AROCLOR RESINS AND PLASTICIZERS FOR HALF-SECOND CELLULOSE ACE,, TATE BUTYRATE (C.A.B.) May 18, 1954 *#**#*###**###########*#********,***#*#***#*.******.*****
SEP 1 1 '
HALF-SECOND CELLULOSE ACETATE BUTYRATE Excerpts from article by W. M. aearhsrt and F. M. Ball
Official Digest, Vol, 343, August, 1953
I,
TABLE 1."Properties of Cellulose Acetate Butyrate' Type EA6-381
Half-Second 20-Second
Specific gravity
1.20
Wt. per gal., lbs.
10.01
Acetyl content, $
13.00
Butyryl content, $
37.00
Refractive Index 25C.
1.48
Resistance to ultraviolet radla. Excellent
Melting range, C.
140-170
Intrinsic Vise. @ 25C. In acetone 0.6-0.8
1,21 10.08 13.00 37.00
1.48 Excellent
197-204 1.85 "
II.
Solubility of Half-Second Butyrate
"Half-Second Butyrate Is soluble In a blend of ethyl alco hol and toluene. However, the main solvents are esters and ketones. Both esters and ketones tolerate high dilution with alcohols and aromatic hydrooarbons, Half-Second Buty rate Is somewhat like cellulose nitrate In this respect, but dilution with aromatic hydrocarbons can be carried to very high proportions without precipitation. At a 10$ end point, the dilution ratio with acetone Is 8.8 using toluene as the diluent. However, the aliphatic hydrocarbons are not effective diluents.
0613535
TOWOLDMON0037753
TABLE 2
Solvent combinations for Half'-Second Butyrate
Ingredient
Acetone Ethyl Alcohol Toluene Methyl CellOBOlve Methyl Isobutyl Ketone
Composition, wt. ;%
12
24
50 20
15 20 15 50 20
* " 10
20 1 55 20 20 79
5 --
100 100
100 100
The selection of a solvent blend must be made with care because the solvent balance Influences adhesion and film properties. Four.widely different solvent blends which are possible are shown in Table 2.
"When Half-Second Butyrate is dissolved in solvent combi nation 1, the dried film exhibits very good adhesion to glass, metal, and wood; adhesion of films from combinations 2 and 3 is not as good. However, films made from combina tion 2 give higher tensile strength, elongation, and tear resistance than those prepared from combination 1 or 3. Combination 4 is for low cost coating compositions. Further studies are being made."
III.
Plastlolzatlon of Half-Second Butyrate
"Generally those plasticizers which are used with vinyl co polymers may be used with Half-Second Butyrate. Of the plastlolzers studied, oastor oil is the most effective in decreasing film hardness and trlcresyl phosphate is the least effective. Paraplex 0-62, di-2-ethylbutyl phthalate, dibutyl sebaoate, and tetrahydrofurfuryl oleate are inter mediate in effect."
2
0613536
TOWOLDMON0037754
IV.
Modification of Half-Second Butyrate by Resins
"Half-Second Butyrate Is compatible with acrylics, non drying alkyds, silicone alkyds, chlorinated hydroearbons (Aroclors), phenolios, cellulose nitrate, rosin deriva tives, Santollte MHP, vinyl acetate, Vinsol, and dewaxed damar."
V.
Formulations Containing Half-Second Butyrate
"Half-Second Butyrate possesses many properties of Interest to a laoquer formulator, and preliminary work has shown that It Is a versatile raw material. Much work remains to be done in refining formulas that have been made in the laboratory. But to serve those who wish to have basic
formulas to start from, the following information Is pre sented.
TABLE 3.
Lacquers for Paper
Ingredient
Composition, Wt. ft 1 214
Half-Second Butyrate Santollte MHP
Aroolor 1260 Paraplex 0-40
Acetone Isobutyl Acetate
Ethyl Alcohol
Toluene
20 20 20 20 -- 10 - --
-- 20 - -
3 --
--
3
15 10 10
1
22 10 10
10 10 10 17
30 40 30 59
--
--
--
--
100 100 100 100
Nonvolatile, <f> Viscosity, eps.
23 300 -500
. 30 400-600
40 500-700
23 300-:
3 0bV3*i7
TOWOLDMON0037755
"The nonvolatile of lacquer 1 Is almost entirely Half-Second Butyrate plasticized with a small amount of Paraplex 0-40. The solvent combination can be varied considerably to suit the needs of any particular application. This lacquer pro duces a slight curl to paper which Is dried in Individual
sheets. The curl can be partially remedied by a change in the solvent combination or by the use of a resin such as Santolite MHP and Aroelor 1260 as in formulas 2 and 3, The
second formula yields a film with slightly higher gloss than the first. Formulas 3 end 4 are low cost paper lacquers.
TABLE 4.
Clear Lacquers for Metals Brass, Steel, Aluminum
Ingredient
Half-Second Butyrate Rezyl 92-5 (60g) Plaskon RS-2 (44g) Acetone Isobutyl Acetate Ethyl Alcohol Butyl Cellosolve Toluene
Composition, Wt. % 12 15 T2
13 --
- - 2.25 31 16 17 20
9 10
8 9.75 7 30
Nonvolatile, <f> Viscosity, cps.
100 23
80-90
100 13
50-70
"It has been found that a high acetone concentration Is
conducive to good adhesion on metals. However, formula 2 has better all-around adhesion. These lacquers are not affected by a 24-hour immersion in water after the film has dried for three days. The solvent combination can be varied from those shown, but these formulations may be used
as starting points.
4
ObU*38
TOWOLDMONOQ37756
TABLE 5.
Wood Lacquer System
Composition, Wt. %
1 2 34 Filler Sealer Finish Finish
Half-Second Butyrate Arochem 404 Dewaxed damar Aroclor 5460 Paraplex 0-62
Asbestine X Acetone Ethyl Acetate
Isobutyl Acetate Butyl CellOBOlve Ethyl Alcohol
Butyl Alcohol Toluene
Xylene Phenyl Salicylate
7 14
9 10
-- --- --
9 -10
15 -- -- --
... --
45 --
4.5
__ --
- - 4l -- - -
-- 12 12 22 16 13 13
10 8 10
-- 9 14 14
5 -- -- - 6 10 17.25 17.75
13 13 O.25 O.25
--
100
--
100
,
100
_______
100
Nonvolatile, <f> Viscosity, cps.
67 1.4 2000 50-75
22.5 20 40-56 40-57
"These formulas represent our first attempts at wood finishes with this particular polymer. Formula 1 shows the use of
Half-Second Butyrate In a filler, where good clarity Is es sential.
"The second formula shows a sealer composed of Half-Second Butyrate as the only film former In a solvent containing a high proportion of acetone. High acetone concentrations have been found to contribute considerably to adhesion on wood. Such a sealer gives slight clogging at two hours with ordinary sandpaper, but with stearated sandpaper it performs very nicely. Zinc stearate has been omitted in an effort to obtain optimum adhesion throughout the system. A top finish high in aromatic hydrocarbon content will, for the reasons mentioned under the section on solubility, benefit the sealer. The third formula shows a finish that gives good resistance to water and 60-proof alcohol, gives a Sward hardness of 18 at two hours and 40 at 24 hours, has moder ately good oold check resistance, and rubs well after dry ing overnight.
5
TOWOLDMONOQ37757
"The fourth formula Is a result of the observation that de waxed damar gave good tensile strength and elongation. A finish was prepared without plasticizer and applied to a maple panel. This panel was subjected to a wear test on an interior hall floor. It was the only one of a series of lac quers that retained its high gloss after six months of wear. The integrity and color of the film were also very good after this exposure.
TABLE 6.
Laoquers for Plastics
Composition, Wt. %
1 '2 3 4 5
Half-Second Butyrate "5
5
5
Acrylold B-72 (100$6)
--
--
5.5 5 .5 --
Acetone
19 19 19 18 28
.Toluene
-- -- 19 -- 57
Butyl Cellosolve
76 -- 57 73
Diaoetone alcohol
76- - -- -- --
Ethyl alcohol
-- - - 10
Nonvolatile, %
Viscosity, cps. Surface
ICO 100 ICO 100 100
55 5 9 5 13 12 10 14 14
Acrylic Cello Cellulose Cel.
Cel.
and phane nitrate Acetate, Ace.
phenolic
poly acrylic
resins
styrene. poly-
cellulose styrene,
acetate cellu-
butyrate lose
nitrate
"Applications on plastics include polishing, protection, decoration, and silk screening. For decoration and silk screening, pigmentation and increased concentration of non volatile ingredients are required. Half-Second Butyrate
adheres well and gives glossy films on acrylic and phenolic resins, using a solvent combination consisting of acetone and Butyl Cellosolve. On cellophane, better adhesion is ob tained by replacing Butyl Cellosolve with diacetone alcohol.
The addition of a small amount of toluene to the first lac-
6
0613540
TOWOLDMONOQ37758
quer permits application on cellulose nitrate. In order to get satisfactory results on cellulose acetate, cellu lose acetate butyrate, and both high- and low- impact poly
styrene, it was necessary in formula 4 to use Acryloid B-72, No doubt some variation in solvent combination can be made, (see formula 5) but these formulations can be used success fully.
TABLE 7.
Heat-Sealing Adhesives
Ingredient
Half-Second Butyrate Vinyl Acetate (AYAA) Vinsol Acetone Isopropyl alcohol Toluene VM and P naphtha
Composition, Wt. % 12 1(3 10
15 -- - 15 40 40 10 10
15 15 10 10
100 100
Nonvolatile, % Viscosity, cps.
25 40-50
25 30-38
Behavior of Coated Paper to Uncoated Paper
Blocking temperature (1 psl., 24 Hr.)
Over 175F.
130F.
Heat-sealing property (200F., 50 psi., 5 sec.)
Very good
Very good
"The first adhesive is water white and of high qualluy, whereas the second is colored brown and is of the low-cost type. The Half-Second Butyrate serves to reduce the block
ing tendencies of vinyl aoetate without interfering with its heat sealing properties. The blocking temperature of the second adhesive may be raised by increasing the HalfSecond Butyrate content. Other modifying resins useful in
this application are Abalyn, Flexalyn C, Newport V-40, Neolyn 40, Paraplex d-40, Heresite RO-88, and Santolite MHP.
7
06135*1
TOWOLDMONOQ37759
TABLE 8.
Melt Coating for Paper and Cloth*
Ingredient
.
Wt. %
Wt. %
Half-Second Butyrate Dioctyl phthalate
Aroclor 1260 Ionol
60 39.9
0.1
50
9.9 40
0.1
Applied at 350F.
100
100
"These coatings have extremely good flexibility. They may be prepared by heating the plasticizer to 350F., then add ing the Half-Second Butyrate with agitation. The melt coat ing may be applied by a knife and rolled smooth if desired. This application requires no solvent, and it is possible to apply films of almost unlimited thickness. To prevent
development of color and odor, the melt should be kept hot for as short a time as possible. Such a melt coating may be pigmented for exterior exposure. For such use, it is suggested that phenyl salicylate and Ionol be incorporated,
as shown in Table 9. The former absorbs radiation, and tho latter acts as an antioxidant.
TABLE 9.
Melt Coating for Fiberboard*
Ingredient
Wt. %
Half-Second Butyrate Dioctyl phthalate Asbestine X
T1 Pure R-110 Phenyl salicylate Ionol
30.0 20.0 40,0
9.6
0.3 0.1
Applied at 350F.
100.0
8 ObiI**2
TOWOLDMONOQ37760
"Half-Second Butyrate also has possibilities in quick-gelling lacquers automotive finishes, alkyd varnishes, and hot-spray laoquers. Tests are already in progress on these applications and this information will be published as soon as possible."
VI.
Summary
"Half-Second Butyrate overcomes the obstacles of viscosity and adhesion which held back other medium butyryl esters. It dissolves quickly, has good clarity, is light stable, and has good film properties. It is soluble in esters and ketones, although a blend of 80 toluene and 20 ethyl alcohol will also dissolve it. Generally, those plasticizers used with vinyl copolymers may be used with it. It is compatible with many coatings resins.
"Half-Second Butyrate is a versatile raw material. It can be used to prepare lacquers for paper, metal, wood, and plastlosj heat sealing adhesivesj and melt coatings."
9 ***#*End of Bulletin*****
P0B;MS-400-5/l8/54
Printed in U. S. A.
06135<>3
TOWOLDMONOQ37761