Document MJ6D71GXvVM2NEe7ndE1rmp89

* X >( j.Ai' V ,i 4I1 . 1 f! I a* Tho Aroclor* dielectrics are a range of chlorinated diphenyls pro duced by Monsanto for tho manufacture of impregnated paper capacitors. These products are gcnerically known as `askftrels', that Is, synthetic fire resistant Insulating liquids which, If decomposed by an electric arc, evolve only non-explosive gaseous mixtures. The Aroclor liquids were first used in the United States (n 1931 and to-day they are extensively used in the capacitor industry through out the world. Monsanto has been producing Aroclor at Its Newport plant since 1951. There are three grades of Aroclor, identified by their code numbers: Aroclor 1242 (Commercially known as Trichlorodiphenyl) the most economically attractive, is essential for outdoor capacitors in a low temperature environment, but is the most difficult to handle In production. ' Aroclor 1248 (Commercially known as Tetrachlorodlphenyl) is a compromise between the economic advantages of 1242 and the ease of handling of 1254. . Aroclor 1254 (Commercially known as Pentaohlorodlphenyl) Is tho easiest to handle In production and is sometimes chosen for capacitors to operate in exceptionally hot environments, but does not gain the maximum economic advantage. Advantages of using Aroclor Reduced else capacitors arc possible for a givon rating; fluorescent lighting units are a particular application in Mich this is utilised. Reduced raw material cost arising from tho smaller quantity of paper nnd foil needed in manufacture. * Aroclor is a Registered Trado Mark. 0221628 TOWOLDMON0026269 WATER_PCB-00010738 INTRODUCTION * Tho Advantages of Aroclor PROPERTIES Composition Physical Properties Viscosity Vapour Pressure Chemical Properties Electrical Properties Permittivity Loss Tangent D.C. Resistivity CONSTRUCTION OF AROCLOR CAPACITORS Paper Assembly of Capacitors . PRODUCTION OF AROCLOR CAPACITORS Earth Treatment Impregnation ' PERFORMANCE OF AROCLOR CAPACITORS A.C. Capacitors D.C. Capacitors 17 17 17 18 18 19 20 20 TOXICITY AND HANDLING PRECAUTIONS APPENDIX A laboratory Measurements on Aroclor APPENDIX B Compatibility Testing Method 02Zlb*9 23 23 TOWOLDMON0026270 WATER PCB-00010739 Reduced labour content bccauso of the fewer windings required. Increased through-put from a given plant capacity with existing labour force. Higher stress operation of capacitors Is possible because of a more uniform permittivity In the capacitor. Longer lifo capacitors are produced because of the high stability and resistance to oxidation of Aroclor. Small fire hazard because Aroclor is fire-resistant. 0221630 i 4I TOWOLDMON0026271 WATER_PCB-00010740 -Values for the most Important properties of the Aroclor dielectrics are given in the Table. . Typical properties of the Aroclor dielectrics (These values do not constitute a specification) Property Aroclor 1242 Aroclor 1248 Aroclor 1254 Relative Density at 20/20'C Pour Point O'C) Viscosity at 80'C (cS) Coefficient of expansion *C Specific heat at 75'C (J/g *C) Thermal conductivity at 75C (W/m *C) Evaporation loss (%) <2 h at 1255C) Plash Point OC) ASTM D93/62 Fire Point Refractive Index Inorganic chlorides (ppm) .. . Acid number (mgKOIl/g) Water content (ppm) Permittivity at 20'C and 80 c/s Permittivity at 100'C and 50 c/s Loss tangent at 100'C and 50 c/s D.C. resistivity at lOCC and 600 V/mm after 1 min. electricification (T fl cm) Dielect ric strength at 20*0 (kV) (B.8.148:1050) 1-385 -19 95 000068 1-24 0-1039 012 154 (min) None 1-6240 0-1 (max) 001 (max) 85 (max) 697 483 0-018 1456 -7 52 0 00070 1-16 01003 0<I7 154 (min) Nono 1-6295 0-1 (max) 0-01 (max) 85 (max) 558 467 0015 1-649 + 10 102 000066 1-08 0-09743 003 204 (min) None 16370 01 (max) 001 (max) 85 (max) 5-04 4-25 0010 60 50 (min) 7-0 60 (min) 80 70 (min) 0221631 Composition Aroclor is made by the chlorination of diphenyl to predetermined chlorine contents which are indicated as a percentage by the last two digits in theeode number e.g. Aroclor 1218 oontains 48 % chlorino by weight. Each Aroclor contains a range of Chlorodiphcnyls with differing numbers of hydrogen atoms substituted by chlorine, and in each of theso ehlorodiphenyls thcro Is abundant isomerism, Physical properties Viscosity Tho viscosity-temperature characteristics of tlio Aroclor liquids aro shown in Figure 1. It can bo seon that Aroclor 12M is tho most viscous at all temporatures and Aroclor 1242 tho least. Tho differences betweon tho threo grades aro greatest at lower tempera- 6 TOWOLDMON0026272 WATER_PCB-00010741 turc and become Jess as the temperature is raised, As previously explained, Aroclor consists of a number of homologues and conse quently each grade does not have a sharply defined molting point, but remains liquid over a wide temperature range, Instead, tlioir viscosities increase smoothly but sharply as the temperature is reduced. Aroclor 1242 has the lowest pour point of all three grades. Vapour Pressure It can be seen that Aroclor 1242 hfts the greatest vapour pressure at a given temperature and Aroclor 1254 the least, and this needs to be considered when deciding the temperature of Aroclor during degasification and impregnation, Tho vapour pres sure of Aroclor varies with absolute temperature according to tho visual logarithmic law. The variation of the vapour pressures of the Aroclor dielectrics with temperature is Shown in Figure 2. Chemical properties The chemical inertness of Aroclor is outstanding. The liquids are not oxidised by exposure to air or oxygen even under extreme condi tions of temperature and pressure, nor do they react with moisture. When subjected to a bomb test at 1405C in oxygen at a pressure of 250 p.s.i.g. (17 kg/'em*), there was no evidence of oxidation as judged by development of acidity or formation of sludge. They can withstand i. many years of service in electrical equipment at high temperatures without oxidation. Aroclor is manufactured to a rigid specification ensuring a low Initial value for free acidity and free chlorides. Tests have shown that these low values are maintained even when the liquids are heated for prolonged periods in the presence of air an(l moisture at temperatures of 100C. Aroclor 1242 is slightly sensitive to ultra-violet light, which can result in the formation of traces of ionic contaminants. Tho other grades are relatively unaffected by exposure to light. Aroclor undergoes no decomposition at temperatures up to 175 C. At much higher temperatures, or when subjected to afes, the prin. cipal decomposition products are carbon atid hydrogen chloride. .Laboratory tests and practical experience have shown that phosgene, chlorine, or hydrocarbons are not formed as decomposition products of Aroclor. . 0221632 Electrical properties The laboratory methods used to measure tho electrical properties of the Aroclor dielectrics aro described in Appendix A. Permittivity (Dielectric *cortslant')ThopormHtivity ofAroclor is high er than that of minoral oil, which accounts for the eisjc reduction 6 TOWOLDMON0026273 WATER_PCB-00010742 ---p- and Increase in stress that is possible. Stresses of 15 to 17 V/gm are common with Aroelor and higher values aro reported. Since chlorinated diphenyls are polar compounds, their permittivi ties are highly temperaturo-depondent. This Is illustrated in the upper part of Figure 4, which shows the variation with temporature of the permittivity of each of the three grades of AroCior. These readings were taken at a frequency of 50 c,'s And an electric stress of 1 Vfpm. . 'At the lowest temperatures, all three grades have a perrrtittivity of about 2-8, since, because of the very high viscosity, there is no con tribution from dipole orientation polarizability. As the temporature is increased, the permittivity begins to increase when the viscosity becomes sufficiently reduced to allow the molecular dipoles to orientate themselves in the alternating electric field. The tempera ture at which this increase in permittivity begins is dependent upon both the grade of Aroelor, being lowest for Aroolor 1212, and the frequency of the applied field. As the temperature is further increased, the permittivity passes through a maximum, and then decreases. This decrease in permit tivity with increase of temperature is due mainly to the disturbance of the alignment of the dipoles by thermal agitation. The maximum permittivities attained vary with the grade of Aroolor. boipg great est for Aroolor 1242 and least for Aroolor 1254. With Aroolor 1242 the permittivity of this series reaches a maximum, and a further reduc tion in chlorine content causes a reduction in permittivity, as shown in Figure 3.' Althoughtlio permittivity ofAroelor 1242 is of a high order,continued research on these products has revealed the possibility of obtaining even higher permittivities with this class of material. It ip likely therefore, that the final word has not been written on this subject and that improved products will become available in this field in the coui'se of the next few years. 0231633 Z.oss Tangent The loss tangent, or power factor, of Aroelor is also highly temporature dependent. Tills Is illustrated in the lower part of Figuro 4, which shows how tlio loss tangents plotted heto on a logarithmic scale of each of the three grades of Aroelor vary with temperature. Tlio curve for each grade ofAroelor consists of a peak due to absorp tion associated with tho transition in permittivity, followed by a region whero the loss tangent steadily increases with temperature. In this latter region, tho loss tangent follows tho increase in fluidity with increasing temporature and is highly dependent upon tho purity of tho Aroelor. Tho temperature at which tho peak occurs is about 19 - bolow tho pour point. TOWOLDMON0026274 WATER_PCB-00010743 !,) Tho loss tangent of Aroclor Is greater than that of fresh mineral oil, but by seloction of a paper of lower density tho loss tangent or tho Impregnated capacitor can bo minimised without sacrificing tho economic advantages. Furthermore, the internal tetnperature does not rise beyond acceptable values. D.C. Resistivity The values quoted in the table are typical for Aroclor as produced, but they can be improved by vacuum dehydration and values of 20 to 60 T 0 cm at 100'C are common. The values for Aroclor 1212 and 1248 are lower than 1254 because a given amount of contamination reduces the d.c. resistivity more with a liquid of lower viscosity and higher permittivity, The variation of the d.c. resistivity of the 3 grades Of Aroclor with temperature is shown In Figure 5. I II !I 0Z216J* _LM TOWOLDMON0026275 WATEFLPCB-00010744 toss U N G E N T I. >I1 I TOLVME HCJISTfTITT (T J ta n ) tlI ! V..' J I . 7. >"' ; ^64o I Figure 6 The variation of tho DC resistivity of the Aroctor dielectrics with tomperaturo I 54 ` TOWOLDMON0026281 WATER_PCB-00010750 -T I : ;!! i! ; ' ;r ii WATER_PCB-00010751 CONSTRUCTION OF AROCLOR CAPACITORS Paper Kraft paper is strongly recommended since it has nearly 5 times the acid neutralising properties of rag tissue. The permittivity of impregnated paper depends upon the density of tho paper as well as the permittivity of the impregnant, This rela tionship is shown if Figure 6 for the 3 grades of Aroclor and for mineral oil, the values being calculated at a temperature of 20"C. Since paper impregnated with Aroclor 1242 has the highest per mittivity, the least area of windings is needed to obtain a given value of capacitance and the greatest economy is obtained. It is advantageous to use low density paper Since It has been shown both theoretically and practically that such paper gives the least , dielectric loss in a capacitor. This effect arises from the distribution of electrical stress between the cellulose fibres and the impregnant and is in addition to, and independent of, apy losses in the impreg nant itself. Most manufacturers of capacitor tissue are familiar with Aroclor and have developed suitable grades for use with it. Assembly of capacitors It cannot be emphasised too strongly that every material ^hat comes into contact with Aroclor must be carefully checked tot compati bility. Aroclor is a good solvent for many thermoplastics and elastomers and tho resulting solution has a high dielectric loss tangent. Materials which must be considered include the major insulation, the lead-through insulators, any means of scaling the container and tho residues from the manufacturing process c.g. fluxes left after soldering. Tho windings should bo sealed with a suitable adhesive such as gum arable or Gloy. Connection tags If of copper should bo tinned, othcrwise stainless steel can be used. Soldering should ho kept to a minimum and whoro possiblo tho special cored solders which have been developed by manufacturers for use with Aroclor phould bo employed. Opaquo bushings must bo used because of tho slight light eonsltivity of some grades of Aroclor, particularly Aroclof 1242. TOWOLDMON0026284 WATER_PCB-00010753 02216*3 PRODUCTION OF AROCIOR CAPACITORS Although tho production of Aroclor impregnated capacitors is generally similar to that of oil impregnated units, and similar plant may be used, there are soveral differences in detail And theso are described in the following sections. If an oil plant is to be changed to Aroclor, no special cleaning is necessary, although it is advisable to rinse the plant first with Aroclor which is subsequently discarded. It must bo noted at this point and always borne in mind that Aroclor has a very considerable detergent effect. That is to say that since the density is hearly twice that of oil, any dirt existing in the system will be washed out due to the greater density effect of the Aroclor. Earth treatment The main difference between Aroclor and oil capacitor impregnation . plant is the earth treatment section. Aroclor, as received in drams, is suitable for filling into capacitors after vacuum treatment but it is generally advisable to have an earth treating facility available to treat any Aroclor which could become contaminated during tho process cycle. For example if capacitors are filled by a flooding technique, then Aroclor which is unused and which is returned to the system will be found to be slightly contaminatecj and earth treatment is advised. For this to bo fully appreciated, it must be realised that the Aroclor liquids are more susceptible to contamina tion than their mineral oil counterpart. Because of their higher solvent action and higher permittivity, the contamination level which would be acceptable in mineral oil and which is commonly encountered in an impregnation plant will bo unacceptable for Aroclor. The earth treatment can be carried out in two principal ways. In the first place the earth is contained in a column and the liquid is circulated until the contamination is removed. Altcrna- tively, activated earth is added to tho liquid in a container and it is stirred to ensuro intimato mixing and then the earth is filtered through a normal paper filter. In both cases either Fuller's Earth or Alumina may bo used and each must ho activated. It has been found by experience in laboratory tests that the earth may bo over activated and tho optimum temperature is about 100 C for 6 hours. If this is tlion added in quantities to tho material to bo treated, It Is OZZlfcqq ensured that tho fresh activated oarth is utod each tlmo and the TOWOLDMON0026285 WATEFLPCB-00010754 treatment may bo more easily controlled in this way In the mixing technique. However, thoro still exists tlio problom of separating the earth and here tlio column technique has a considerable advantage, since circulation through the column floes not necessitate further filtration. This method has the disaflvantage that the column gradually becomes less active during its life and there is not always tho same degree of control over the treatment process. Impregnation it is customary to store the capacitor liquid in a large tank the size , of which depends on whether the material is delivered in drums or tankers. It is strongly recommended that these storage tanks be lagged and heated since at low temperatures difficulty would be , encountered in pumping the Aroclor 1254 and in certain extremes of temperature even Aroelor 1242 can become unpurnpable. After transfer from the storage tank the liquid is first earth treated and mixed with any unused liquid drawn back from the capacitor Impregnation tank, if applicable. The treated liquid is then sub jected to vacuum drying and de-gassing In exactly the same way as with mineral oil and after this process it is passed to the final storage vessel where it is held before being passed to the impregna tion section. Aroclor capacitors may be vacuum impregnated by a manifold technique in which the liquid is piped individually to each capacitor can and this is perhaps more suitable for the larger power factor correction capacitors. Alternatively, they majr be filled by ft flooding technique which is more applicable to the smaller fluores cent lighting capacitors. Here the capacitors can be goaded in wire cages and completely immersed in the liquid in the same way as with mineral oil. For the actual impregnation cycle the following temperatures are recommended: Aroclor 1242 70- 80"C Aroclor 1248/1254 90-100'C ' The lower impregnation temperatures are recommended for Aroclor 1242 since as this process Is carried out under vacuum the losses will be greater with a liquid which Is more volatile! After the Impregnation cycle has been completed the vessel should be cooled to below 50'C before being opened and this Is to avoid the unpleasant fumes of Aroclor escaping fnto the work-shop. The capacitors should thenbo sealed as quickly as possible and degreased beforo final painting and testing. Toxicity precautions nnd the handling of Aroclor is dqalt with in a separate section but workers handling tho liquid, Or capacitors coated with it, are advised to wear rubber gloves of uso barrier cream. 1 0221*** TOWOLDMON0026286 WATER_PCB-00010755 PERFORMANCE OF AROCLOR CAPACITORS A.C. capacitors at If a capacitor is continuously energised before and whilst subjected law ambient temperatures to a low temperature environment it operates satisfactorily because the heat produced in the dielectric balances the heat lost from the case. A self-compensating process exists Biich that if the tempera ture of the dielectric falls the losses increase, and more heat is generated to establish a new equilibrium. 'Tests have shown that a capacitor impregnated with Aroclor 1254 can operate continuously energised in ambient temperatures down to -60C, and it was found that such capacitors satisfactorily survived whilst installed out doors during the winter 1052-3. If, however, a capacitor is subjected to a low temperature environ ment first and then energised it may be damaged by discharges occurring in voids formed by the contraction of the dielectric before it has time to heat up sufficiently. Cases when this might occur are in streot lighting capacitors during winter, or capacitors installed in a plant that has been shut down during winter holiday periods. For this reason, the following minimum ambient temperatures are suggested for the 3 grades: Aroclor 1254 - 7C ' . Aroclor 1248 -28C > f\ Aroclor 1312 -38'C For operation at still lower temperatures a blend of Aroclor 1254 and trichlorobenzeno lias been used. , D.C. capacitors Aroclor is also used in d.c. capacitors but it has been found that at the high stresses used tho service life of tho capacitor tends to bo reduced if tho working temperature is raised above 40 C. This can be ' overcomo by using stabilisers in tho Aroclor to overcomo tho slight electrochemical degradation which tends to take place. Dencrally I, the effect is proportional to tho quantity of stabiliser used and up to 1 per cont of antliraquinono or 2-cthyl anthrnquiponc and 2 per cent of nzobonzono havo been used. 20 --------------------------- " '! TOWOLDMON0026287 WATER_PCB-00010756 TOXICITY AND HANDLING PRECAUTIONS Aroclor made by Monsanto has been used for over 30 years without causing any toxic effects, but it mutt be handled with care. These precautions should bo observed: 1 Avoid skin contact. Protect the hands, preferably by oil-resistant gloves. 2 If skin contact should occur, wash off with soap and water, 3 If hot Aroclor must be handled in a closed or confined area provide exhaust ventilation or Wear an approved respirator. i If Aroclor gets in the eyes, flush with large amounts of water. In the event that irritation persists refer the patient to a Physician. 6 Infrequent exposure to Aroclor vapour will not cause any ill effect, but prolonged exposure to a high vapour concentration should be avoided. If these precautions are neglected acne may develop and excessive exposure may cause liver damage. 02*16*7 TOWOLDMON0026288 WATER_PCB-00010757 LABORATORY MEASUREMENTS ON AROCLOR The Monsanto There are many test cells available for measuring the electric dielectric test cell properties of liquid dielectrics, but since most of these were de signed for use With mineral oil, Monsanto has designed a test cell especially for use with Aroclor. This de$ign of cell is used in our laboratories and is available for sale to customers. It ig essentially a . three terminal cell with cylindrical stainless steel electrodes separated by a 1 mm gap. Figure 7 shows details of the construction of this cell. The procedure for Great care must be taken to ensure careful cleaning for Aroclor Cleaning and filling the cell measurements with this or any other cell. Tho Monsanto cell is designed for easy cleaning and accurate assembly. The Monsanto cell is first cleaned by a series of thorough washings as follows: ' 1 A wash with benzene 2 A thorough washing with detergent and hot tap water 3 Repeated rinsing with hot tap water 4 6 rinses in distilled water . 6 2 rinses in analytical grade acetone During the wash with the powder detergent a soft hair brush is used and all parts of tho electrodes are thoroughly brushed. The cell is then dried in an air oven at ljpC for 30 minutes. Finally it is rinsed twice with the Aroclor to bo measured before filling a third time, when tho electrical measurements are taken. Measurements The temperature at which the electrical properties are made is measured by, a thermometer resting in the central well pf the coll. For routine tests a temperature of 100'C is used. Permittivity and loss tangent are measured first with a transformer bridge at a stress of 1 V/|xm and at mains frequency of &0 c s. D.C. resistivity is then measured with an electronic megohtnotcr one minute after the application of a stress of 0-5 V/ym. If repeated readings of d.c. resistivity aro performed on tho samo quantity of Aroclor in tho cell, a gradual increase is noted. It is therefore recommended that if a repeat measurement of resistivity is re : qulred, tho coll bo emptied, thoroughly cleaned, and then refilled. ' 22 02216*8 TOWOLDMON0026289 WATEFLPCB-00010758 Process control measurements For operating an impregnation plant, it i$ convenient to be able to measure tho electrical properties of the Aroclor without the necesslty of taking samples, and a coll can be incorporated In the system c.g, in a flow lino. It should be arranged that there is a turbulent ' flow of Aroclor through the gap between the electrodes except when a measurement is being taken so that adequate cleaning of the electrode surfaces occurs. To obtain the Same value Of d,c, resis tivity with a plant cell and with a laboratory cell it is necessary for the Aroclor to bo (I) stationary whilst the measurement is made, _ (2) subjected to the electric field for one minute, and (3) at the same temperature. Procedure If the material is available in a laminar form or Is a surface coating, apiece 25mm square is cut from a sheet. Other materials are selected so that the sample taken is present at the same concentration as in the finished article. .The sample is put into a glass jar that has previously been cleaned and dried in the following sequence: 1 Wash in benzene 2 Wash with hot water and detergent 8 Bix rinses with distilled water 4 Rinse twice with analytical grade acetone 6 Dry in an oven at 130"C for 1 hour To this jar, and to a similar one without a specimen within it, are added 50 ml of Aroclor. The Jars are then closed with ground glass lids and aged in an oven at 100'C for 7 days. After ageing, tlie jars are removed from the oven and the Electrical properties of the Aroclor in both tho specimen jar and tho control jar are measured at 100"C according to the method described in Appendix A. The specimens are examined for swelling or other signs of deterioration, and any colour change of the Aroclor is noted. oz?ifc<,q Results Tho Aroclor In which tho Bample has been immersed must not ex perience n decrcaso in resistivity below 10 terojim cm. Information on materials which have boon tested is available on request. . TOWOLDMON0026290 WATER_PCB-00010759 Technical Service Tho technical service staff of Monsanto Is always ready to provide additional Informa tion on the use of the materials indicated in this roport, and to assist manufacturers in the solution of particular problems ensuing from their application. . Front cover illustration bp courtesy >/ Industria Condensatori Applicazioni ElcttroeleUroniche Milano Every effort has bee made to ensure that the information in this publication in reliable, but as the conditions under which it may bo applied arc beyond onr control, wo cannot accept responsibility for any results of its use. Forme No. P.D, C74-E1-0I1) Published by Monsanto Chemicals Limited, Printed In Ennlnnd by Vaitlkhard & Farnsworth Ltd. Nottingham I I H TOWOLDMON0026291 WATER_PCB-00010760