Document KGoNN5aGKK4mxOjE818NbBqLX
FLAMMABILITY OF PLASTICS AND FLAME TEST METHODS
A. W. Morgan and C. P. Farley Monsanto Company St. Louis, Missouri
INTRODUCTION
Use of a single test method in rating flammability of plastics may lead to confusing results when variations in test geometry are ignored. The use of a multiple test method with wide variation in test geometry great ly reduces this problem and allows a better understand ing of flammability parameters inherent in plastics systems.
The nature of a relatively simple fire such as a match burning can be observed and studied carefully without various observers agreeing fully on the mechanism of burning. If this simple illustration is extended to a more complex fire, such as a sofa or chair burning, we see many other factors coming into play. As the ex ample is carried even further, to a house or nursing home fire, the act of burning of the individual items is a most complex and baffling phenomena.
To attempt to predict the burning characteristics of pl astics or wood or metal by a single test which would be a valid prediction under various condition of burn ing seems unrealistic. The main advantage is a time saving in testing.
With increased awareness of safety in consumer products resulting from both legislation and publicity, high interest has evolved in the flammability characteris tics of plastic materials used in such conventional home products as furniture, mattresses, carpeting, wall covering and appliance housings. In rating flammability of such materials the investigator must choose from a great number of tests recommended by many organizations. These include technical associ ations, such as ASTM, SPI, SAE; state, local and fed eral governmental agencies? independent laboratories of Underwriters Laboratories, insurance groups, build ing code groups and many industrial corporations. Of ten, however, these tests are designed to measure one particular parameter of flame testing such as ease of ignition, surface flame spread, fuel contribution, or fire endurance. Quite often, the bench scale test may have little resemblance to the logical fire conditions to be expected in the end-use application.
Consequently, flammability test methods for plastics are often misleading in their results. Ideally, a given test should allow the formulator to rank his product as being satisfactory or unsatisfactory ac cording to the degree of flame retardance required in a given application. A single test, however, can rarely satisfactorily rate materials which are rou tinely used in a variety of complex shapes or in com posites with many other materials.
As an example one may consider the wide variation in flame testing geometry inherent in a chair. It is readily seen that the flame may propagate on a number of surfaces at angles to 0 to 360. Propagation up the back would be 90, along the top of the arm 0, under the arm 180, or down the back 270. All other angles of burn as well as many combinations are possi ble. Figure 1 illustrates these flame progation an gles. Additionally, in such an article the flame may propagate on the exposed outer surface or, if igni tion occurs under a cushion or on the c^air bottom, propagation may occur as internal or backside burning. It is evident that the ignition source and point of ignition may greatly influence the behavior of the
58 ' ..........
\
DSW 587783
STLCOPCB4093119
Finally# the proximity .and use of other materials may greatly affect propagation. A piece of non-flame re tarded plastic sheeting will burn readily if unsup ported and ignited at 90 with a'match. If laminated to a rigid substrate with reasonable resistance to ignition the same film will have reduced propagation and may not ignite under identical conditions.
It is evident that a single test cannot pncompass all parameters possible for combustion in a complex arti cle. It is also evident that testing of every para meter would be a costly and laborious process. In actual practice a combination of three or four test methods will generally give a good estimation of the relative flame retardance of a given system1. If one
is formulating to meet a specific test, of course, these additional test results are valuable as formu lation aids to measure incremental changes.
A variety of test methods exist which consider var iations in burning conditions.lf^^ Figure 2
demonstrates several tests which vary sample geometry. From this it is seen that one can measure the flamma bility of a sample under a variety of conditions. In general, the most severe condition is that in which the sample is ignited in a vertical configuration (90) If the sample is mounted in a ceiling position (180d) as in ASTM E-84, equal severity is often obtained. Samples in which the flame propagates away from the surface or propagates downward are less severe pro viding burning conditions are equivalent.
A convenient method of measuring flame spread has been found to be the Monsanto two foot tunnel . In this test the sample forms the roof of a tunnel and is in clined 28 from the horizontal (Figure 3). The spread over a four minute period is measured and a flame rating is determined based on an assigned value of zero for asbestos and one hundred for red oak. In this test the method of mounting the sample is partic ularly important. A free film of plasticized poly vinyl chloride (PVC) supported by chicken wire will burn much more rapidly than will the same film mounted to a rigid substrate with good thermal conductivity.
\ The Fenimore-Kartin oxygen index test ' is an example
! of a downward burning test. In this test the oxygen ; * *' content of the atmosphere is raised until the minimum
. oxygen concentration for combustion to occur is reach| ed. The oxygen index method has been found to be pre-
j ' cise, reproducible, and a highly valuable formulation
fc guide. It is important to note, however, that results
from this test frequently do not correlate with flame | spread results obtained when the bottom of the sample
; is ignited and the flame propagates upward.
Other tests of interest for screening include the methenemine pill test and the proposed Department of Transportation horizontal bum test9. In the pill
test the pill is ignited on a horizontal surface and allowed to burn. While this test is quite mild on most flat surfaces, it can be of great value when ap plied to irregular areas as in the right angle formed by a seat cushion and a chair back. The effect is very similar to that caused by a dropped match or cigarette. The DOT test is a method which measures the burning rate of materials in a horizontal config uration. While a useful tool, this test has little correlation to results obtained when the same material is burned in a vertical configuration.
By selecting from these tests, as well as by spot tests
such as simply lighting the materials with a match or
bunsen burner, it is generally possible to formulate
satisfactory flame retardant compositions with a min
imum of risk. It also becomes easier to measure in
cremental changes which might be missed if only one
test is used.
.
In our laboratories, oxygen index, Monsanto two foot tunnel, DOT horizontal burn, and a vertical test (ASTM D-56810), are routinely used to screen formula
tions. Other tests to meet given specifications or accommodate different materials, or shapes are added as necessary.* -
To illustrate the usefulness of multiple tests in formulating, consider an experiment involving flame retarding plasticized PVC of the type normally used in furniture covering. In the experiment incremental
69
DSW 587784
STLCOPCB4093120
additions of a flame retardant plasticizer were made to a standard formulation. Oxygen index, DOT hori zontal burn, Monsanto two foot tunnel, and vertical burn data were obtained. Samples were milled five minutes at 350F (176C) and^ were calendered into ten mil (0.025 cm) films for testing. The formulations and results are described in Table 1.
Several points are immediately evident. The increase in oxygen index is nearly linear as the concentration of flame retardant phosphate increases. It is also readily seen that the horizontal burning configuration is much less severe than the vertical configuration. In the horizontal test the control burns readily but at a measurable rate (12.5 in./min.). Jn the vertical
TABLE I
'
Flame Test Data on 10 mil Unsupported Polyvinylchloride Film
12
3
PVC Homopolymer (Opalon 650)
Di(2-ethylhfcxyl) Phthalate
Cresyl Diphenyl Phosphate (Santicizer"l40)
Ba/Cd Stabilizer
`
Epoxidized Soya Oil
Calcium Carbonate
100 70 1 3 12
100 63 7 1 3 12
100 56 14 1 3 12
Methenemine Pill (Applied to 90 bend)
Ignites
Ignites
Burns Slowly
Oxygen Index Flame Spread (Monsanto Two Foot Tunnel)
Film Supported on Wire Film Laminated to Transite
21.6
135 54
22.4
72 34
23.6
64 - 26
DOT Horizontal Burn Distance Burned (in.) Time of Burn (sec.)
10 1.5 48 27
0* 0
Vertical Burn (5 sec. burner ignition
of a 1 x 12 inch sample)
Distance Burned (inc.)
.
Time of Burn (sec.)
12 3.6
12 6.9
% 6.4*
iL 6
4
100 49 21 1 3 12
Does Not Ignite 24.1
48 17
5
100 42 28 1
"3 12
Does Not Ignite 25.1
29 10
0* 'V * 00
3.2* 5
1* 2
* Self-extinguishing results
Opalon and Santicizer are Trade Marks of Monsanto Company
TABLE II
Relative Flame Hazards Presented by Films from Table I In Practical Furniture End-Use
Formulation One
(0% Flame Retardant)
Two (10% Santicizer 140)
Three (20% Santicizer 140)
Four (30% Santicizer 140)
Five (40% Santicizer 140)
Probable Result
Relative Flame Hazard
Ignites readily, burns violently up back, fire spreads readily across arms and cushions.
Very High
Ignites readily, burns readily up back, slower propagation than Formulation One.
High
Ignites slowly, propagation up back is slow and may self-extinguish. Little spread across arms or back.
Moderate
Does not ignite. scorchs.
Probably only
Low
Does not ignite.
Low
Santicizer*3 140 plasticizer is cresyl diphenyl phosphate.
DSW 587785
STLCOPCB4093121
t
test the rate is so rapid (200 in./min.) as to be nearly explosive. The problem previously discussed of geometry in flame testing is well illustrated by these results.
It is also evident by the tunnel test results that
mounting a sample on a rigid substrate effectively
lowers the flame hazard particularly if the substrate
is high in thermal conductivity with good resistance
to ignition. Metal, asbestos board, and wood panels
have been effective for this purpose. In many cases,
however, the improvement is also seen with rigid
plastics which prevent the sample from sagging and
hence falling into the much more severe vertical con
figuration.
.
From the results it is seen that there is little correlation between tests. A relative correlation does exist between the Monsanto two foot tunnel and the oxygen index test in this experiment as incre mental additions gave generally linear results in each case. The only reasonable correlation which can be made, however, is that the flammability of the sample decreases with increasing amounts of flame retardant plasticizer.
This approach is valuable as a guide to formulating
for a given application. If a specification is to be
met one simply picks the geometry and result closest
to that required by the specified test and adjusts
the formulation as needed. The data obtained by the
other tests guard against a false result. Although
this example is based on PVC the same general consider
ations in testing have been found to be valid in other
resins, such as polyurethane, polystyrene, polyolefins,
etc.
`
Several factors, particularly the flammability of the substrate,, can affect the results and for real con- ' fidence a full scale test should be run. It is pro bable, however, that the results will be within the "ball-park." The formulator can then work for the best cost-performance system. In the case in point, as the flammability of the vinyl system would be generally reduced by the normal practice of laminating the vinyl film on cloth, a "safe" formulation might require between fifteen and twenty-five per cent of the flame retardant plasticizer.
An additional advantage of the use of multiple tests is that it allows better comparisons of flame re tardant systems between different laboratories. Po tentially costly anomalous results seldom escape the cross checks of-multiple testing. As an example, al though the performance of isodecyldiphenyl phosphate (Monsanto's Santicizer 148) and trioctyl phosphate
in a PVC system may appear almost identical in oxygen index and horizontal burn tests (Tabic III), in verti cal burn and tunnel tests, the flame retardance of isodecyl diphenyl phosphate is far superior to that of trioctyl phosphate. Thus, by routinely using multiple tests, product advantages may be easily found.
SUMMARY AND CONCLUSIONS
It has been shown that reliance on a single flame test method may give erroneous or misleading results. The use of several tests utilizing different geometry will generally reduce these potential errors, and may generate bonuses in the comparison of results or in formulating for other applications.
If no specific requirements must be met the results serve as guides for determining how the material will behave in the application. If the vinyl formulations tested were used to cover the chair previously dis cussed and if ignition occurs at the junction of the back and cushion with a careless match the performance of each formulation may be predicted (Table II).
TABLE III
PVC Homopolymer (Opalon 650) Di (2-ethylhexyl) Phthalate Trioctyl Phosphate Isodecyl Diphenyl Phosphate* Calcium Carbonate Ba/Cd Stabilizer Epoxidized Soya Oil
Oxygen Index
DOT Horizontal Burn Inches Burned Seconds
Monsanto Two Foot Tunnel Free Film, Flame Spread
Vertical Burn Inches Burned Seconds
1
100 42 28 -- 12 1 3
23.3
3.6 48
97
12 17
2 100
42
28
12
1 3
23.3
3.4 50
54
4.5 3.2
* Santicizer 148
Opalon and Santicizer are Trade Marks of Monsanto Company.
'61 -
.
DSW 587786
STLCOPCB4093122
REFERENCES
Hilado, C. J., Flammability Handbook for Plastics, Technomic, Stamford, Conn., 1969, pp 60-61. (2) "Fire Test Methods" ASTM S.T.P. No. 344 (1962).
(3) "fire Test Methods" ASTM S.T.P. No. 422 (1967).
Vandersall, H. L. , J. Paint Technology _39 No. 511 pp 494-500, (August, 1967).
(5) Fenimore, C. P. and Martin, F. J., Modern Plastics 44, No. 3, 141 (November 1966).
(6) Goldblum, K. B., SPE Journal 2ji, 50-52 (February, 1969).
(7) Am. Soc. Testing Materials, ASTM Std. 14, pp 358 365 (November, 1967).
Federal Specification FS DDD C-95.
'
(9) Department of Transportation, Docket 3-3, Federal Register, Vol. 34, No. 249, December 31, 1969.
(10)
Soc. Testing Materials, ASTM Std. 27, 160-162
(June, 1967).
f 62
l" .
DSW 587787
fc- -
L
STLCOPCB4093123