Document LJYXZOyRoO1KwJkb3n1Qy7zoz

UNION CARBIDE CORPORATION MINING AND METALS DIVISION 270 PARK AVENUE, NEW YORK, NEW YORK 10017 UNION CARBIDE HIGH-PURITY ASBESTOS A UNIQUE FIBROUS SOFTENING AGENT AND RETENTION AID FOR TISSUE AND TOWELS PROVIDES FEXIBILITY; DRAPE; VELVET SURFACE FEEL CLARK SOFTNESS VALUES : BLEACHED SULFITE UNFILLED-----------9.5 SAME WITH 5% ASBESTOS --14.1 PLUS IMPROVED RETENTION OF CELLULOSE FINES AND FILLERS SEE ATTACHED GRAPHS AND MILL TRIAL DATA UCC 001803 APPLICATION SOFTNESS FOR FACIAL TISSUE Purpose of Trial: Improve overall softness and reduce raw material costs. Type of Paper Machine: Yankee -- 120" Trim with 75/58 mesh wire Machine Speed: 1000 ft./min. with 10% Crepe Production Rate: 20 tons/day Furnish (in use): 10% Kraft Bleached Hardwood ($90 per ton) 66% Spruce Sulfite ($150 per ton) 24% Broke ($130 per ton) Furnish Possible Using 4% High Purity Asbestos: 29% Kraft Bleached Hardwood ($90 per ton) 43% Kraft Bleached Pine ($110 per ton) 24% Broke ($102 per ton) 4% Asbestos ($ 150/ton) Furnish Cost... $139 per ton paper $110 per ton paper Savings to paper company per year (300 days) ........................................................................................................$174,000 Economic Gain and Quality Improvement: This trial indicated that this paper company can save $174,000 per year in their facial operation alone. High Purity Asbestos was evaluated at the 2%, 4%, and 6% level. A panel of people experienced in evaluating facial tissue handfeel judged the 4 and 6% asbestos content paper the best they had felt for handfeel. A side benefit was noted by the paper company people--that the asbestos contributed to more uniform formation. Physical Characteristics of the Facial Tissue: Percent Asbestos: Basis Weight (Lbs./3000 ft.*) Bulk or Caliper (Std. Test) Machine Direction Tensile (oz./15 mm strip) Cross Direction Tensile (oz./15 mm strip) Tensile Ratio (M.D./C.D.) Absorption (seconds/.01 ml) 0% 11.53 32 9.3 4.8 2.0 5 2% 10.96 31 8.6 3.8 2.2 5 4% 10.66 30.9 7.1 3.4 2.1 5 4-6% 10.94 31.2 5.1 2.6 2.0 5 RESULT OF THIS WORK WITH THIS PAPER COMPANY: This company now uses asbestos in all products: tissue, towels, and facial tissue. UCC 001804 SOFTNESS AND FORMATION Another example of paper properties experienced with High Purity Asbestos additions is illustrated in Table 1. High Purity Avhestos was added to a 30 lb. wet creped towel and softness was found to improve over 20%. Additional benefits included improvements in wet tear. % stretch, and an obvious reduction of solids in the clarified water at the effluent of the saveall. TABLE I TRIAL DATA Basis Weight (Ibs./24"x36"x48'') Softness (Crush Test) Bulk (4 ply cap.) % Stretch Wet Tensile Aged (one inch strip aged in oven at I08CC for 10 min.) Machine Direction Cross Direction Dry Tensile (one inch strip) Machine Direction Cross Direction Wet Tear Machine Direction Cross Direction Absorbency (I /1 Occ) Seconds No Aubnliu 30.0 2200 0.267 6.5 2.7 1.7 9.6 5.7 30 34 35 Wtlh Aibfglos in Ppcr 2% 3% 4% 30.1 29.8 30.4 1700 1680 1680 0.268 0.266 0.274 7.4 7.2 7.1 2.8 2.7 -- 1.5 1.6 9.3 8.6 -- 5.5 5.5 36 42 -- 42 52 33 35 Formation improvements are often dramatic with High Purity Asbestos addition. UCC 001805 Asbestos softening of a 40-lb. towel. UCC 001806 TEAR FACTOR SOFTNESS UNITS % ASBESTOS IN HANDSHEET % CHEMICAL SOFTENER x IO'1 Effects of asbestos on paper softness and tear (kraft pulp,standard weight). UCC 001807 Asbestos improving aged towel absorbency. UCC 001808