -- -- -- -- --
--
p.p'-Dihydroxy Ethyl Ether 16.923c
1999C
SS
SS
830*C
JQIOO-'C
--
--
SS
--
-- -- -- -- -
_
-- -- --
Hydrocarbon Benzene Gasoline Kerosene Mineral Spirits Paraffin Pine Oil Totuene Turpentine Xylene
VS vs vs vs VS vs
s
s vs VS 143
VS vs vs vs vs vs -- -- vs vs --
vs vs vs vs vs vs SS s vs VS -
vs vs VS vs vs vs s s vs vs --
2.02?-5^ s 2.028C s
-s
-- -- 5.0 s
--
s s vs vs s s s s s s --
vs VS vs vs vs vs s
s vs vs 142
vs VS vs vs vs vs s s vs vs --
vs VS vs vs vs vs s
s vs vs 178
Hydroxy derivatives Amyl Alcohol
S S -- -- s s SS s s s --
/7-Butyl Alcohol
s s -- -- s s 1 SS SS s --
Ethyl Alcohol (3-AJ
23329-c
S0.07t,c
--
I--
1Q27-C
2S75C
1 SS -- -
Glycerine
1 1 1 1 l 1 1 1 1 1--
Methyl Alcohol
42.5Z9*c 88.500*c
--
--
1526-C
22.26sc
--
-- SS
--
--
Phenol -- 90%
S -- -- SS s SS s s s --
Ketone: Acetone
s s -- -- s s l 1 S s 260
Miscellaneous Carbon Disulfide Nitrobenzene Water
s s -- -- s s S s VS vs -- s s -- -- s s -- -- VS -- -- 1 1 1 1 1 1 1 1 1 1-
! -- insoluble SS -- Slightly Soluble S -- Soluble VS -- Very Soluble.
Figures show grams of Arocior per 100 milliliters of solvent at 25X unless otherwise indicated.
''Ulitrrortol CuMf C*rp.
0509910
TOWOLDMONOQ35177
TABLE 14 CHEMICAL AND PHYSICAL PROPERTIES OF REPRESENTATIVE AROCLOR PLASTICIZERS AND RESINS
Property Appearance
Arocfor 1221
Clear, mobile oil
Arocfor 1232
Clear, mobile oil
Arocfor 1242
Clear, mobile oil
Arochr 1248
Clear, mobile oil
Arocfor 1254
Light-yellow viscous liquid
Color, maximum
*100 APHA
100 APHA
100 APHA
*100 APHA
*100 APHA
Chlorine, percent
20.6-21.5
Acidity, mg KOH/g. maximum
0.014
Moisture, ppm, maximum
-
Ave. Coefficient of Expansion, cc/cc/*C 0.00071 (15'-40*C)
Specific Gravity
*1.182-1.192 (25715.5'C),
Density, pounds per gajjon, 25*C
9.85
Distillation Range, *C, corrected (ASTM 0-20. modified)
275-320
Evaporation Loss, %, 10Q*C, 6 hours (ASTM 0-6, mod.) 163`C, 6 hours
1.0-1.5
Flash Point (Cleveland Open Cup), *C 141-150 *F 286-302
Fire Point (Cleveland Open Cup), *C 176 *F 349
Pour Point (ASTM E-97).
'C 1 (crystals) F 34 (crystals)
Softening Point (ASTM E-28),
-C F
Refractive Index, n D-20
20*C 1.617-1.618
Viscosity, Seconds Saybolt Universal
(ASTM 0-88)
100'F (37.8'C)
130F (54.4"C)
210`F (98.9`C)
38-41
35-37 30-31
31.5-32.5
*0.014
0.00073 (25M00X)
*1.270-1.280 (25715.6X)
10.55
290-325
1.0-1.5
152-154 305-310
238 460
-35.5 -32
-
1.620-1.622
*44-51 39-41 31-32
42
*0.015
*50
0.00068 (25*-65*C)
*1.381-1.392 (25715.5'C)
11.50
325-366
0-0.4 3.0-3.6
176-180 348-356
None to boiling point
-19 2
-
1.627-1.629
*82-92 49-56 34-35
48
0.010
*50
0.00070 ps'-esx)
*1.405-1.415 (65715.5`C)
12.04
340-375
0-0.3 3.0-4.0
193-196 379-384
None to boiling point
-7 19.4
-
1.630-1.631
185-240 *73-80 36-37
54
*0.010
*50
0.00066 (25*-65C*)
t.495-1.505 (65*/15.5*C)
12.82
365-390
0-0.2 1.1 -1.3
None to boiling point
None to boiling point
10 50
-
1.639-1.641
1800-2500 260-340 44-48
42 0S099U
TOWOLDMONOQ35178
Aroclor mo
Light-yellow. soft. sticky resin
150 APHA
60
0.014
60
0.00067 (20M00*C)
1.555-1.566 (90*/16.S*CJ
13.50
385-420
0-0.1 0.5-0.8
None to boiling point
None to boiling point
31 88
1.647-1.649
Aroclor m2
Aroclor S442
Light-yellow Clear yellow sticky, viscous sticky resin
resin
150 APHA
*2 NPA (molten)
61.5-62.5
42
0.014
0.05
-
0.00C64 (25*-65'C)
*1.572-1.583 (90715.5*0}
13.72 ~
-
0.00123 (25*-99*C)
1.470 (25725'C)
12.24
390-425
215-300 (4 mm. Hg)
0-0.1 0.5-0.6
0.01 0.2
None to boiling point
None to boiling point
35-38 99
247 477
>350 >662
46 115
*46-52 115-126
1.6501-1.6517 -
Aroclor 4405
Clear, light-yellow. resin
2 NPA (molten)
65
0.05
-
0.00061 (25*-65"C)
1.670 (25725 "C)
13.91
230-320 (4 mm. Hg)
0-0.02 0.2-0.3
None to boiling point
None to boiling point
_
Aroclor 2565
Aroclor 5460
Aroclor 1268
Black, opaque. brittle resin
_
Clear, yellowto-amber. brittle resin or flakes
*2 NPA (molten)
White to off-white powder
*1.5 NPA (molten)
65
58.5-60.6
68
1.4 0.05 0.05
0.00066 (25*-65*C) 1.734 (25725`C) 14.44
_
0.2-0.3
_
__
--
-
0.00179 (25* 124-C)
1.670 (25725`C)
13.91
280-335 (5 mm. Hg)
0.03
None to boiling point
None to boiling point
__
-
0.00067 (20'-100'C)
1.804-1.811 (25725*C)
15.09
435-450
0-0.06 0.1-0.2
None to boiling point
None to boiling point
_
60-66 140-151
1.664-1.667
66-72 149-162
-
98-105 208-222
1.660-1.665
150-170 (hold 302-338 point)
-
3200-4500 72-78
600-850 (160"F; 71*C) 86-100
300-400
90-150
--
(266'F; 130C)
--
--
0509912
TOWOLDMONOQ35179
Density
All the Aroclor plasticizers are heavier than water, a valuable propertytor many applications. Densities are shown in Figure 2.
l
Temperature, *C Fig. 2 -- Densities of Aroclor Plasticizers at Various Temperatures
Specific Volume 44
The specific volume of Aroclor 1248 at different temperatures is as follows:
Temperature m 0
Aroclor 1248 Specific Volume fmllgJ
0.674
100 0.699
200 0.726
300 0.755 400 0.790 500 0.828 600 0.870
0509913
TOWOLDMONOQ35180
Volatility
The low vaporization loss of Aroclor plasticizers is indicated in Table 15.
TABLE 15
VAPORIZATION RATES OF AROCLOR PLASTICIZERS
Plasticizer (Surface area: 1228 sq. cm.)
Aroclor 1221
Wt. Loss (9)
0.5125
Exposure at 100'C
/hr.)
24
Vaporization Rate
fgjsg. cm.fhr.)
0.00174
Aroclor 1232
0.2572
24
0.000874
Aroclor 1242
0.0995
24
0.000338
Aroclor 1248
0.0448
24
0.000152
Cbrafin'42 -S
0.0745
48
0.000126
Dioctyl phthalata
0.0S86
46
0.000117
Dutrex** 25 .
0.0256
24
0.000087
Aroclor 1254
0.0156
24
0.000053
Shell Dutrex 20
0.0047
24
0.000016
Aroclor 1262
0.0039
24
0.000013
Aroclor 1260
0.0026
24
0.000009
Aroclor 4465
0.0064
72
0.000007
Aroclor 5442
0.0039
72
0.000004
Aroclor 5460 Tricresyl phosphate
0.0032 0.0010
72 24
0.000004 0.000003
It is concluded that the vaporization rates of Aroclor plasticizers -- especially the most widely used 1254 and 1260 -- compare most favorably with the similar constants of other plasticizers selected specifically for these tests because of their low vaporization rates.
'TfitStimikofHwculn.lne. *rTrdim4ikolSh*IIOIIC.
05099^
45
TOWOLDMON0035181
Vapor Pressure
The vapor pressures of several Aroclor plasticizers are indicated in Figure 3 over the temperature range 150 to 300C.
10* t, K
\
Temperature, C
Fig. 3 -- Vapor Pressures of Aroclor Plasticizers
The estimated vapor pressures of several Aroclor plasticizers at 100F shown in the following table were determined by extrapolation from the values shown in Figure 3.
Approximate Vapor Pressure ofAroclor Plasticizers Estimated at 1006 F f37.8* C)
Aroclor 1232
0.005 mm. Hg
Aroclor 1242 Aroclor 1248
0.001 mm. Kg 0.00037 mm. Hg
Aroclor 1254
0.00006 mm. Hg
0509915
TOWOLDMONOQ35182
Viscosity
The viscosities of the Aroclor plasticizers vary according to whether the base material is a biphenyl or a polyphenyl and on the degree of chlorination. In general the low-chlorinated biphenyls have the lowest viscosities (Figure 4).
Stability
'
Toward Alkalies
The Aroclor plasticizers are remarkably resistant to the action of either hydrolyzing agents or high temperature. They are not affected by boiling with sodium hydroxide solution.
Toward Acids
No hydrogen chloride was evolved when Aroclor 1254 was stirred with an equal volume of 10 percent sulfuric acid for 150 hours. Even after prolonged treatment (255 hours) with concentrated sulfuric acid only a slight trace (too small for quantitative measurement) of hydrogen chloride was evolved.
Toward Heal
Because of their stability to heat, the Aroclor plasticizers are useful heat-transfer media. Aroclor 1254 and particularly the less viscous Aroclor 1248 are recommended for this purpose, because they may be heated up to 315C (600F) in a closed system for long periods without appreciable decomposition, and because they are nonflammable.
Toward Light
The Aroclor plasticizers have good light stability in heavily pigmented compounds and fair light stability in clear formulations. The materials become discolored, but their physical properties are not degraded. For critical applications, incorporation of a small amount of a light-
obtmib
*
TOWOLDMON0035183
screening agent greatly improves light stability at reasonable cost. The following data show that as little as 0.0X percent Tinuvin P in Aroelor 1254 nearly doubles the service life in the 50-to-100-hour range and that 0.1 percent Tinuvin P results in a 10-fold improvement.
Tinuvin P Concentration m
Fade-Omater Exposure (hours)
0 SO 100 150 500 Color (Gardner Units)
0
05
10 11
14
0.01 0 1 i 7 14
0.05 0 0 3 4 11
0.1 0 0 1 2 6
Toward Oxidation
When Aroelor plasticizers are heated to 140C with oxygen in a bomb at 250 psi, no evidence of oxidation occurs, as judged by absence of sludge formation or increased acidity. Also, no increase in acidity occurred after 4 hours heating with air at 260C and 210 psi.
Nonflammability
The viscous Aroelor liquids and the resins do not support combustion when heated alone, even at their boiling points -- above 350C. Most of the Aroelor plasticizers flux readily with resinous and pitch-like materials to give products with decreased fire hazard. Aroelor products incorporated in plastic products and rubber foams retard the rate of burning.
Nondrying Properties And Thermoplasticity
The Aroelor plasticizers are nondrying. When exposed to the air, even in thin films, no noticable oxidation or hardening takes place. Despite this property, Aroelor plasticizers do not retard the drying rate of lacquer films. Quick-drying varnishes and paints may be made with Aroelor resins without affect on drying characteristics.
The Aroelor plasticizers are permanently thermoplastic. They appar ently undergo no condensation or hardening upon repeated melting and cooling. Clear Aroelor resins are available with softening points up to 105C. The opaque crystalline solids are available with melting points up to about 160C.
Electrical Properties
The electrical properties of Aroelor plasticizers are extremely interest ing: high resistivity and dielectric strength and low power factor, as listed in Table 16. The dielectric constants of the various Aroelor plasticizers range from 3.3 to 4.9 at 100C and 1000 cycles.
O50991?
'"l
TOWOLDMONOQ35184
How To Emulsify Aroclor
TABLE 16
ELECTRICAL PROPERTIES OF AROCLOR
Volume
Dielectric
Resistivity
Power
Constant
(ASTM D-257-46) Dielectric
Factor
(ASTM D-150-47T) 500 Volts D.C.,
Strength (ASTM D-U0-47T)
1000 cycles
100*C
(ASTM D-149-44) WOO cycles. 100'C
Aroclor 25*C 100*C
(obm-cm.)
m
m
1232 5.7 4.6
1242 5.8 4.9 Above 500 x 10s Above 35
Below 0.1
1248 5.6 4.6 Above 500 x 10* Above 35
Below 0.1
1254 5.0 4.3 Above 500 x 10* Above 35
Below 0.1
1260 4.3 3.7 Above 500 x 10s Above 35
Below 0.1
1268 2.5
5442 3.0 4.9 Above 500 x 10*
5454 2.7 4.2
5460 2.5 3.7
4465 2.7 3.3
Emulsions of Aroclor plasticizers can be made simply in several ways; the method can be selected to suit the particular Aroclor and the type of formulation in which it will be used.
Emulsifiabie Concentrated Stock Solutions of Aroclor
Stock solutions made according to the following formulation are readily emulsified with water. The amount of toluene may be increased as needed to dissolve the more resinous Aroclor plasticizers.
Ingredient Aroclor Toluene Isopropanol Sterox CD (nonionic emulsifier) Santomerse No. 3 (anionic wetting agent)
Parts by Weight 79 16.70 3.55 1.00 0.75
Emulsifying LiquidAroclor Ingredient Portion 1 Aroclor 1254 Oleic Acid
Portion 2 Water Ammonium Hydroxide (28%)
Parts by Weight
100 4
100 2
9
0509918
49
TOWOLDMONOQ35185
Mix the polystyrene and ammonium hydroxide in warmed water with vigorous agitation. Mix the Aroclor 1254 and oleic acid, heat to 45C, and agitate vigorously. Maintain the 45C temperature and agitation, and slowly add in the aqueous portion (Portion 2). Continue agitation for one-half hour until phase inversion is complete.
Emulsifying Viscous Aroclor Ingredient Portion 1 Aroclor 1254 Stearic Acid
Portion 2 Water Triethanolamine
Parts by Weight
64 4
32 1
Heat the Aroclor to a workable viscosity (180F or higher) and stir in the stearic acid thoroughly. Heat the water almost to boiling (207F) and stir in the triethanolamine thoroughly. Pour the Aroclor-stearic acid portion into the water-triethanolamine portion with vigorous agitation. Process the combined portions either with a high-speed emulsifying stirrer or through a colloid mill.
Toxicity And Safe Handling
Inhalation
At ordinary temperatures the Aroclor chlorinated polyphenyls have not presented industrial toxicological problems. The hazard of potential toxic exposure varies with their volatility: the lower-chlorinated, morevolatile ones present more of a potential problem from the standpoint of both inhalation and skin contact. When Aroclor plasticizers are used at elevated temperatures, engineering controls must be applied, either by the use of closed systems or by effective local-exhaust ventilation together with general workroom exhaust.
Vapor of the liquid Aroclor plasticizers at room temperature should not be breathed in a confined space, and no vapor of any Aroclor evolved at elevated temperatures should be allowed to be dispersed into the general workroom.
Inhalation tests on animals indicate that the maximum safe concen tration of vapor is in the range of from 0.5 to 1.0 milligram of the lower-chlorinated Aroclor plasticizers per cubic meter of air. The threshold limits (maximum allowable concentration for an 8-hour working day) set by the American Conference of Government Hygien ists are 1.0 milligram of the lower-chlorinated Aroclor compounds per cubic meter of air and 0.5 milligram of the morc-highly-chlorinated compounds, such as Aroclor 1254, per cubic meter of air.
Skin Contact
Schwartz patch tests on 200 volunteers showed that Aroclor 1254 was neither a primary skin irritant or a sensitizer.
0509919
C c
c
TOWOLDMONOQ35186
Shipping
Continuous or repeated skin contact with the Aroclor plasticizers must be avoided by the use of gloves and protective garments, because of the possible occurrence of a condition called chloracne. Although reports of this condition caused by Aroclor are rare, it can be produced by excessive skin contact. If any Aroclor is spilled on the skin, the skin should be washed in the usual manner with a soap solution.
A bum caused by contact with a hot Aroclor should be treated like any ordinary bum. Aroclor plasticizer adhering to the burned area need not be removed immediately, unless treatment of the burn demands it, in which case either soap and water or repeated washings with a vegetable oil are recommended.
Freight Classification
Aroclor 1221,1243,1242, 1248, 1254,1260, 1262
Synthetic Resin, Liquid, NOIBN
Rail Classification
Aroclor 1268, 2565, 4465, 5442, 5460
Synthetic Resin, Other Than Liquid, NOIBN
Truck Classification Aroclor 1268, 2565 Aroclor 4465, 5442, 5460
Synthetic Resin, Powder, NOI
Synthetic Resin, Lumps or Solid Mass, NOI
Skipping Regulations
None
Standard Containers Aroclor 1221
Aroclor 1232
Aroclor 1242, 1248, 1254, 1260, 1262
Aroclor 1268
Aroclor 2565, 4465 Aroclor 5442 Aroclor 5460 (flaked)
Tank car, 520-lb. steel drum, 50-lb. can
Tank car, 550-lb. steel drum, 50-lb. can
Tank car, 600-lb. steel drum, 50-lb. can
200-lb. fiber drum, 25-lb. fiber drum
500-lb. steel drum, 50-lb. can
450-lb. steel drum, 50-lb. can
100-lb. bag
0509920
f
L
TOWOLDMONOQ35187
DISTRICT SALES OFFICES
Additional District Offices ere maintained by:
\
ALL DIVISIONS
ATLANTA, GEORGIA 30326 Lenox Towers West, 3390 Peachtree Rd. N.E. Tei. (404) 231-4320
BOSTON, MASSACHUSETTS 02149 Everett Station Tel. (617) 387-5010
CHICAGO, ILLINOIS 3158 Des Plaines Ave. Des Plaines, Illinois 60018 Tel. (312) 296-6688
i] CINCINNATI, OHIO 45206 1501 Madison Road Tel. (513) 751-6707
CLEVELAND, OHIO 44122 3645 V/arransvilfe Center Rd.
t Tel. (216) 991-5400
DETROIT, MICHIGAN 48235 500 Northland Towers Tei (313) 357-0910
HOUSTON, TEXAS 77002 1300 Main Street Tel. (713) Capitol 3-4011
LOS ANGELES, CALIFORNIA 90022 6670 Prflctilla St. Tel. (213) Raymond 3-2492
MINNEAPOLIS, MINNESOTA 55402 912 Northstar Center 110 S. Seventh St.
1 Tel. (612) 339-4651 NEW YORK, NEW YORK 10017 277 Park Avenue Tei (212) 922-4111
PITTSBURGH, PENNSYLVANIA 15222
! No. 4 Gateway Center Bldg. Room 534 Tel. (412) 261-2156
ST. LOUIS, MISSOURI 63166 800 N. Lindbergh Blvd. Tei (314) Wydown 3-1000
> SAN FRANCISCO BAY AREA
\ 2710 Lafayette, Santa Clara, Calif. 95052 Tel. (408) 243-0414
SEATTLE, WASHINGTON 98104 911 Western Avenue Tel. (206) Main 2-4203
I.1 SPRINGFIELD, MASSACHUSETTS 01101
730 Worcester Ave. Tei (413) 788-6911
fc'l WILMINGTON, DELAWARE 19803
I 2005 Concord Pike. Fairfax Tei (302) Olympia 8-6531
Agricultural Division
EL DORADO, ARKANSAS 71731 Smackover Highway P. 0. Box 231 Tel. (501) Union 3-3151
LULING. LOUISIANA 70070 P.O. Box 174 Tel. (504) 784-6253
Textiles Division
AKRON. OHIO 44313 3030 West Market St. Tel. (216) 838-7841
CHARLOTTE. NORTH CAROLINA 28202 Wachovia Bank Building 129 West Trade St Tel. (704) 370-9871
NEW YORK. NEW YORK 10001 360 Fifth Ave. Tel. (212) 556-5100
ENGLEWOOD CLIFFS, N. J.` 661 Palisades Ave. Englewood Cliffs, New Jersey 07831 Tel. (201) 568-2151
Hydrocarbons & Polymers Divlsion-Lion Oil
EL DORADO. ARKANSAS 71730 Lion Oil Building Tel. (501) Union 3-3111
JACKSON. MISSISSIPPI 39209 P. 0. Box 10937 Westland Station Tel. (601) 352-3648
LITTLE ROCK. ARKANSAS 72203 1615 West Seventh St Tel. (501) Franklin 6-2437
MEMPHIS. TENNESSEE 38101 1023 Riverside Drive P. 0. Box 252 Tel. (901) Whitehall 8-4451
Organic Chemicals Division (Rubber Industry)
AKRON. OHIO 44311 920 Brown Street P. 0. Box 2307 Tel. (216) Hemlock 4-1921
MONSANTO. 800 N. LINDBERGH BLVD.. ST. LOUIS, MISSOURI 63166
J
OSOSVil
c c c
2 2240-096&-6 LITHO IN U.S.4.
TOWOLDMONOQ35188