Document MJV54qGbQwaLzxqO6pDJ69b6L
TECHN
CAL
BULLET
N
; THE AROCLOR*
i POLYCHLORINATED
POLYPHENYLS ^
r A mhm of het-reti*t*nt. chemically inert and fire-retarding compounds ranging from mobile oily liquids through viscous resins and solids that
' perform unique functions in over a hundred dif* - ferent industrial and product applications.
I I
> ? * ^
TECHNICAL BULLETIN O-FF/1
; f
miffiin
I- "1
- EXHIBIT I [ J&z3L I c
6BRN 00026?
mm
TOWOLDMONOOQ2654
THE AROCLOR* POLYCHLORINATED POLYPHENYLS
A MriM of heat-resistant, chemically inert and fire-ratarding compounds ranging from mobile oily liquids through viscous resins and solids that perform unique functions in ovsr a hundred dif ferent industrial and product applications. TECHNICAL BULLETIN O-FF/1
ritei* MW*e / HI I. Uettsu* MH. / St. Leal*. Mbtseri IStSI GBRN 00026d
TOWOLDMONOOQ2655
Table of Contents
GENERAL PHYSICAL PROPERTIES CHART 4
ELECTRICAL APPLICATION OF AROCLOR Dielectrics for Askarel Typo Capacitors and Transfonnars............................ Impregnating Compounds.................................
7
7 7
MECHANICAL APPLICATIONS OF AROCLOR Expansion Madium............................................... Liquid Saalant for Fumaca Roofs................... Vacuum Diffusion Pump Oil............................
10 11 11 11
AROCLOR IN SPECIAL PRODUCT FORMULATIONS................................................... 12
Sealers for Gaskets............................................... 12 Dedusting Agent............................................... 12 Insecticides........................................................ 12 Precision Casting Wsxas................................. 12 Abrasives............................................................. 13 Specialized Lubricants..................................... 13 Industrial Cutting Oils...................................... 14
` ..
Appendix
--
Methods for Emulsifying...................................... 15 Solubility Table........................................................ 16 Vapor Pleasure........................................................ 17 Vaporization Rates................................................... 18 Corrosion Resistance of Structural Materials. . 19 Viscosity Table........................................................ 20 Density Table............................................................. 21 Dermatology fc Toxicity.......................................... 22 Safa Handling........................................................ 23 Shipping Information............................................... 23
Aak your Mm from Monsanto for additional Arochr Utaratura:
Askarel Inspection and Maintenance Guide Aroclor* Plasticizers Technical Bulletin Tharminol* FR Fluid Heat Systema
Engineering Heat Transfer Data
Aroder. Tharminot Stsrox. Santomsra, Fennvw, lustran. and WHinas are lagisMwd eadsmarfw el Monsanto Company-
GBRN 000269
TOWOLDMONOOQ2656
What are the Arodor* Polychlorinated Polyphenyls
These compound* are a series of chlorinated hi* phenyls and chlorinated polyphenyls. They range in form and appearance from mobile oily liquids to fine white crystals and hard transparent resins. Arodor is non-oxidizing, permanently thermo plastic, of low volatility, and non-corrosive to metals. Aroclor is not hydrolyzed by water, al kalis, or adds. The viscous liquids and resins will not support combustion when heated alone, and they impart fire-resistance to'Other materials.
Crystalline Arodor is relatively insoluble, but the liquid and resinous compounds are soluble in moat of the common organic solvents, thinners and oils. All Arodor chlorinated compounds are insoluble in water, glycerine or the glycols. Arodor 5460 is insoluble in the lower molecular weight alcohols; 4465 is only partly soluble in the lower alcohols.
Arodor is used alone for a particular physical job.
such as insulating, and as a sealant or expansion media. Arodor is also used as a component or ex tender in elastomers, adhesives, paints, lacquers, varnishes, pigments and waxes. The properties imparted by Arodor (and their usefulness in par ticular applications) vary in regular gradient over the aeries. Selection of the right Arodor for a par ticular use can generally be made by comparison of the properties, by blending two or more, and by adjusting the percentage used in the particular mixture in which the Arodor will be formulated.
The following table describes the properties of twelve Arodor chlorinated compounds, each of which is representative of a aeries. For almost evay Arodor shown, there is a dark-colored grade of approximately the same physical and chemical characteristics. These darker products are less pure, but are lower in price.
GBRN 000270
TOWOLDMONOOQ2657
General Physical Properties of the Aroclor* Chlorinated Compounds
>
Form........................................................
Arodor 1221 Coloriots mobile oil
Color........................................................
Acidity -- Maximum (M|m. KOH por 6m.)... Average Coefficient of Expansion... .cs/ee/*C.
Typical Density Specific Gravity...................................... Pounds por |illon -- 25X(77*F)..............
Oistillotion (Unto -- ASTM 0-20 (Mod.) Corr. *C.................................................
50 Mas. (APHA)
0.014
0X10071 (15M0X)
1.112-1.152 (2S715XX) 9.1$
275*320*
Evaporation Leu -- 5{ -- ASTM D-S Mod. 163X......... ................................. Shu. 100X............................................Ihrs.
flash Point -- Clovaland Opon Cup...........*C F
Fin Point -- Cleveland Open Cup............ X *F
Pour Point -- ASTM D-97...... '............... X
-X
SoMenint Point - ASTM E-2S................. X
X
-- IX to 1.S
141150* 296*-3G2*
m* 349*
Crystals at IX Crystals at 14X
--
--
Refractive Indei -- (Mina -- 20X...............
Viscosity -- Saybolt Universal 210*f (MAX) Sac. (ASTM -- D-M) J*f (54.4X)
10PX (37XX)
1X17-1X11 30-31 15-37 3M1
Arodor US Practically eoloriess mobile oH SO Max. (APHA) 0.014
0X0071 (25M00X) 1X70-1X90 (25715XX) 10X5
290*-325*
-- 1.0 to IX
1S2--1S4* 30S*-310*
231* 4S0* -3SX*
-32*
-
--
1.120-1X22
31-32 39-41
44-51
Arodor 1242 nacDcaity eolorteo HQ^jjl qU
90 Max. (APHA) 0X10 0X0061 (2S*-6SX) 1J11-1X92 (2S71SXX) 11.50
32S*-3K*
3.0 to 3.6 OX to 0.4
17t*-190* 3tt*-3S6* None*
-19* 2*
--
1X27-1.129 34-35 49-51 12-92
Arodor 1241 Coioriess to Ngtit yellowgreen, dear, mobile oil 50 Max. (APHA) 0.010 a00070 (25*-S5X) 1.405-1.415 (65V15XX) 12.04
340*-375*
3.0 to 4.0 OX to OX
I93M96* 379*-314 None
-7* 19.4*
--
1X30-1X31 31-37 73-10 115-240
Arodor 1254 Light yellow viscous oil
,
SO Mu. (APHA)
0.010
0X0QGS (25*-6SX)
1.495-1X05 (B5M5XX) 12.12
Ai 365*-390
. '
1.1 to 1.3 0.0 to OX
None
None
10* 1
50*
--
1X39-1X41 44-41 260-340 1900-2500 .
t)
4 6BRN 000271
TOWOLDMONOOQ2658
>
Aroctor 1260 Light yellow soft sticky resin 50 mix. (APHA) 0.014 0.00067 (20*-100*C) 1.5551.566 (907153*9 13.50
1 36*420'
0.5 to 0.1
0.0 to 0.1
None
None
31* *8*
-
1.$47-1.649 72-70 32004500
'
Aroctor 1262 Light yellow sticky detr resin SO Mix. (APHA) 0.014 0.00064 (25*-65*C) 1.572-1.563 (90V15i*O 13.72
395*425*
0.5 to 0.6 ootoo.1
None
None
35*-30* 99*
-
1.6501-1.6517 06-100 00-850
Aroctor 1268 White to off-white powder IS Mu. NPA (molten)
0.05 0310067 (2QM00*C) 1.604-1.811 (25V25-C) 15.09
435*450*
0.1 to 0.2 0.0 to 0.06
None
None
-
-
150* to 170* (Onto pi) 302* to 333* (hold pi)
--
-
--
Aroctor 4465 Light-yellow, elitr, brittle resin 2 Mix. NPA (molten) 0.05 0.00061 (25*-65*C) 1.670 (2S72S*C) 13.91
230*-320* st 4 mm. Hg.
02 to 0.3 0.0 to 0.02
None
None
-
60* to 66* 140* to 151*
1A64-1.667 90-150
CMTrar IWO "*
hk
AA
Aroctor 5442 Yellow trsnspirent sticky resin 2 Mu. NPA (molten) 0.05 0310123 (25*-99*0 1.470 (2S*/25*C) 1224
215*-300* at 4 mm. Hg.
02 0.01
247* 477*
46* 115*
46* to 52* 115* to 126*
--
300400
--
Aroctor 5460 Clisr, yellowto-imber, brittle resin
2 Mu. NPA (molten)
0.05
0.00179 (25*-124*C)
1.670 (25V25-C) 13.91
Aroctor 2565 Btock. opique, brittle resin
__ '
1.4
0.00066 (25*-65*C)
1.734 (25*/25*C) 14.44
_ *
290*-335* it 5 mm. Hg.
-
0.03 1.5 to 1.7
(t 2W-5 hrt.)
None
02 to 0.3
--
None
None
None
--
-- .--
98* to 1052* 206* to 222*
1.660-1.665
--
66* to 72* 149* to 162*
-- -- --
GBRN 000272
5
TOWOLDMONOOQ2659
RESISTANCE TO DRYING
Arodor is non-drying. Even when exposed to sir in the form of thin films, no noticeable oxidation or hardening takes place. However, when used as a component of paints, varnishes or lacquers, it does not retard the rate of drying of the* films. Quick drying varnishes and paints can be made using Aroelor in the formulation.
FIRE-RESISTANCE
Viscous, oil-like Aroelor and the Aroelor resins do not support combustion when heated alone, even at their boiling points -- temperatures in excess of 350*C. Most of the Aroelor chlorinated com pounds flux readily with other resinous and pitch like materials to make mixtures that gain in fire retardance properties. Even when incorporated in nitro-cellulose films and rubber foams, Aroelor will retard the rate of burning.
ADHESIVENESS AND THERMOPLASTICITY
The Aroelor resins adhere strongly to smooth surfaces such as glass, metal, vanished or lac quered coatings.
Aroelor is permanently thermoplastic. It appar
ently undergoes no condensation or hardening
upon repeated melting and coding. Clear Aroelor
resins can be supplied with softening points up to
105C. Opaque, crystalline Aroelor can be'sup
plied with initial melting points^ up to approxi
mately 290*F.
'
STABILITY
Toward Alidtm -- Arodar is remarkably re sistant to the action of either hydrolysing agents or high temperature. It is not affected by boiling with sodium hydroxide solution.
Toward Arid* -- Experiments were made to de termine whether hydrogen chloride it evolved dur ing the treatment of Arodar with sulfuric add.
Aroelor 1254 (selected as typical) was stirred with an equal volume of ten per cent sulfuric add for a period of 150 hours. Any gases escaping from the reaction flask had to pass through a trap filled with silver nitrate eolution, which would give a precipitate of silver ehloride if any HC1 came in contact with it. After 150 hours of treatment, neither the trap solution nor the add layer in the treating flask showed any hydrogen ehloride present.
Even prolonged treatment (255 hours) with con centrated sulfuric add indicated negligible effect.
Toward Hoot -- Arodar is n useful heat transfer media because at its stability to heat. Aroelor 1254 and particularly the less viscous Arodor 1248 are recommended for this purpose because they may be heated at temperatures up to 315*C (600*F) in a dosed system for long periods without appre ciable decomposition and they are fire-resistant.
Toward Oxidatum -- When Arodar is subjected to a bomb teat at 140*C with 250 pounds oxygen per square inch, there is no evidence of oxidation as judged by development of addity or formation of sludge.
ELECTRICAL RESISTIVITY
Aroelor has extremely interesting electrical charac teristics: high resistivity and dielectric strength and low power factor. The dielectric constant ranges from 8.4 to 5.0 at 100*C and 1000 cycles, depending upon the particular Arodar.
SOLUBILITY
All Arodor chlorinated compounds are insoluble in water. They are soluble, however, in most of the common advents, plasticizers, and resins.
The Arodar oils and resins are readily aduble in most of the common organic solvents and drying oils. Hard crystalline Arodor is in general less soluble than the liquid or softer Arodor resins. Arodor is heavier than water, a valuable property for many applications.
f) 0
D
68RN 000273
TOWOLDMON0002660
Electrical Applications
of Aroclor
Aroclor is one of the purest commercial chemical compounds, virtually free of even traces of con ducting impurities: For this reason, dielectric properties of Aroclor closely approximate the theoretical maximum for these particular organic compounds. With its stability, heat-resistance and fire resistance -- Aroclor can be used for a variety of heavy-duty dielectric applications.
DIELECTRICS FOR ASKAREL TYPE CAPACITORS AND TRANSFORMERS
Aroclor is used per se in capacitors and is formu lated for the liquid coolant-insulation fluids in transformers. Such dielectrics must be highly pure with dependably minimal traces of electrolytes. They must be chemically stable and non-corrosive to a wide variety of structural materials. Most im portant, the dielectric fluid must be fire-resistant.
Aroclor is the only liquid in low cost commercial supply that meets these exacting requirements.
Aroclor liquids 1242, 1248, 1254, and 1260 are used directly, or are carefully formulated with chlorinated benzene and other additives to make askarel fluid for particular needs. Typical formu lated askarel fluids are shown on the following pages.
Aroclor liquids 1242 and 1254, themselves or in special formulations, are used as the dielectric in
fixed paper capacitors, for the power factor correc tion in utility transmission lines; for home ap pliances such as air conditioners, furnaces, washers and driers; for electric motors; and for ballast in fluorescent fixtures. There are also a number of applications in DC systems, in con densers, and the new energy storage capacitors.
.The Aroclor fluids can be used in a wide variety of applications requiring a specialized dielectric. Monsanto works closely with electrical equipment makers to develop the proper dielectric with the exact physical properties required by the engineer ing of the equipment.
II
IMPREGNATING COMPOUNDS
Because of its nonflammability, high resistivity, dielectric strength and low power factor, liquid and resinous Aroclor is extremely useful as an impregnating compound. An important applica tion of Aroclor in the electrical field is the use of Aroclor 1260, 4465, and 5460 in wire or cable coatings and as impregnants for cotton and asbes tos braided insulation. Because they possess high purity and excellent electrical resistance, Aroclor 1254, 5460 and 1268 make superior dielectric sealants to dose the pores of carbon resistors, and to seal electrical bushings and terminals.
~ ...
To attain the lowest possible loss factor and gain resistivity, Aroclor is often treated with about 0.20% by weight of Attaupulgus clay or Fullers earth. To activate the earth it should be heated to 450*-500*F.
ELECTRICAL PROPERTIES
DitltrUt eeartsat si 14N Oydse (1)
Amt*
H*C
1M*t
Vehms RssMMfr (t) Ofcw-M 01166*6, MOVsHiDX.
OhtaMs MeeRb O)
1232 5.7
44
1242 5J
44
Abort 500x10*
Critter thin 35KV
1241 5.6
44
Abets 500x10*
Crestir thin 3SKV
12S4 5.0
44
Abort SOOxlP
Gmtir thin 3SKV
1260 U
17
Abets 500x10*
Greater thin 3SKV
1261 1$
--
6442 3.0 44 Abote 500x10*
5464 2.7
44
5460 15
17
4465 2.7
13
CUWVfeMMT m am
o> am MMI AIRIbMT
Pee* Fm* (4)
166*6,1466 Cyitot
<0.1* <0.155 <0.1* <0.1*
GBRN 00027*
TOWOLDMONOOQ2661
TYPICAL TRANSFORMER ASKAREL
(MIXTURE OF AROCLOR AND CHLOROBENZENES)
Vise. 37.!*C. (ASTM 088) Spec Gravity 9 15i/15.5*C.. (ASTM 0287)
Color, APHA
Condition
Acidity, mg KOH/g.
Pour Pt, *C,, (ASTM 097)
Inorganic Chloride*, ppm
Refractive Index 9 25*C.
Distillation Ranp (ASTM 020) Corrected for stem and beromctric protsura
First drop 3SR 5595 595 9585 Corrosion
Weter Content ppm.
Resistivity, 100*CM 500v,, 0.1' pp
Dielectric Strength, 25*C.
Dielectric Constant, 100*&, 1000 cycles*
Tin Tetraphenyl*
Burn Point (ASTM 092)*
Fixed Chlorine*
.
Arc Formed Geses* (Oxygen Free Liquid 2S*C.) -
Electrical Stability*
iw
TypUM 4145 Sec Seybolt Univ.
1.S63-L571 ISO max. Clesr HOI mix. --44*C., or lower 0.10 mu. 1.6075-1.608$
210*C., min. 240-2S6*C. 290-330*C. 385400*C. 395415*C-
After hotting with iluminum for 6 hr*. 9 200-220*C., the aluminum must not be corroded either on visuif or weight inspection.
The isktrel fluid meets the following spaeiSeitions:
Color, APHA
200 mix.
Acidity, mg. KOH/g.
0D1 mix.
Inorg. Chlorides,
ppm 5 mix.
Condition
Clear
30 max.
100 x 10* ohm-cm., min.
35 KV, min.
3.84.2
0.12595 0.0195 by weight
None up to Boiling Point
B0J 03
Total combustible gases including carbon monoxide, hydro gen and volatile hydrocarbons.
After heating for 96 houri 9100*C in a closed container, the
resistivity should not decrease mors than 1095.
0
8
i)
GBRN 000275
TOWOLDMONOOQ2662
TYPICAL CAPACITOR AROCLOR
( Pmpsehr
Typical
Vise, ft 37.fC. (ASTM 088)
82-92 seconds Saybolt Univ.
Specific Gravity @ 2S/1S.S*C (ASTM 0287)
1.381-1.392
Color. APHA -
50 max.
Condition
Clear
Acidity, mg. KOH/g.
0.01 max.
Poor PL. *C. (ASTM 097) . --14 or lower
Inorganic Chlorides, ppm
0.10 max.
Refractive Indts ft 25*C.
1^240-1.6260
Distillation Range (ASTM 020) Corrected for stem and barometric pressure
109132S*C. min. 9096 360X. max.
Corrosion
After heating with aluminum for six hours at 210*C 10*C
the aluminum must not be corroded either on visual or weight
inspection and the Arodor 1242 should meet the following
SpiCS!
Color, APHA
60 max.
Acidity, mg. KOH/g.
03)1 max.
Inorg. Chlorides, ppm 0.10 max.
Condition
Clear
Water Content ppm
35 max.
Resistivity 100*C. 500 volts OC ft 0.1' gap
500 x IIP ohm-cm., min.
Dielectric Constant 100*C.ft1000 cydes (ASTM 0924)
47-4.9
Flash Point Clave. Open Cup*
170*C., min.
Fire Point *C.*
None to boiling point
Z Sulfates (ASTM-D117-31)* ! Fised chlorine content (Carius)*
Specific Heat ft 2S*C.*
None
4L542J5S 029
Evaporation @ 100*C for 6 hrs.*
0.49(max.
Dielectric Strength (KV) (ASTM D877)*
35 Min.
DIELECTRIC CONSTANT VS. TEMPERATURE Aroclor* 1242 ft Aroclor* 1254
[
TCMUcnAiunK cgirmnAOC eoum or me jouiiul or nunum luonnnt no ecu mminni luouatodiu
CBRN 000276
9
TOWOLDMONOOQ2663
Mechanical Applications of Aroclor
Because Aroclor chlorinated compounds have ex cellent shear resistance, heat stability, and are chemically stable ... they can serve in dozens of mechanical applications for transferring mechani cal power, beat and variable pressures. Aroclor does not attack metals even at high temperature; it resists oxidation, chemical and mechanical breakdown under a wide variety of environmental conditions. Aroclor liquids used as lubricants im part a high degree of extreme pressure lubricity.
HEAT CAPACITY OF AROCLOR* LIQUIDS at Various Temperatures
0
0
THERMAL CONDUCTIVITY OF AROCLOR 124S
Twees c.
30 CO 100
r.
10 MO 212
BTU./Hr./H 81/ *F^FL
04680 CL0687 0.0697
HCw./*e!/cw.
281110--* 28* 110--* 288 110--*
GBRN 000277
TOWOLDMONOOQ2664
t
EXPANSION MEDIUM
Because of their stability at high temperatures and ability to withstand frequent temperature cycles without gum formation, Arodor liquid is used as the actuating medium in bellows controls, thermo stats, industrial temperature control regulators and other kinds of automation equipment.
sealants for any application where the use of oil would mate a fire hazard. In the trough of an nealing furnaces, for example, Arodor makes de pendable fire-safe roof seals.
VACUUM DIFFUSION PUMP OIL
The average coefficient of expansion of Arodor Fluid Arodor 1248 and 1254 are highly stable to
1248 per degree F within the various temperature air; they make good oils for vacuum pumps at a
ranges indicated in the table below was determined much lower cost than high priced silicone type oils.
by using the simple formula Vt - Vt` [1 + a (t -- ti).) The coefficient a, has been calculated at 100'F
Arodor operates efficiently in vacuum diffusion pumps used to pull high vacuum for metalizing
increments as follows:
'
plastics, dehydrating foods, medidnals, and for
Tea*. Rasp *F
Awa|s GssMsat tt r-r-1-- m/n/f
drying capacitor cones.
0 to 100
0.00037
t
100 to 200
0.00039
200 to 300
0.00040
300 to 400
eootosoo
0410046 O.OOOU
500 to GOO
0.00051
The specific volume of Arodor 1248 at different
temperatures is as follows:
Tm*. *r
0 100 200 300 400 500 600
pmHs Mm sd/pi
0.674
0.699
0.726
.
0.755
`
0790
Ad
0470
LIQUID SEALANT FOR FURNACE ROOFS
Because of their low vapor pressures and fireresistance, Arodor 1248 and 1254 make excellent liquid sealants. These non-evaporating fluids have good flow at slightly derated temperatures and are -hmiM-Uy stable at elevated temperatures.
Consequently, Arodor liquid makes excellent fluid
6BRN 000278
I
TOWOLDMONOOQ2665
Aroclor in Special
Product Formulations
With their wide range of physical properties, their
inertness, lubricity, and vapor-suppressing char
acteristics -- Aroclor chlorinated compounds can
be valuable ingredients in an extraordinary variety
of formulated products. They are compatible with
a variety of solvents, oils and resins. Virtually
non-volatile and permanently thermoplastic, they
will not react with other chemicals in the formula
tion. In addition, their low cost makes their use for
special purposes eminently practical and eco
nomical.
--
SEALERS FOR GASKETS
Aroclor -- particularly when hot -- swells rubbers like Hyear*, Koroseal*, PerBuna N, and Neo prene. Wherever seals and gaskets of natural or synthetic rubber tend to shrink under heat and use, Aroclor 1232,1242, or 1254 can be used as a swelling agent to tighten the shrunken seal. An example is in automotive transmission oil: a small amount of Aroclor in the oil swells the seal in place, saving the cost of tearing down the equip ment to replace the seal or gasket. Aroclor can be used in gasket sealing compounds to swell the rubber after the gasket or seal is in place. *
DEDUSTING AGENT ~
Aroclor 1254 is a low cost dedusting agent which can hold down the dusting of a variety of chemical products. Because Aroclor 1254 resists both com bustion and oxidation, it can be used to control dusting of highly reactive compounds. As a typical example,(1) .a few tenths of one percent will con trol the dusting of calcium hypochlorite.
INSECTICIDES
Aroclor 5460 and 1254 act as vapor suppressants. United States Department of Agriculture seienttists reported that the inclusion of from 5 to 25 parts per hundred by weight of Aroclor increased the effective kill-life of a lindane spray up to ten times. A painted or metallic surface sprayed with certain chlorinated insecticides fortified with Aroclor will remain toxic to flies, ants, roaches and silverfish up to 2 to 8 months. The Aroclor resins suppress the rapid evaporation of the volatile insecticides without adding odor or other objec tionable residue. Formulation into insecticides is quite simple; the Aroclor is dissolved in a suitable solvent compatible with the insecticide formula tion, and mixed in. The most pronounced effect for increasing the kill-life of the insecticide is ob tained with lindane, chlordane and BHC. Aroclor is recommended for chlorinated insecticide formu lations to be used far non-crop spraying. Their low cost makes this use a most practical way to lower the ultimate cost of insect control.
PRECISION CASTING WAXES
Aroclor is compatible with various natural waxes,
such as earnauba and others, including those used
to formulate easting wax. Aroclor helps impart to
the finished casting wax a number of desirable
properties: hardness without brittleness; resist
ance to shrinking; sharp definition; sharp melting
point; and fire-resistance. Waxes formulated with
Aroclor are non-taeky and highly stable. Waxes
containing Aroclor are widely used in making
dental castings, in the precision casting of aircraft
parts, and far
costume jewelry. Aroclor
1254,4465 and 5460 are mast frequently used ...
proportions dependent upon the properties re-
0
0 0
12 GBRN 000279
TOWOLDMONOOQ2666
quired in the finished wax. Much of the highest quality precision casting wax used in the lost wax process is formulated with Arodor.
AROCLOR IN ABRASIVES
Arodor 1254,1268 and 5460 are used in the manu facture of specialized abrasives. Because of their excellent bonding characteristics, high thermal stability and resistance to oxidation and corrosion -- Arodor is used as the carrier for abrasive ma terials. A major use is as part of the bonding agent in specialized grinding wheels.
AROCLOR IN SPECIALIZED LUBRICANTS
For specialized lubricants requiring good extreme pressure (EP) characteristics, the Arodor liquids make excellent additives. They impart high tem perature stability, excellent lubricating qualities, and weather and corrosion resistance. As an ex ample, Arodor is used to formulate grease and pipe thread compounds for use in oxygen systems. Greases formulated with Arodor have a high chemical resistance and are suitable for use in contact with corrosive chemicals. Gear oil lubri cants containing Arodor have good resistance to shew degradation and high temperature stability. Added in small amounts to railroad car journal box oils, Arodor imparts better extreme pressure lubricity and reduces the incidence of hot boxes.
The heat-resisting, nonflammable characteristics of the Arodor chlorinated compounds make them attractive in themselves as lubricants under condi tions of high temperature. As an example: in gov ernor systems of central poerar stations, Arodor 1248 is well suited to this lubricating application.
Straight Arodor 1254 gives excellent results on a
roller bearing test operating at 255-260F with much leas carbonization or decomposition than the usual spindle oil under the same conditions.
As an extreme pressure (EP) lubricant base added to a petroleum hydrocarbon oQ in amounts up to approximately 15% by weight, Arodor 1248 and 1254 materially increase the load-carrying proper ties without reducing the viscosity of the resulting composition. These two compounds represent one of the more satisfactory carriers for the element chlorine as an extreme pressure base, possessing the following advantages:
1. STABILITY. Even at higher temperatures, there will be neither separation of components nor appreciable change in physical or chemical properties during long periods of operation.
2. NON-VOLATILE. Many other types of chlo rine bearing compounds are so volatile as to render them unfit for long periods of service. Arodor is non-volatile at normal temperatures.
8. NON-OXIDIZING. Arodor does not oxidize nor thicken up to an objectionable degree.
4. NON-CORROSIVE. Arodor does not attack metal surfaces.
5. NON-ABRASIVE. Arodor exerts no abrasion on the machined surfaces.
6. NON-HYDROLYSIS. Arodor does not hy drolyse in the presence of water, thus avoiding the generation of hydrochloric add.
7. COMPATIBILITY. Arodor ia completely misdble with mineral oils.
8. COLOR. Arodor does not darken or change the color of lubricating oS.
GBRN 000260
13
TOWOLDMONOOQ2667
Where lubrication is subjected to water displace ment exposure, for example in the lubrication of bridge rollers, a heavier-than-water lubricant can be prepared from mixtures of Aroclor and oil. The following are typical examples: '
Mis Ne.
1 Z
MkyvsifM OR* Ami* 1141
50 SO 25 75
Viscosity 210*F-160 Siybolt Sacs. Color ASTM 7- Flish Point SWF. Pouf Point 15*F. mi mak- imi m no
toarPt
0*F +S*F
nelly at 1UTL
1.1263 12703
]
0
Aspni. Paurts/Osi.
94 10.6
AROCLOR IN INDUSTRIAL CUTTING OILS
Aroclor 1254 is used to formulate the finest quality straight and soluble or emulsifiable-type cutting oils. The Aroclor functions as an excellent extremepressure lubricant and is far superior to aliphatic chlorinated hydrocarbons because of its higher order of thermal stability. The heat resistance is most important in cutting oils for machining high grade steel. With Aroclor cutting oils there is a lower degree of hydrolysis which minimizes the staining of the metal.
GBRN 000281 --I
14
TOWOLDMONOOQ2668
Appendix
Methods for Emulsifying
and Making Stock Solutions of Aroclor
There are several simple methods for making Aroclor emulsions; the one used may be selected to suit the kind of Aroclor and type of formulation in which it will be used.
Emulsifying Viscous Aroclor
(Portion 1)
16 lbs. of Aroclor
1 lb. of stearic acid
(Portion 2)
8 lbs. of water
4 oz. Triethanolamine
~ ...
Heat the Aroclor to a workable viscosity (180*F plus) and stir in the stearic add thoroughly. Heat the water to almost boiling (207*F) and stir in the triethanolamine thoroughly. Pour the Aroclor stearic add portion into the water portion, agitat ing vigorously. Then process the combined por tions with a highspeed emulsifying stirrer ... or process through a colloid mill.
Emulsifiable Concentrated Stock Solutions of Aroclor
79 parts of Arodor 16.70 parts of toluene 3.55 parts of isopropyl alcohol
1.00 parts of Sterox CD non-ionic emulsifier 0.75 parts of Santomerse* anionic wetting
agent
The above formulation is readily emulsifiable with water. If a more resinous Arodor is used, increase the amount of toluene (or xylene) as needed to dissolve the Arodor resin.
6B*N QQQ282
TOWOLDMONOOQ2669
SOLUBILITY OF AROCLOR* CHLORINATED COMPOUNDS IN 100 MILLILITERS OF VARIOUS SOLVENTS
Arodor . Typ* of S#*v*nl
1242 2S*C Mot
Acid Aeetic Add.................. Oleic Add ................ SenzotcAcrd.............
S * lo.o we
S 2 ---
Aidehyo# 40% Fomwidahyd*..........
t
Furfural....................
vs
Amina
Aniline.......................... s Pyndin. ....................... 122.2 am
Chlero -- tfwinthm
Amyl cMohdM--mimd...... Carbon Tetrachloride......... Chloroform..................... Dichlorethylene .......... ..
% s s --
Ethylene Dsehloritfe........... s MonocMorobenzene.......... s
1 VS s 440 IPS s s s -- s s
1242 2S*C Hot
_ 10.0 we
--t -- --
11 V2 vs _-- ----
ss
ss
2s
----
2 s
s s
TatracMorothana............. Trichloretheno................. Trlchlerethytene...............
s s s
s s s
Oryinf OH
. ..
Tun OH........................ s
linuid OM.....................
s 2
lit.r Amyl Acotato.................. Butyl Acotato.................. CaNetdvt AcMt4............ Cottonsoad OH................. Oibutyt Phtholote............. Diethyl Phtholote............. Ethyl Acotato.................. Ethyl Lactato................... Cthytam aiyfcot DiaeaUM.. Methyl Acotato............... Trieraayt Fhosphato...........
s s s s s 2 s 2 2 2 s
s s s s 2 s s 2 2 2 s
Cthor: Ethyl Ethar............... s
2
Ethar Alcohol Carbttoi*........................
224 IP*
CaHoaohra ..................... s
ixatnyiaitO WyCOi.............. M1 DlhyOraay Ethyl Ethar...
U.ot
207 am s
IS we
Hydrocarbon Bonxana........................ VS Gaoolino........................ vs Koroaono....................... vs Mineral Spirits................. vs Paraffin......................... 2.0 9** Pino OH......................... 2 VS Turp.mtn...................... vs Xylene......................... *. vs
VS VS vs vs s a vs vs vs
Hydroiy derivethret
Amyl Alcohol..............
s
n-2uty< Alcoftct................ Ethyl Alcahol (S-A)............
21ja m
Gtyc.fiim....................... MMhyl AleaMd................. Ptiwot-*0%..................
42.*1 am 124 am
s 2 *04 Wb 1 N.6 wc 2
Kotono Acotono......................... 2
2
MiM#N.fMOW* ' Carbon CNowHMo.............. NltfoMnz.M.................. Water...........................
s 2 1
s s I
t s s s 2 s s 2 s s s 2 s 2 2 s
vs s ts vs vs vs v vs toot vs vs vs vs
-- -- 1 -- -- -- -- -- 1
s s s
s s
s s s s s s s s s s s s
vs s ss
vs vs vs vs s vs vs vs vs
-- -- 1 --
--
----
1
1224 1270 4462 5460 25*C Met Cold Hot Cold Hot 25*C
ss
- ss 9 --
2 s -- -- 2 vs --
-- " --"
* --
1 vs
1 vs
1 1 1 1-- ss ss vs vs --
s s -- -- vs vs -- 114am 422 arc -- -- vs vs . " .
s s
s s
-- -- vs vs -- S.T -- vs vs 156
s s--
vs vs --
-- s
-- s
S.0 --
--
vs vs
vs vs
-- --
s s 2.*
vs vs
s s -- -- vs vs _
s s
s s
2.2
--
vs vs
vvss
--
s s
s s s s s s s s 2 s s 2 ITS we s we
vs vs vs vs -- 2 vs vt vs
s 2
s s s s s s s 2 s s s 2*9 am s 10 MPC
vs vs vs vs s s vs vs vs
-- -- -- -- -- -- -- ---- -- -- -- -- 2 -- -- -- 3--.S -- -- -- -- -- -- --
-- vs vs -- -- vs vs --
-- vs vs --
-- vs vs --
-- vs vs "
-- s vs ""
-- s vs --
-- --
s s
vs vs
----
-- vs vs
-- vs vs --
-- s s --
-- ss s --
s s ----
-- 11 -- -- -- s -- --
-- ss -- --
-- -- --
vs vs vs
vs vs vs
143 -- --
-- -- -- --
vs vs <s.o s
ss vs vs
-- -- -- 142
-- vs vs --
-- vs vs 17S
s s"
s s -
102we
aws e
-- --
-- --
a ss
s --
-- --
1 1 11
1--
IS we 824 Wt -- -- a -- --
ts s -- -- 2 s
s s -- -- 2 s 260
s s
s s
----
--
vt vs
vs --
-- --
1 1 111
.
(i
C *
18 6BRN 000233
TOWOLDMONOOQ2670
VAPOR PRESSURE m m MERCURY-
VAPOR PRESSURE OF AROCLOR* CHLORINATED COMPOUNDS
'I
Cl
6BRN 000284 1
TOWOLDMONOOQ2671
VAPORIZATION RATES
W.
WLLaaa
Araelot*122I
Aroclor 1232
Aroclor 1242
Aroclor 1248
425? chloriniM paraffin
dioctyl pMhalata
Dutnx*2S
Aroclor 1254
Dutrax 20
Aroclor 1262
Aroclor 1260
. ..
Aroclor 4465
Aroclor 1270
Aroclor 5442
Aroclor 5460
Tricrtiyl phoxphatt
0.5125 112572 0.0995 0.0448 0.0745 0.0686 0.0256 0.0156 0.0047 0.0039 0.0026 0.0064 0.0045 0.0039 0.0032 0.0010
iSMMIDIIti
ff
24 24 24 24 48 48 24 24 24 24 24 72 72 72 72 24
Snrfaaa Atm Cm.'
12.28 12-28 1228 1228 1228 1228 1228 1221 1228 1228 1228 1228 1228 1228 1228 1228
VaparlaMaa Rata PM./ml4v./1M*C
0.00174 0.000874 0.000338 0.000152 A00012S 02)00117 0.000087 0.000053 0.000016 0.000013 0.000009 0.000007 0.000005 0.000004 0.000004 0.000003
I
APPROXIMATE VAPOR PRESSURES
CALCULATED AT 100* F (37.r C)
ft: GBRN 000285
TOWOLDMONOOQ2672
!>
CORROSION RESISTANCE OF STRUCTURAL MATERIALS
Metals
ItN tre 1t6*6
Aluminum................................................................... Copper........................................................................ Magnesium.................................................................. Nickel......................................................................... Silver..........................................................................
Mild Steel.......................... .............. :........................ Phosphor Bronze.......................................................... Red Brass.................................................................... Stainless Steel (Type 316)............................................ Yellow Brass................................................................
Plastics Alkyd Resin No. 46534-12............................................. Alkyd Resin No. 46594-13A........................................... Cellulose Acetate (Fibcstos).......................................... Durite111 Phenol Furfural Resin...................................... Formvai* Highly Plasticized polyvinyl formal resins...... Formvar* Low Plasticized polyvinyl formal resins.......... Glyptal 1276................................................................ Glyptaf 7136................................................................ Maleic Resin No. 46SS4-13B.......................................... Maleic Resin No. 46S94-13C..........................:.............. Methyl Methacrylate......................................... .......... Lustron* B Polystyrene'............................................... Resinoz* Mineral Filled Melamine Rash)....................... Resinox Wood Flour Filled Melamine Resia.................... Resinoz Mineral Filled Phenol roneoldohyds.................. Resinoi Wood Flour FiHad Phenol Formaldehyde............ Resinoz Rag Filed Phonal Fornnidohydo.................... Urea Formaldehyde Rosie (Ptaskon Co.).........................
R R RR RR R R R RR R b RR R
P 0
0 D Oe PS R D P P 0 P 0 0 0 0 0 0
R 0 R R R R R R 0 D RR Rs
P P P P T T P T P P P T P P 0 P 0 P
iaM wt m*e
RR R0 RR R RR RR RR RR RR RR RR RD RR RR R Os
P P 0 P 0P R P Pe T PS T 0P R T P P R P 0 P PT R R R D 0 0 0 R 0 0 0 P
44M m*e
RR 0 RR RR R R R R R R RR Re
P P P 0 T T P T P P P T P R R 0 0 P
6408 itt*e
RR D RR R R R RR RR R De RR Re
P P P P T T P T P P P T 0 P P P P P
6BRN 000286
19
TOWOLDMONOOQ2673
r
VISCOSITY RANGES OF SOME OF THE AROCLOR* CHLORINATED COMPOUNDS
I
VISCOSITY, SAV0OLT UNIVERSAL SECONDS
GBRN 000287 20
TOWOLDMONOOQ2674
TOWOLDMONOOQ2675
Dermatology and Toxicology
At ordinary temperatures the Arodor poly chlorinated polyphenyls have not presented in dustrial toxicological problems. The hazard of potential toxic exposure varies with their vola tility: the lower-chlorinated ones, being more volatile, present more of a potential problem from the standpoint of both inhalation and skin eontact. When Arodor is used at elevated tempera tures, engineering controls must be applied, either by the use of dosed systems orby effective localexhaust ventilation together with general work room exhaust.
Inhalation tests on "*" indicate that the maxi mum safe concentration of vapor is in the range of 0.5 to 1.0 milligram at the lower-chlorinated Aro dor compounds per cubic meter of air. The thresh old limits (marimiim allowable concentration for an 8-hour working day) set by the American Con ference of Government Hygienists are 1.0 milli
gram of the lower-chlorinated Arodor compounds per cubic meter of air and 0.5 milligram of the more-highly-chlorinated compounds, such as Aro dor 1254, per cubic meter of air.
Schwartz patch tests on 200 volunteers showed that neither Arodor 1254 alone when applied to gauze nor a polyvinyl chloride film containing 11.5-weight-per cent Arodor 1254 was a primary irritant or a sensitizer. Canvas coated with an oilmodified alkyd resin (17-weight-per cent of the paint-film aolids and 7-weight-per cent of the painted fabric was Arodor 6480) did not produce primary skin irritancy or sensitization according to the same Schwartz technique. Continuous or re peated skin contact with Arodor must be avoided because at the possible occurence of a condition called chloranee. Although reports of this condi tion caused by Arodor are rare, it can be produced by excessive skin contact.
6BRN 000289 22
TOWOLDMONOOQ2676
I
Safe Handling
Vapors of the Aroelor liquids at room temperature
should not be breathed in a confined space. Vapors
evolved at elevated temperatures should not be
allowed to be dispersed into the general workroom.
Instead, engineering control must be applied to
reduce vapor concentrations below the allowable
concentrations mentioned above.
a
Continuous or repeated skin contact with Arodor
must be avoided by the use o#-gloves and pro
tective garments. If any Arodor is spilled on the
sldn, the skin should be washed in the usual man-
A burn caused by contact with a hot Arodor should be treated like any ordinary burn. Arodor etUwring to the burned area need not be removed immediately, unless treatment of the burn de mands it, in which case either soap and water or repeated washings with a vegetable oil are recom
0 mended.
Shipping Information
AXOCLOX1221,1243,1242, 1241,1254.126a 1262
AR0C10R1268,2565,4465, 5442,5460
AMCLOIUWI, 2S6S
AXOCIOX 446a 5442,6460
Synthetic Kssin, Liquid, NOIBN
Synthetic Resin. Other Than Liquid, NOIBN
Synthetic Resin, Powder, NOI
Synthetic Resin, Lumps or Solid Mass, NOI
AXOCLOX1221
AXOCLOX 1232
AXOCLOX 1242.124A 1254, 1260.1262 AXOCLOX 1261 AXOCLOX 2565,4455 AXOCLOX 5442 AXOCLOX 5460 (Hiked)
Tank car, $20-Ih. stool drum,
50-lb. CM Tank car, 550-lb. steel drum,
50-lb.ean Tank car, 600-lb. steel drum,
50.1b. cm 200-lb. (her drum, 50-lb. can 500-lb. steal drum, SO-lb. can 450-lb. steal drum, 50-lb. can 100-lb. bag
66RN 000290
23
\
TOWOLDMONOOQ2677
-DISTRICT SALES OFFICES . ALL DIVISIONS
ATLANTA. GEORGIA 30326
Lonet Towort Watt.
3390 Patchtraa Pd. N.C.
Tal. (404) 231.4320
'
.
BOSTON. MASSACHUSETTS 02149 Cvaratt Station
Tal. (617) Dunkirk 7-6010
CHICAGO. ILLINOIS 3156 Ota Plamat Ava. Oat Ptainaa. IHinoia 60016 Tal. (312) 296-6668
CINCINNATI. OHIO 45206 1501 Madiaon Poad Tal. (513) 751-5707
CLEVELAND. OHIO 44122
3645 Warranavida Cantor Pd. Tat. (216) 991-5400
DETROIT. MICHIGAN 48235 500 Northland Towart Tat (313) 357-0910
HOUSTON. TEXAS 77002 1300 Mam Straat Tal (713) Capitol 3-4011
LOS ANGELES. CALIFORNIA 90022 6670 5. flotilla St Tal. (213) Paymond 3-24S2
MINNEAPOLIS. MINNESOTA 55402
912 Northttat Cantar 110 S. Seventh St Tat (612) ftdaral 9-4651
NEW YORK. NEW YORK 10017 277 Park Avanua Tal. (212) 922-4111
PITTSBURGH. PENNSYLVANIA 15222 No. 4 Gateway Cantor 6ldg. Poem 1406 Tat (412) 261-2156
ST. LOUIS. MISSOURI 63166
600 N. Lindbergh 6hd.
,
Tat (314) Wydown 3-1000
SAN PRANCICSO BAY AREA 2710 Lofayana. Santa Clara. Calf. 95052 Tat (406) 243-0414
SEATTLE. WASHINGTON 98104 Sit Waatam Avanua
7* (206) Main 2-4303
.
SPRINGFIELD. MASSACHUSETTS 01101 730 WorcesterAva.
Tat (413) 756-6911
WILMINGTON. DELAWARE 19B03
2005 Concord Pika. Pokfox Tat (302) Olympia 6-5531
Additional Dlatrict Offlcai art maintained ay:
Agricultural Division
EL DORADO. ARKANSAS 71731 Smeckovei Highway P. 0. tom 231 Tel. (Ml) Union 3-31 SI
LULING. LOUISIANA 70070 a. o. Sox i74 Tel (S04) 7S4-2911
tutlding Products Department
ST. LOUIS. MISSOURI S31SS too N. Undeergh Shid. Tat (314) Wydown 3-1000
LOS ANGELES. CALIFORNIA SOOtt SI 4 San Famanso Read TaL (21S) CA. 2-S111
Cbomstrand Company Division
AKRON. OHIO 44313 3030 Watt Meikat St TaL (211) Temele S-7S41
-
CHARLOTTE. NORTH CAROLINA 23202 Wachovia Sank Building 121 Watt Trada Si
Tal. (704) 37S-SS71
NEW YORK. NEW YORK 10001 3M Fifth Aye.
Tal. (212) SSt-9100
ENGLEWOOD CUFFS. N. J. SSI Pakeodea Aye. Englewood Ckfft. New Jetoey 07831 Tal. (201) MS-21 SI
Hydrocarbons I Polymers Olvtsion lion Oil
EL DORADO. ARKANSAS 71730 Lien Oil Building Tal. (Ml) Urnon 3-3111
JACKSON. MISSISSIPPI 38208 P. 0. tea 10937 Weadand Station ToL (Ml) Fleetwood 2-3849
LITTLE ROCK. ARKANSAS 72203 tfIS Waat Seventh St TeL (Ml) Franklin t-2437
MEMPHIS TENNESSEE 39101 1023 Riyaraida Ome P. 0.30x252
ToL (Ml) WIM0h9K'l*44S1
Organic ChorniesIs Division (Author tndurtry)
AKRON. OHIO 44311 820 Brown Seat! P 0. Soi 2M7 Tat (211) Hemlock 4-1321
MONSANTO, 900 N. LINDBERGH BL0., ST. LOUIS, MISSOURI 03100
V.
J
tno chi i unto m m
CORN
FUNCTIONAL flfiTiffiTiifil
FLUIDS
00029I
TOWOLDMONOOQ2678
6BRN 000292
HONSANTO. tOO N. LINDBERGH BlVD., ST. LOUIS. MISSOURI 03100
TOWOLDMONOOQ2679