Document K6xZOg7Jr5E57OQL5xM0gXQer
Heat Treatment of Chrysotile Asbestos Fibres
" i a By M. S. BADOLLET' and W.C. STREIB* . v.-
(Annual General Meeting, Toronto, 1953) (Traneactions, Volume LVIII, 1955, pp. 33-37)
ABSTRACT
harsh types they are as low as
A commercial method has been de veloped for controlling the texture of chrysotile asbestos fibres so that they may possess properties compar able with natural semi-harsh fibres for use in wet processes.
The physical properties of the soft, silky and slimy fibres are partially altered by a flash-heating process which removes a portion of the mole cular water.
The heat-treated fibres show an improvement in filterability, an in crease in bulk, absorption, and sur face area, and better electrical prop erties, such as volume resistivity.
llM'/g. The reason for these differences
in fibre textnre has been a matter of conjectnre for some time, and the literature (2) contains several suggested explanations, snch as the MgO : SiO, ratio, lime content, presence of calcite, pressure of formation, weathering, transition be tween asbestos and talc, and mole cular water content of the fibre. After examining fibres of widely differing textnres, it was found that the best correlation seems to exist
between the water of constitution
and the degree of harshness. The
Introduction
paramount differences between harsh- and soft-textured fibres, how
CHRYSOTILE ASBESTOS fi ever, are in their . respective bres are found in nature having strengths and filtration characteris varying degrees of texture, referredtics Furthermore, it is the wide dif
to as soft, semi-barsh, and harsh. ference in these properties which
Fibres of each type of texture have directly influences their industrial
inherent characteristics which di usages. For example, 5 soft, silky
rectly affect their usefulness to in fibre usually" has high tensile-
dustry. Visual differences are ap strength and is extremely flexible.
parent under a microscope where it However, it is also usually slimy
is seen that the soft-textured fibres and difficult to de-water when used
have a silky, serpentine or wavy ap commercially to produce products
pearance, whereas the harsh-tex- involving wet methods. On the other
tured fibres are coarser and spicn- hand, harsh and semi-harsh - fibres
lart. .Semi-barsh fibres, of course, de-water rapidly, but are generally
have properties intermediate be low in tensile strength, and, in many
tween these extremes.
cases,, brittle to- the point that the
Fankuehen and Schneider (l) hare shown by the vmp-yd low-angle
X-ray scattering Uurigttar diameter of the harsh typradjre!e^fysotile fibre is somewhat gjrSflfctribnn that of the soft variety. **3i!Wltce area measurements on retinae chrysotile# of different textures tend to con firm their findings. By nitrogen adsorption methods, it was fonnd that the surface areas of soft types of chrysotile asbestos are approxi mately 23M3/g whereas for the
flexing characteristics are vastly in ferior to those of the soft chrysotilea. - Obviously, it would be desirable to produce a- fibre incorporating the strength properties of the soft-tex tured fibres with the rapid filtering
properties of die harsher types. The commercial or industrial importance of such a fibre, would be an increase in the production rate of- wet-ma
chine products and possibly the util isation of lower grades of poorer filtering fibres were high product
strength might not be of the utmost
`Research Center, Johns-Mansville Products Corporation, Manville, N.J.,
U.S.A.
(Photomicrographs showing these differences were published in C.I.M.
Transactions, Vol. LIV, 1951, p, 1`66.
(1) For references see end of pa per.
importance. Since the water content
of chrysotile appears to be corre lated with its texture,- it was de cided to examine heat-treatment as a means of modifying the textnre of the soft fibres and itnproivng their physical properties.
Effect of Heat on Texture
or Fibre
Samples of chrysotile crudes, carefully cleaned of wall-rock and fibreized, were prepared and classed as soft, silky, and slimy when wet by .water. Careful heating of these samples in the laboratory under controlled conditions at various tem peratures and for various durations of exposure definitely indicated that a soft fibre can be converted to one exhibiting the. characteristics of a harsh or semi-barsh fibre.
Dehydration studies of chrysotile asbestos have been made by numer ous investigators (3) and the ef fects of temperature are well known. However, the purpose in the pres ent application was to dehydrate the chrysotile molecule only partially and to bring the water content in the range normally encountered in the harab-textured fibres.
The "loss on ignition" shown in analyses of semi-harsh to harsh chrysotile fibres usually ranges from less than 12 per cent to 13 per cent, depending upon the degree of harsh ness. The theoretical percentage of molecular water or water of consti tution in pare asbestos is approxi mately 13 per cent. This is repre sented by the hydroxyl radical in the molecular structure is expressed by the formula Mga(OH)gSi,Olo, where the heat first breaks down the components to 8Mg,SiO,, SiO,, and 4H,0. Therefore, any reduc tion in the number of hydroxy rad icals present, as would be effected by heat, will decrease the total amount of water of constitution, and this affects the physical properties of the fibre.
For the applications under con sideration, the water of constitution was to be reduced about 30 per cent, or, in other words, the fibre sample was to be heated until its loss in weight amounted to about 4 per cent- In most of the tests, however, this loss actually ranged from 0.3 per cent to 3 per cent. Excessive heating has a deleterious effect upon
-- 33 --
UCC 004655
ae&h* 0$filkt.
"'r- -v^ >4 ^ */ * J '
Temferatt^oc
Increase Tim* IN FlLTER-
Min. ' .: ABtiirr
ItBSHKMi `Mmkbt-
Asbestos-Cement
. Panel* '
RtsrouAf.
aid <m.
^^ ^^^^^^^^^ ^ ^ ^^
from regular pt&KB&ifr which
they, too,, were 'iii>^jy,||v;.to heat
treatment at various temperature*
for varying time intervals. Again,
the fibres produced possessed tex
ture characteristics similar to those
of semi-harsh and harsh fibres. In
- ;
__ J.
60(h...:....... 15
600.
30
906.----------....
7-
906. '..
.:"... 15-
1^00........ 1
1^00,. ... .... 2
1,200...............
3
S:i-
*
7SF ' . 98.4,"' '
250- :
98.7-
25.0
-5'; 97.1-, -
79.0/::
98^:
25.0. * 994'-
67.0
. 94.9'
7L6 -
93A'
902
(SLSJ-.
8SJ' 78.7
sww;TM-
Vy7lap' "
.2,766"
82.6
the fibres from regular production,
there are impurities such as brncite,
. carbonates, and others. Heating will result in ignition losses higher than the theoretical 13 per cent of water
gree of filterability as that obtained, mode with fibres heated at 1,200
by heating, at a lower temperature, Vi tal % minute? still Retained 82.6: .'
for a longer period.
'C - percent of their, normal strength,'
of constitution of pure asbestos.
Another interesting comparison, ih' \ .' Another advantage of beat-treat-' .v, that of the percentage of residual .' men! of chrysolite is its effect upon'
Physical Properties op Heat-
Treated 0D Fibre
/
Table I lists some of the physical
properties of the 6D fibres before
and after the heat treatment. The
water with the percentage, of &-:> tho vpfume resistivity , of the fibre. '
crease in filterability. As saowibi itti.:
illustrates the' vast iiH .
Figure 3, there is a definite W*\ crease in the. resistivity of a heat- -
relation, and the amount* ofwatey treated CanadOui SD fibre which is -
in the molecule governs th$. degree'*. used in the manofaetora of asbestos
of filterability of the fibre," . . '
-
data show that as the heat-treat
tim effect of heat nps <& '"":
ifcnt,aa tkr -
ment temperatures and times ore. increased, filtration is improved, water of constitution is reduced, magnetite is decreased,- and thestrength of an asbestos-cement block
containing the heat-treated fibre is decreased.
netlte present in chrysdtile-: from?, ntofceula*: Satot-vivax reduced, tfts > i
regular production is to PSatTertST: vo&igut r tesialirif* expressed jo - '
partially, the |A * git^r;,~Xr
greatly
?"
is non-magnetfe? In Table I, (BA re?* efehaodC; VigfVfcZil* ifitwtratej t& :.
duetion in the amount of magpedter>
gy ypWfr-Sf the percent-'
remaUing-in the fibre; after; fttatiiig, siifeSbJ *esidbaiJTi*irtet against thd *'"*
mwr,a-.w*
and 1,200 ^^rtegi^bi^S:>:roi^shiavitK, :
Figure I, in which percentage i&- that tb^.tnalnethr'.'chstactee' -df-.-thd;/'Tte area-between? theae-curves repy^
crease in filterability is plotted
against temperature, shows the ef by-hert t^atftknte
' *>$
fect of the heating at time inter vals of fifteen minutes and three minutes.
.Table bant treatment Upon aabeatos-eemen^ face. However, eye. wften tie fly' ift* paneb made of a Canadian 8l>fJb*iBu'. breR./were tested',at .74,? and 4*''. w
Figure 2, showing the percentage
thcTahfc, the strengths' of' these'J
the hai-l.
increase in fibre filter-ability at dif panels are expressed a* modufea ofi^ pruventeht'ig.. electrical pro^sjetef^'
ferent heating-time intervals at tem mpture in pbpnds per square;DscK '' waohigbfy si|--a -- -'i-tu
peratures of 700F. and
demonstrates that heating at o- big??: frhri'temparatura of
ftnp'-lj~th sstegf'
temperature for a short pearitoed*?3**?
yield a fibre having t& same?
hnr^i^^st*ingtf|i'}.ffUillf
ifitWiifr
,
Jwti; - -1^
s' i
/
'
:v'
. NtN '
/
_ _ _ _ _ _ U.
/-
O 200 400 400 600 BOC COO MOO two
TtWfgRATUM V
Figure 1.--Percent increoee in filterability rs. temperature (F.)
Figure 2s^-P<fctni. increeae in ffltrmbillty rr. time of
(mm*)
X. / 7.' . "ri V- * ' . ,-*i -
' 'sl&r# ' ~ V " ''
Boss*aMioao
Figure J.--Percent residual HiO v. percent increase in f ilierability.
1 OOOCoO
Z) 3| > i oo f1 100 S -o
i' t 0.
001
to
9 MV s4u4mXs8ksb''
m n n to
| an rm
4
w is
m
Figurt 4,--Effect of heat treatment upon volume resistivity of 6D rhrysodfe asbestos.
properties is of direct interest and importance in the manufacture of electrical papers.
X-ray diffraction studies were made on a Canadian chrysotile fibre heated for one hour at temperatures of tOO0. 500, 600, 700, 800, and 900 F. They showed that the structure remained typical of chrysotile. At 1,000 F. for one hour, the surface was amorphous, but. after carefully scraping off the surface, examination of the interior revealed the X-ray diffraction pat terns were mostly those of chryso tile. At l,tOO"F. for one hour, the entire mass had the structure of olivine. This study indicated that chrysotile, after losing small amounts of its molecular water, still retains much of its general struc ture. Anderson and Clark (5) heat ed chrysotile to constant weight at 900 C. and showed that the result ing fibre structure was not so defi nite as in natural fibre.
Application of Heat
Various types of,, heating units were investigated, Mek as muffle, infrared, dielectric, different types of commercial furnaces, and flash calcining. The main problem was to obtain a uniformly heated asbestos particle throughout any given mass, whether suspended in a gas atmos phere or as a thin or thick layer on a conveyor belt. Another problem was to devise a temperature control system that could be regulated man ually or made automatic. A final problem was cooling of the treated fibre before it was bagged.
Several years were required to in vestigate all of the possible methods of applying heat to produce heat-
Table II.--Effect of Heat Treatment on Resistivity of Fiber
Residual Water
%
100 97.3 97.0 94.5 93.3 76.7 89.4 68.2
Residual Water. Log
2000 1.988 1.987 1.975 1.970 1885 1.951 1.834
Volume R ESJST1VITY 74T'\, 44RH
Megohm inches
Log resistivity
0.016 0.023'
0.026 0.075
0.110 13.30
0.25
45.30
-1.796 -1.638
-1.585 -1.1249
-0.9586 +1.1239 -0.6021
1.656
Volume Resistivity Bone Dry
Megohm inches
Log resistivity
0.08 0.29 0.29 4.10 4.80 52,000 41.0
300,000
--1.097 '
-0.538 -0.538 +0.613
0.681 4.716 1.613 5.477
treated fibre. Finally, the flash-cal cining system was selected as the most appropriate.
Heat-Theatmbnt Pilot Plant
A flash-calcining unit was pur chased from the Nichols Engineer ing and Research Corporation, and a pilot plant with a processing ca pacity of two tons of fibre per hour was erected at Asbestos, Que.
A diagram of the unit is presented in Figure S, which shows the path of asbestos particles and gases throughout the system. Thermocou ples were installed at strategic points, and the temperatures were recorded on charts for a permanent record. After some experience, it was decided which thermocouple provided the most critical control, and from then on, the desired tem peratures were regulated by this particular thermocouple reading.
The furnace, which was oil-fired, left no deposit of soot or other im purity in the fibre product since complete combustion took place in the chamber outside of the calcining tower. A gas-fired furnace would be
ideal because the combustion cham ber could be reduced in size or en tirely eliminated.
The pilot plant bnilding was a three-story structure located on a railway siding near the asbestos mill at Asbestos. In the basement was placed the mechanical driving mechanism for operating the air locks and a fan. The first floor con tained the combustion chamber, pyrometer recorders, oil burner, and fibre-feeding conveyor. The second floor contained the bagging spouts where the fibre was sampled, bagged, sewed, and chuted to the boxcar for shipment.
The flash caleiner unit was 26 ft. high by 81/j ft. in diameter, and was lined with fire brick. The bot tom of the caleiner was conical to enable the heated fibre to drop au tomatically into an air lock and be removed from the heating unit as rapidly as it collected.
The natural fibre was fed to a fan unit that gently willowed the fibre, freed it of lumps, and suspended it in an air stream so that it would fall by gravity down through the hot gas-heating zone. Peepholes
36 --
UCC 004657
into fibres possessing properties competitive with those of natural semi-harsh to harsh fibres. The pro
volume resistivity,' are all a direct function of the temperature and time of heating.
<3) Nutting, P. G., Some Standard Thermal Dehydration Curves of Minerals; Professional Papers 196-198, P.T.B., 1941--1943.
cess, a flash-heating system, was
operated as a pilot plant at the rate of 2 tons per hoar for several years.
(5) The tensile strength of heattreated fibres, as well as the strengths of asbestos-cement panels containing them, will decrease as the
Gill, A. F., The Thermal De hydration on Composition, of Certain Minerals and Salts; Can. Jour. Research, Voi. 10, 1934, pp. 703--712.
(2) The process allows the mine temperature and time of treatment
Wolochow, D-., and Whit, W.
and mill operator to control hts product and tu produce any desired texture for fibres grading from
is increased. However, this disad vantage is minor and the products are equal to those obtained by using
H,, Thermal Studies on Asbes tos; Can. Jour. Research, Vol. 19, Feb., 1941, pp. 49--56.
Group 3 to Group 7 and 'floats,' at nominal additional cost.
natural semi-harsh to harsh fibres.
(4) Badollet, M. S., Asbestos; A Mineral of Unparalleled Prop erties; C.I.M., Trans., Vol. LIV,
(3) By heat treatment, the phys
1961, pp. 151--160.
ical properties of the fibres have
References
(5) Anderson, H. V., and Clark,
been partially altered by the re
G. L., Application of X-rays in
moval of small quantities of mole cular water and a partial conversion
(1) Fankuchen, I., and Schneid
er, M., Cow-Angle X my Scat tering from Cnrysotiles; Am.
the Classification of Fibrous Silicate Minerals Commonly Termed Asbestos; Ind. and Eng.
i
of magnetic iron oxide (magnetite) to the non-magnetic oxide, Fe.Oj.
Chem. Soc., Jour., Vol. 66, 1944, p. 500.
Chem., Vol. 21, No. 10, 1929, pp. 924--933.
(4) The improvements in filterability, increased bulk,increased ab sorption, increased surface area, and better electrical properties, such as
(2) SOBOLEFF, N. D.. and LaTAXINoff, M. W., The Cause of Brit tleness in Chrysolite Asbestos; Econ. Geol., VoL 28, January-- July, 1933, p. 171.
(6) Badollet, M. S., and Streib, W. C., U.S. Patent 2,616,801, Partially Dehydrated Ckryeotiie
Fibres and Method of Making; also Canadian Patent 504,310.
-- 37 --
UCC 004658.