Document KGOw6YLkEyMMogzOVdQbRg156

United States Patent [i9j Sheer [ii] 4,317,764 [45] Mar. 2,1982 [54] POLYBUTYLENE TEREPHTHALATE MOLDING BLENDS [75] Inventor: M. Lana Sheer, Chadds Ford, Pa. [73] Assignee: E. I. Du Pont de Nemours and Company, Wilmington, Del. [21] Appl. No.: 252,884 [22] Filed: Apr. 10, 1981 [51] Int. Cl.3 ............................................ C03L 67/00 [52] U.S. Cl................................ 524/449; 264/331.13; 525/63; 525/66; 525/69; 525/166; 525/173; 525/174; 524/513 [58] Field of Search ................ 260/40 R; 525/63, 66, 525/69, 166, 173, 174; 264/299, 331.13 [56] References Cited U.S. PATENT DOCUMENTS 3,579,609 5/1971 Sevenich ............................... 525/166 4,172,859 10/1979 Epstein.................................. 428/402 FOREIGN PATENT DOCUMENTS 1208585 10/1970 United Kingdom ............. 260/40 R Primary Examiner--J. Ziegler [57] ABSTRACT A polybutylene terephthalate homopolymer or copoly mer molding blend having good impact resistance is obtained by incorporating into the resin a selected or ganic compound and an ethylene polymer. 12 Claims, No Drawings 4,317,764 12 and combinations of them. These materials, if present, POLYBUTYLENE TEREPHTHALATE MOLDING are preferably present in an amount between 15 and 50 BLENDS percent by weight of blend. Representative polyalkylene oxides are polyether FIELD OF THE INVENTION 5 glycols having terminal hydroxyl groups. Du Pont This invention relates to polybutylene terephthalate molding materials, and more specifically to such materi "Teracol" materials are examples of this family. The preferred molecular weight range is 600-3000. als that may be molded to obtain shaped articles of Polyhexamethylene adipamide oligomers include improved impact strength. polyhexamethylene adipamide copolymer oligomers. 10 For example, an adipamide oligomer of 66/69/610 ny BACKGROUND OF THE INVENTION lons having ~380 amine ends/10 g, ~40acid ends/10 g It is desirable to enhance the strength of articles and a melting point of approximately 180 C. or a hexa- molded from thermoplastic resins, such as polybutylene methylene adipamide oligomer having ~470 amine terephthalate. Usually a reinforcing material such as ends/10 g, --9 acid ends/10 g and a molecular weight glass fiber, asbestos fiber or other fibrous material may 15 of approximately 4200 can be used in this capacity. be employed in the resin to increase strength. In addi Preferably the organic compound is present in an tion, fillers such as glass beads, platelets, or particulate amount of 0.3-5% by weight of blend. minerals may be used to aid in increasing modulus. Representative ethylene polymers having carboxyl or Even though reinforcing and filling materials en ester fucntionality and a modulus less than 50,000, in hance the strength of articles molded from the resin, it 20 clude adducts of ethylene and ethylenically unsaturated is desirable to obtain even stronger articles, and particu compounds containing carboxyl or carboxyl deriva larly desirable to obtain articles having good resistance tives. A preferred ethylene polymer for adduct forma to breakage on sudden impact. tion is a copolymer of ethylene, at least one C3 to C6 SUMMARY OF THE INVENTION a-olefin, and at least one nonconjugated diene. The 25 adduct may be prepared as described in Flexman U.S. A polybutylene terephthalate homopolymer or co Pat. No. 4,026,067 or Caywood U.S. Pat. No. 3,884,882 polymer molding blend having good impact resistance and U.S. Pat. No. 4,010,223. Propylene is normally is obtained by incorporating into the resin an organic compound selected from polyalkylene oxides and adipamide oligomers; and an ethylene polymer having ester or acid functionality and a modulus less than 50000 psi. It has been found that the organic compound and the ethylene polymer act synergistically to improve impact 30 selected as the C3-C6 a-olefin in preparing such poly mers. Other C3-C6 a-olefins, namely 1-butene, 1-pentene, and 1-hexene can be selected in place of or in addition to propylene in preparing the elastomeric poly mers. Preferably the nonconjugated diene is monoreac resistance of the blend over that of a similar blend that tive. Monoreactive nonconjugated dienes have one does not contain the two additives. The polybutylene terephthalate blends of this inven 35 double bond which readily enters the polymerization reaction with ethylene and propylene, and a second tion may be described as a blend of double bond which does not, to any appreciable extent, (a) 20-95% by weight of blend of polybutylene tere enter the polymerization reaction. The nonconjugated phthalate having an inherent viscosity of at least diene imparts side chain unsaturation, which unsatura about 0.5, or a copolymer of polybutylene tere 40 tion is available for adduct formation. Monoreactive phthalate and less than 50% by weight of a como nonconjugated dienes include linear alipahtic dienes of nomer polymerizable therewith; at least six carbon atoms which have one terminal dou (b) 0.1-10% by weight of blend of an organic com ble bond and one internal double bond, and cyclic di pound having a molecular weight less than 16000 enes wherein one or both of the carbon-to-carbon dou which is selected from the class consisting of a 45 ble bonds are part of a carbocyclic ring. Of these dienes, polyalkylene oxide and a polyhexamethylene adip- 1,4-hexadiene is preferred. amide oligomer; and A class of preferred ethylene polymers include ad (c) 5-35% by weight of blend of an ethylene polymer ducts of tetrapolymers made from ethylene, at least one containing ester or acid functionality and having a C3 to Ct, a-monoolefin, at least one monoreactive non modulus less than 50,000 psi. 50 conjugated diene, and at least one direactive nonconju The resin blend may also contain up to 60% by gated diene such as 2,5-norbornadiene or 1,7-octadiene. weight of blend of reinforcing or filling material. DESCRIPTION OF THE INVENTION A preferred polymer of this class is a tetrapolymer of ethylene, propylene, 1,4-hexadiene, and 2,5-norbornadi ene. The polybutylene terephthalate employed herein is 55 , The ethylenically unsaturated compound containing one which has an inherent viscosity of at least 0.5 as carboxyl groups or carboxyl derivatives that are used in measured by ASTM D-2857. The polybutylene tere adduct formation are preferably a,/3-ethylenically un phthalate preferably has an upper limit on inherent saturated carboxylic acids having from 3 to 8 carbon viscosity of about 1.1. Inherent viscosity is measured in atoms, and esters of anhydrides thereof. Illustrative of a 3:1 by volume ratio of methylene chloride and trifluo- 60 such compounds are maleic acid, maleic anhydride, roacetic acid at 30 C. The polybutylene terephthalate maleic acid monoethyl ester, fumaric acid, fumaric acid can contain less than 50% by weight of other comono monoethyl ester, itaconic acid, vinyl benzoic acid, vinyl mers such as diethylene glycol, glutaric acid, polyethyl phthalic acid. These compounds provide pendant car ene terephthalate or polyalkyene oxide, cyclohexane boxyl or anhydride groups to the polymer. dimethanol, and other diols. 65 It is generally desired to form adducts containing The reinforcing or filler materials employed herein about 0.5 to 9 percent, and preferably about 1 to 5 per include glass fibers, graphite fibers, aramid fibers, glass cent, by weight of compound that contains carboxyl beads, aluminum silicate, asbestos, mica, and the like, groups. 4,317,764 34 Other representative ethylene polymers of include ethylene/vinyl acetate/glycidyl methacrylate; EXPERIMENTS 1^4 ethylene/methyl acrylate/glycidyl methacrylate; and Experiments 1 and 2 demonstrate the use of polytet- emulsion-type modifiers of methyl methacrylate/- ramethylene oxide or a polyamide oligomer with an butadiene/styrene or methyl methacrylate/acryloni- 5 ethylene polymer. These blends do not contain glass- trile/butadiene/styrene. reinforcing fibers. They illustrate that the addition of an Preferably 15-30% by weight based on blend of the organic compound as described herein with the ethyl adduct will be employed on the blends of this invention. ene polymer produced ductile rather than brittle It is believed that the organic compound reacts with notched Izod breaks in molded specimens. The compa the ethylene polymer at one functional site and with the 10 rable 30% glass-reinforced blends are also demon polybutylene terephthalate at another site. strated in Experiments 3 and 4. In addition to the components discussed hereinabove, the compositions of this invention may contain addi The blends of Experiments 1-4 are shown in Tables 1 and 2 along with the respective properties. tives commonly employed with polyester resins, such as colorants, mold release agents, flame retardants, antioxi 15 Sample dants, ultraviolet light or heat stabilizers and the like. (% by weight) The compositions of this invention are prepared by intimately blending the components together by any % PTMO1 % Polyamide convenient means to obtain an intimate blend. Neither temperature nor pressure are critical. For example, the 20 oligomer2 % Ethylene TABLE 1 Experiment AB 1 00 1.05 00 0 2 0 2.0 polybutylene terephthalate can be mixed dry in any suitable blender or tumbler with the other components Polymer3 % PBT (IV 0.83) Notched Izod 0 100 20 28 80 -- 71 20 78 and the mixture melt-extruded. The extrudate can be (ft-lb/in) 1.04 3.14 20.45 15.9s chopped. If desired, a reinforcing or filling agent can be added after the first melt extrusion, and the resulting 25 'Polytetramethylene oxide with MW =,1000. 2Ny!on oligomer of a 66/69/610 copolymer having --380 amine ends/106 g. and mixture can then be melt-extruded. -40 acid ends/IO`g,, MP -ISO- C. 3A polymer of fumaric acid grafted onto a polymer ofethylene, propylene, 1,4-hex- EXPERIMENTS adiene and norbomadiene was employed. The graft polymer had an anhydride functionality of 0.42 meg/g acid. ^Brittle break. In the Experiments which follow, percents are based on total blend unless otherwise noted. The polybutylene 30 ^Ductile break. terephthalate blends used in the Experiments were pre pared as follows: All ingredients except the glass were dry blended and Samples then extruded through a 28 mm twin-screw extruder at a melt temperature of approximately 260-270 C. The polybutylene terephthalate (PBT) was dried prior to 35 (% by weight) % PTMO1 % Polyamide oligomer2 blending. It had an inherent viscosity of 0.83. The ex % Ethylene TABLE 2 ________________Experiment cD 3 00 1 000 truded strands were chopped into pellets and dried at Polymer3 about 110 C. for 16 hours in a vacuum oven. The dried 40 % Fiber Glass3 % PBT3 pellets were blended with the desired amount of OCF Elong (%) 419AA glass fiber (chopped to 3/16") where used and Unnotched Impact 0 20 20 30 30 30 70 50 49 2.6 1.5 5.1 extruded through a two-stage single screw extruder at a (ft-lb/in) 15.7 melt temperature of about 240-260 C. The extruded Notched Izod (ft-lb/in) 2.0 strands were cooled, chopped into pellets and dried at about 110 C. for 16 hours in a vacuum oven. The pel 45 *Samc as used in Experiment 1. 2Same as used in Experiment 2. 9.4 21.7 2.6 6.0 lets were molded into test bars in a 6 oz injection mold 3Same as used in Experiment 1. 4 0 2 20 30 48 4.5 16.0 3.4 ing machine with a melt temperature of about 250 C., fast ram, 10 seconds injection forward time, 20 seconds mold close time, and a cavity temperature of about 90 50 C. The bars were 5"x''X8" for notched Izod and EXPERIMENT 5 This experiment demonstrates the applicability of one unnotched impact tests and thick ASTM D-638- of the toughening systems of this invention in a flame- Type I bars for tensile and elongation measurements. retardant, 30% glass reinforced PET blend. This blend Properties of the test bars were measured according is identical to Example 1, except it contains 4.6% (wt) to the following procedures: 55 antimony oxide and 13% (wt) decabromodiphenyl Tensile strength and elongation were measured on ether (common flame retardant additives). injection molded bars by ASTM Method D638. Blend information and properties are given in Table Notched Izod impact strength was measured on the 3. injection molded bars by ASTM Method D256. Unnotched impact strength was measured by cutting 60 5X2Xg"0 injection molded bars to the size specified for the Izod test in ASTM Method D256, but without notching the bars, and otherside running the test by Izod method ASTM Method D256. The three properties--elongation, notched Izod im 65 pact and unnotched impact strength--give a measure of the toughness or impact resistance of a material in end- use applications. TABLE 3 Sample (% by weight) A % PTMO1 % Ethylene Polymer2 Elong - (%) Unnotched Impact (ft-lb/in) Notched Izod (ft-lb/in) UL 94 Test Rating3 0 0 2.3 14.9 2.2 Experiment 5 1 20 4.0 17.6 6.1 4,317,764 56 TABLE 3-continued 2. The blend of claim 1 wherein the blend contains up to 60% by weight of blend of a reinforcing agent or Sample Experiment filler. (% by weight) at J" and 1/16" thicknesses A V-O 5 3. The blend of claims 1 or 2 wherein Component (b) 5 is a polytetramethylene oxide. V-0 4. The blend of claims 1 or 2 wherein Component (c) 'Same as used in Experiment 1. is an adduct of maleic anhydride and a copolymer of 2Same as used in Experiment 1. ethylene, propylene, and at least one linear aliphatic 3Not UL certified. diene of at least 6 carbon atoms. 10 5. The blend of claim 4 wherein the diene is 1,4-hex- I claim: adiene. 1. A polybutylene terephthalate molding blend con 6. The blend of claim 2 wherein the reinforcing agent sisting essentially of is glass fiber. 7. The blend of claim 2 wherein the reinforcing agent (a) 20-95% by weight of blend of polybutylene tere 15 is glass fiber and mica. phthalate having an inherent viscosity of at least 8. The blend of claim 2 wherein the reinforcing agent about 0.5, or a copolymer of polybutylene tere is mica. phthalate and less than 50% by weight of a como 9. The blend of claim 1 which contains, additionally, nomer polymerizable therewith; a flame retardant. 20 10. The blend of claim 3 which contains, additionally, (b) 0.1-10% by weight of blend of an organic com a flame retardant. pound having a molecular weight less than 16000 11. Process for preparing the blend of claim 1 which which is selected from the class consisting of a comprises mixing the components of the blend and then polyalkylene oxide and a polyhexamethylene adip- melt-extruding the mixture. amide oligomer; and 25 12. Process for preparing a molded article which comprises melting a blend of claim 1, placing the melted (c) 5-35% by weight of blend of an ethylene polymer blend into a mold, and then allowing the blend to solid containing ester or acid functionality and having a modulus less than 50,000 psi. ify. ***** 30 3'5 40 45 50 55 60 65