Document M4wwkJxmNrdemVRYgrLVEVypM

United States Patent [191 Vecchiotti Hi] 3,966,870 145] June 29, 1976 [54] HOLLOW, MULTI-LAYERED, CROSS-LINKED PLASTIC STRUCTURES AND PROCESS FOR PRODUCING SAME [75] Inventor: Camillo M. Vecchiotti, Ridgewood, N.J. [73] Assignee: Amerace Corporation, New York, NY. [22] Filed: Feb. 7, 1975 [21] Appl. No : 548,088 [62] Related U.S. Application Data Division of Ser. No. 410,815, Oct 29, 1973, Pat. No. 3,900,640. [52] [51 ] [58] U.S. Cl................................... 264/255; 260/873; 264/114; 264/310 Int. Cl.2........................B29C 5/04; B29D 9/00; B29D 23/08 Field of Search........... 264/310, 311, 114, 255, 264/240, 270; 260/873, 94.9 GA [56] 2,649,622 2,919,474 3,214,422 3,350,745 3,449,191 References Cited UNITED STATES PATENTS 8/1953 1/1960 10/1965 11/1967 6/1969 Piccard.......................... 264/126 Cole.................................... 264/349 Mageli et al........................ 260/94.9 Schott et al.......................... 264/311 Taylor................................. 156/306 3,455,483 7/1969 Inklaar................................ 264/310 3,816,582 6/1974 Tennyson............................ 264/311 Primary Examiner--Willard E. Hoag Attorney, Agent, or Firm--S. Michael Bender; Gregory J. Battersby [57] ABSTRACT Hollow, multi-layered plastic structures are provided comprising a layer of thermoplastic polyester material and a layer of polyethylene, the polyethylene and polyester layers being cross-linked together at their interface. A process for producing such structures which comprises charging a mold with thermoplastic polyester material, rotating and heating the mold so as to fuse and form a layer of the polyester material on the inner surface of the mold, cooling the mold to a point below the melting point of the polyester but above the melting point of a subsequently added cross-linkable polyethylene material, stopping the ro tation and charging the mold with the cross-linkable polyethylene material, resuming the rotation of the mold and heating it to a temperature sufficient to fuse and cross-link the polyethylene with the polyester layer, cooling the mold to a point below the melting point of the polyethylene and removing the finished structure from the mold. 6 Claims, No Drawings 3,966,870 56 chamber where the biaxial rotation was maintained and the melting point of the polyethylene and sufficiently a fan directed on the mold for 7 minutes to set the below the melting point of the polyester so as not to polyester layer within. The spindle was then indexed cause dimensional distortion of the polyester; rotating with the mold to a load-unload station where rotation the polyethylene charged mold for a sufficient period was stopped and the Teflon plug removed from the 5 of time to firse said polyethylene, uniformly distribute filling opening in the mold end opening cover. Through the polyethylene on the inner surface of the polyester this filler opening, 15 lbs. of cross-linkable polyethy layer and effect cross-linking of said polyethylene so as lene (FLAMOLIN MF-15711) in finely divided pow to set the polyethylene layer and effect cross-linking of der form of about 50 mesh was dumped into the mold said polyethylene to said linear polyester; and stopping and the filling plug replaced in the mold cover. Biaxial 10 the rotation of said mold to remove the resulting hol rotation was restarted and the spindle was then indexed low, cross-linked multi-layered polymeric structure. with the mold to an oven station set at 450F where it 2. A process as defined in claim 1 wherein said ther was kept for 25 minutes so that a layer of polyethylene moplastic polyester is a glass-fiber filled polyester of was formed on and cross-linked to the polyester layer. terephthalic acid and a glycol of the series HO(CH2)n The speeds and ratio of rotation thereof were the same 15 OH wherein n is a whole number within the range of 2 as employed in the first heating station. At the end of to 10. the second oven cycle the mold was positioned in a 3. A process as defined in claim 2 wherein said cross- cooling chamber where it was subjected to a fan for 8 linkable polyethylene includes a fire retardant agent. minutes followed by a water spray for 10 minutes and 4. A process as defined in claim 3 wherein said cross- then a fan again for 2 minutes; thus lowering the tem 20 linkable polyethylene includes a cross-linking agent perature to a point below the melting point of the poly selected from the group consisting of dicumyl peroxide, ethylene. Following this cooling, the mold was indexed 2-5 dimethyl 2,5-di(t-butyl peroxy) hexane and 2,5- to the unload station where the cover was unclamped dimethyi-2,5-di(t-butyl peroxy) hexyne -3 and a halo- from the mold and set aside. The mold was then tilted genated fire retardant agent. to a 30 angle whereupon the molded battery case 25 5. A process for producing a fire retardant, hollow, dropped out of the mold with a slight pulling force on multi-layered, cross-linked, plastic structure compris the case. After suitable cooling at room temperature, ing the following steps: charging a mold with a suffi the molded case was cut to desired height. The polyes cient amount of a linear, thermoplastic polyester mate ter layer in the finished product had a thickness of approximately 34 inch while the polyethylene layer was 30 rial having a melting point between about 500F to form a substantially about 400F and uniform layer on approximately 0.100 inch thick. the inner surface of said mold biaxially rotating and As used in this description of the invention the term heating said mold to a temperature between about "multi" is intended to encompass two layers of layered 500F and about 650F for a period of time between polymeric material. The above described process may be used in the 35 about 20 and about 30 minutes so as to fuse the polyes ter contained within the mold and uniformly distribute production of a wide variety of structures including said fused polyester on the inner surface of said mold; tanks, containers, vessels, barrels, and the like. Particu cooling said mold while maintaining its biaxial rotation larly useful multi-layered structures produced accord to a temperature between about 280F and about ing to this invention serve as cases for industrial size batteries. Such a case will have an outer surface with 40 350F to stopping set the polyester to a substantially set layer; the rotation of the mold and charging said the characteristic structural strength and other proper mold with a sufficient amount of cross-linkable poly ties of polyester but the added feature of resistivity to ethylene including a cross-linking agent and a fire re chemical attack in its inner surface. tardant agent; biaxially rotating and heating the poly I claim: 45 ethylene charged mold to a temperature between about 1. A process for producing a hollow, multi-layered 425F and about 450F for a period of time between cross-linked, plastic structure from a linear thermoplas about 20 and about 25 minutes so as to uniformly dis tic polyester and a cross-linkable polyethylene having a tribute the polyethylene on the inner surface of the melting point lower than the melting point of the poly polyester layer and effect cross-linking of said polyeth ester, said process comprising the steps of: charging a 50 ylene and said linear polyester at their interface; cool mold with a sufficient amount of the thermoplastic ing said mold to a temperature below the melting point polyester material to form a substantially uniform layer of said polyethylene so as to substantially set the poly on the inner surface of said mold; heating said mold to ethylene layer; and stopping the rotation of said mold a temperature above the melting point of the polyester; to remove the resulting fire retardant, hollow, cross- rotating said mold so as to fuse the polyester contained 55 linked, multi-layered polymeric structure. within the mold and to uniformly distribute the fused 6. A process as defined in claim 5 wherein said cool polyester on the inner surface of the mold; cooling said ing of the mold containing said fused polyester is ef mold to a temperature below the melting point of the fected by exposing the mold to a fan and the cooling of polyester but above that of the cross-linkable polyethy the mold containing both the set polyester layer and the lene thus crystallizing the polyester to a solid layer; 60 fused polyethylene layer is achieved in a three-step stopping the rotation of the mold; charging said mold procedure including exposing the mold to a fan for with a sufficient amount of the cross-linkable polyethy about 8 minutes followed by a water spray for about 10 lene to form a substantially uniform layer on said poly minutes and a fan again for about 2 minutes. ester layer; heating said mold to a temperature above ***** 65