Document LJXR1r27YOdk6eaba5O3ooDD5

f 1. ' [Monsanto : \ FROM (NAME * LOCATION) 1 . . j. i jT. C. Mathis - St. Louis Organic Research |. OATS UJCT REFERENCE TO December 22, 19^7 mead: packaging work: request #67-161 K. A> Wells, KWELL Farrar, Res. 1 Darby, Res._JL__ jm. uoaKeirr~ResT~^) J. A. Cannon, Res. 3 N. W. Touchette, Res. 3 C. D. Bias, Res. 3 R. H. Mills, Res. 3 R. M. Parks, RPARK W. F. Waychoff, WWAYC E. C. Wilde, EWILD ' J. S. Bagnall, JBAGN Tests for water resistance, heat resistance, and wet tack did not show superiority of our plasticizers over the Mead control. Four out of five of the Monsanto plasticizer blends showed equivalence in these tests, and gave strong resistance to delamination under the test conditions. Perhaps the plasti cizer performances are too similar for these tests to dis criminate. The blends showing equivalence to the control plasticizer in the iAC-59 emulsion are these: 1) jSanticizer 218a (S-l6o/S-l4l/DIBP 75/15/10) 2) S-218A/A-1254 (90/10) ' 3) S-218A/S-8 (90/10) 4) S-160/A-1254 (80/20) S-l6p/S-8 (80/20) gave inferior performance as described in later discussion. I haye two unanswered questions: l) Could we better discriminate between plasticizers by changing the test methods used by Mead? 2) Since Mead proposes to market an Improved soda carrying |case and since their wet tack is very slow, is it possible jthat they have gained resistance to delamination at too biuch sacrifice in wet tack? In yiour call report dated November 7, 1967, I note that Santlolite MHP, used as a tackifier, has been removed from their emuljsion systems. Knowledge that they are altering their system, combined with lack of experience with adhesives, leaves me rjeluctant to make any recommendations other than that we try to giet more information before we do more work. - DSW 586959 STLCOPCB4092293 To; K. A. Wells 2- - December 22, 1967 My experiences with the tests were briefly as follows; Wet Tack -- fiber tear on kraft paper I was unable to determine a time to tear due to slow tack. The method was the same as that used in Request No. 67-114 (a 2-inch, 5-mil film). Heat Age Tests This test was started at 140F raising the temperature in 20 increments. S-I60/S-8 (80/20) failed at 200F. The test was terminated at 480F because no other test specimens failed. In a repeat test the specimens were entered in an oven adjusted to 550F. Only S-I60/S-8 (80/20) failed during 52 hours at this temperature. This failure occurred at two hours. Water Resistance Tests These tests were carried out at 5^F and 90F> The 54F test was continued for 48 hours. Only S-I60/S-8 (80/20) failed. This: occurred during the last 8 hours of the 48-hour period. The 90F test was done twice. Results.did not check but the average time to failure for each system.'was roughly 7 to 8 hours. Ken,: do you know or can you learn the conditions of time, pressure, and temperature under which the soda cartons are glued together, and do they actually use a 10-mil film as pre scribed by the test method? Due to the very slow tack develop ment, I had to be very careful to avoid having the top portion of the carton slide before tack developed between it and the lower portion of carton. I suppose the acrylic latex coating may have contributed to this problem. We would appreciate any Information regarding how this operation is carried out. In the progress of this work there was no instance of box fibejr tear at failure. In the water resistance tests the separations appear to be primarily separation within the adhe'jsive itself. I believe most of the adhesive stays on the white surface rather than on the brown (backside) surface. Time:; 24 hours k- DS\N 586960 STLCOPCB4092294