Document K6Y7QRBbOpkXqaoZbNkBa5NQr

2815 CALDERA AVENUE POST OFFICE BOX 18 BEAUMONT, TEXA8 17704 TELEPHONE (408) 836-6011 FAX (408) 835-5177 (408) 835-5728 MtHAhhY & WEBER A PROFESSIONAL CORPORATION ATTORNEYS AT LAW ONE ALLEN CENTER 500 DALLAS. SUITE 1200 HOUSTON. TEXAS 77002 TELEPHONE (713)655-1200 FAX (713) 865-0222 1006 GREEN AVEN POST OFFICE BOX ORANGE, TEXAS 77 TELEPHONE (408) 886-7766 FAX (409) 886-7780 August 24, 2001 Re: Cause No. 10346*BH99; Donald R. Kinsey, et at vs. Owens Corning, et al; In the 23rd Judicial District Court of Brazoria County, Texas (M/W No. 0829-0338; Dow No. 0002086) Mr. Allen R. Vaught Baron & Budd, P.C. 3102 Oak Lawn Ave., Ste. 1100 Dallas, TX 75219-4281 Via Facsimile: 214/520-1181 Dear Allen: As I indicated to you by phone 1 would like to take the deposition of your economist Dr. Thompson in this case. In addition I wanted to take the depositions of any liability experts that will offer any testimony concerning The Dow Chemical Company. I know you have a very long list of potential expertsTn the case and I know that most ofthem will not testify but to the extent that there are those who will testify I would appreciate if you would let me know that as soon as possible as to which experts will be testifying and provide me with some dates when they can be made available for deposition. Thank you for your consideration. Very truly yours, ARA/fmh Arthur R. Almquist, For the Firm MW/116381 ".I HOOD DESIGN DATA 4-7 H in, therefore, desirable tn minimize the air stream contraction which occur:; at (he vena contracts zone by rultable hood design. Figure 4-3 illusirntes the effect of hood design en the ciitry coefficient urul on ihe -) entry loss in terms of velocity head in the connecting duct, the latter being another way of expressing hood entry loss. Consider;::;..'; the grinding wheel hood r'u. vu in Fiirnrc 4-3, some typical calcnhitions a re'as fiillo'-vs: i Example;^'robbum I GIVEN - 1 C = 0.7(1 e ST1. 2.50 inches water li ') -J Duct Diameter - 5 inches Duct Area = 0.136 square feet TO PINO a. Air Volume b. Duct Velocity c. Per Cunt Loss in Velocity Head a. Q = 4005 CA c_ /SpTh 4005 x 0.73 x 0.136 /2d.U G72 cfr.i 2.50" H20 (GVj.) b` % A ' 0.156 4050 Ion: c-vp " te)3 - {MJ * v.'h'-iv Si'j static prensusv, inches '.>'.~ier V d -- velocity pres care, inche: vib-ar Ji e -- lium! entry loss, inches wafer 1' - hood entry toss factor SP. = VP + |i 1; c h. - ST', - VP e Ji X.50 0.0R I; " 0.03 l.r,v - 0.(143 c: Loss = p n 100 0.Si5 x 100 ci.Gm As a veetilattijn r.landa-d, static pressure alone without reference to the duct diameter is meaningloss. I i.'. cr.'Hsiiv-; the branch d' a' si:'..- reset;; i:i higher vein: itv, gr-vAor rasisuiuce and u hj'./cred rate of flow al ii di vim static pr-'-.-.-su re value is inures re-1, fii; ventilation perfcr:n'tnc.e m li-vida should he based pri- ih,' i).! ail V"li.""r-..- J,;, i Ikd. H . - sv A1 r Pi si vil "!; an v ' I c,,.-:.- ;.i\- i.s si i vc ucc'y uce.' !<s ) i c e unifur: :C';r-t aii fl ee at : .decuata Cash.re velocity over a !- . ' i of sec.aa .1 4 yore rutin':--rich s--i an lank-or oyer Ihe face a ir.rfe bond such as a side c .'six.:. The csicfion .! the slot i;. sole';/ io ohiaia iccp-r aimlh-trilr.ij is-i.- Met v aloe tty does not c.c".- . d. o-.v.im* :/ c".; '. rho-.-ity: a Iil..h ski velocity slimd;' ana `rat-'-s high press:in- l-issrr. Note H.ai the enp- \ .kid y ..ho !;u:v 4-4) si '.".o dad the capture velocity is rcViivd r.o the cah:>"st o'-ume ami tee l ' Lr . Ihe v'l v-dciaty. i: . :! - usual iv coa A -1 of a rva'v i--. : - > a"'--re a . .eui a plenum e"".:1 '.dm err " ;':v:si r; r cl ;- ' i : sci o-.s dm i ; -oi'i; in-ii hy can.-V; ..rSiya. dpi tf 'V vanes nvu; hr u in the p'eaurn; however, in Li.a.rial . s.-t ;,y..l'aas v.'nos a 'c subject to co 'Osoph acd/or crcsioi; uad i>rovic!e locations for i; / i; r..|- shits van i-o i;rnv;.;!;-d ij>i' S"y a re subjerc to ta .sparl.y; a;r! mat; .djustrract. i : a: ' i ] a.ad:c hie i: 'n ` >; ^ !m> Lae'' 'A:: r..-'! iinolx-lriicfe.i pienuvn tjve- ` ' nesiua of the slr>t and ptenui.i : : aiiti'i! iso os.sn v lo.-.s ;hrov:;> 'he slot is inyh m-;';: :\-d V/iv;i the ssure loss through the plenuai. II i or: i ass si `ha rad as.- sub'seco-'1 .o ns.sar.fin !!y aaral surtioa and the slot velocity \vili be os? antially i i i o a:; ai'da -ii" d .ai-'ro'l he- calnjlatipa'; the pressure amp iron pn> end to the other of a slot :!' i:a,i{"i. *. v.;, y :-;afiil upproxij!i.*.*ion, nifplio.i'ite fo suist hoods, is to ricuicn for :i lniLXimuni : \ :!.verity i /nt Vo 1/II o; slot velocity. For Taos! siol hfH-.ls a 2,0';`t :pm .slot velocity amt 1,000 fpm Vv-Vv-i: .a : p. ;>r ,, vii.ie v.i.'i.icu for laiiiorniity of 1!.y*v and nv Ciar.-V:- pressure drop. Following are . .. .1 :1 -sh.i: a i:i,r . a as: l'a: a :::: f!--s:y.i n. in tin; s make-a practical plenum sire sirs a dm air ;.m> roaches i di s : ia .: \rlarpe. g ....;> piaru-s t a ra p. .ssiit'e, r s with :v;:Aecat ivraJs. the slid 's a- I a . 1, a;', ins a.';'a a : 'I; fpri plrcuai velocity. : ad i'vs *i iri.: :v i; ; - r; ph-nuui si.'.sa is'cauit' nil of the air .'.Hist suss in ane direr't'.oi'.. CAPCO KIN 0000482 4-C INDUSTRIAL VENTILATION Nob* Unit where* slnl-plt-nuni lion's are used fur dust control, plenum velocities music I><j 3,0C0 [pm or higher to transport particulate matter (hrough the hood. Otherwise, saiHing and plugging will occur. Calculation of Static Pressure Losses in IJ.-rliaiist Hoods Simple lloocls: Plain duct openings, flanged duct openings, canopies and similar hoods have only one- su;nilicant energy loss, at 1'ne point where Hie air enters the duct. At this location a pronounced vena contractu is formed and an energy loss occurs first in the conversion of static pressure io velocity pressure. As tiio air passes through the vena contract-., the flow area enlarges to fill the duct end velocity pressure converts to static pressure, again with some energy loss. The more pronounced the vena contracts, the greater will be the energy loss and hood static pressure. The hood entry loss (lic.) can be c.vpre.ssed therefore in terms of <1 single factor (F) which, when multiplied by the duct velocity pressure (\ f*), will give the entry loss (he) in inches of water. K.vn mo I? Problem 11 In a simple hood (Figure 4-f>) the hood static pressure is equal to the velocity pressure in the duct plus the hood entry loss. (See page 1-3, `-Acceleration of Air and jfood Entrance Losses''.) The velocity pressure rvprc.-s.-nts `he pressure neres^ary to ncceb'rate trie air from rest to the duct veiociry; ihe hoed entry loss rep resents the energy neces .ary to overcome the loss as the air enters the duct. Tins may by expressed as: PPh `od r Vi> , cl m.1 en f-.'-.u velocity is !<*. th?u 10CC Sam V.vhesi face veloci-./ is nigher '-..tn ICnO fpt-a, ihe hoed ire.bed as a corp.oocc.d hood. Fee f'dhj'.vj:;.;.). n-j \. here: i;.^ - entry loss of transition (Gee Figaro 0-10) v'Pd, - Duct Velocity Pressure typical cr.lc.ofiifion is as follows: Given: Face Velocity = -- = ?.50 fpm * 'fac.o D"-ct Velocity = = 2COO fpm "duet VV.u .= 0.25" *' - O.V.'1 VP{: s-'h ' \ i ' v" V U'.'k'* j ''-7rz:v;ii.:rn /.Af / ' Y. Dvcf i1. % s ...VL /"iV -ironsition /css J ;>cice? of h C>h)} lo^r, '--.5V:?/' velocity Fiy. <-7 1 V. I;, o- of iiood- i f ::- ;:.*' v. ' r;-r: 1 ;i 'ri.: - -fj > ;' : :v * c h::'-:1:.' ^ ri/j-t. - two or more pu-'is of sisn:::;:',iV on-r::y i. ss curb rc.'ist be L`.? Iiom'Ik 1iuvi0f. di'u'.iip ..rv itiSd-v 'ol tyf'fe >iy (;< y US*d OP. f t`i;;pin;.r and di'/r U\:>;w t'-'ici CAPCO KIN 0000483 it -- .! ! 1 ! tv. A HOOD DK3K1N data d-9 Figure 1-7 illustrates a double entry loss hood; this is a single slot hood vith a pU-rium and a transition from the plenum to the duct. The purpose of the plenum is to give uniform velocity across the slot opening. Air enters the slot, in this (-.use a sharp-edged orifice, and loses energy due to the vena contractu at this point. The air then continues through the plenum where the greater portion (if the slot velocity ir> retained because the air siream projects itself across tee plenum in a manner similar to the "bluwiiig" supply siren..i show;, in Figure 1-6. (Ti.*> retention of velocity in the planun is characteristic of most local exhaust hoods because of the short plenum length. In the case of very large hoods or exhausted .vaT-d rooms, however, the velocity loss must iae taken into account.) .The air then converge.-, ir-to th- duct through the transition where the second significant energy loss occurs. Example Problem Ilf In Figure -5-7 the air enters the slot, a slot entry loss occurs and the air Is accc'erati-! tn the slot velocity. Tt then crosses the plenum and enters the duct through the hoed transition where anether entry loss occurs and the nir is ncce'lerayi further from its initial velocity i:i the slot to the higher duct velocity, In'niost cases, the clot velocity is e.-run! to or lower than the duct velocity; in all cases, however, the air must be accelerated to the higher velocity, Ike hood static pressure ior a double entry hood can he expressed as the conation: SP, - h + VP di t VP, - VP h to u cd ds thus; (1/ b>\J. -= hi;s f ht-d + VPd. .'ira duct velocit.y .is.r.re-ilur thrui slot vsio-.av (.7) IIP,h = hes + hid, + VPs vhea slot velocity Is great.*;' than duct y!cc `.tv here: h = entry toss through slot (bee Figure C-10) VP ~ slot velocity pressure h - entry le.-a ; r transition (tve ; i-igure 6-ib) VP., -- duct veracity pressure P tyyii-il crilcu'.ativin s, usii;;., - Kecati' >u I'1, arc ns follovs PI;.tier : _Q. 'VdOt - i . 7 v'j' s `P'o F<"v.?h..ke.c>t Hood velocify - I nOfl av VP - 0.07" s 1; e; slot - 1.73 V'P J, j r:: Pact '.'..V. ity 3,'iO y ' !! h VPc,i 0.76" h , t; en.Mtion id r0 Cd VPd 0.7 j VP . n ( I 0 id) - ( 0 o.7-` fit', - i.73 VP * 0.75 VP, + VP, 1-. H a c. o,>: FP., (1.70 0.07; (o.y sr. -- 1.07(6" = 1.07" ll 0.70/ 0.73 CAPCO KIN 0000484 4-10 TNOUSTKIAL VENTILATION Tilt- use of t;-;qurtion 2" is illustrated ia the case of a hoot*, where: Slot velocity - -IG'I'O ipa.i Duel velocity = 2fli>0 !';n VPs ^ 1.C0" VP, = 0.25" d sp,ii =ii es + h. ed + vr- :;- s = (1.78 x 1.00") + (0.25x 0.25") SP. 2.8425' 2.04' + 1.00" * in an actual installation there may be some regain of the higher VP us the air passes through the hand. r :s not possible lo predict this, however, and i.t is better to assume that the energy requirement is us ohova. Certain hoods may be constructed r'th internal bullies and/or slots and con have more Ur.tr. two significant energy losses, in such cases, a simple step-by-step calculation of ail losses will result in an accurate ..nforruinaticn of SPjj. Yard i''.t'Oii of itndioartiVH I lugh Toxicity 'opera'icns Vt'r.tilntu.n of rr>dioiti.-tjvu and high toxicity prccr-ssa-J requires a knowledge c.f the Ituvasiis, the use o\ pro. ea control methods :>d oJ*Muati maintenance, i.iciudir.j; ir.nu.lioriii.t. While the d-.yr:-.- ::: air ,jj . clear:;,ness required will vary with the operation, in most cus.-s the r>rdr of cle:t:rr: discharge to ul'mephenc will be coaxidere rly l.-youd fh more usual industrial clean air rhino nr fix. The chemical laboratory exhaust hoe d (VS-203) illustrates typical >gn crterPte.. The vr flounce of I't'dy co.vcuts from air supply sy.-icris, the care in sizing rue locating r-xhaast eammjti-.ns, the of air flow i.tl'crr.; within the hood and die cie'.ir.iny of crhaimt gas;';; are much more Ir.vo'vect than the .lo of cm mb rt -- ol.'oris ice usual laboratory hoods v-heru dilution ventilation greaily contributes :ci suii-.'-CKiry control. 'I a,- scare care is rrr-srdatory for air supply ."ml exhausi systems and the sel .-ciioit of air cle'-taing equiptnuric. At- cnVuninj; of supply air is normally cl a high order of efficiency .'.no the e.'aih .st air cic-rning is often a roi'.'iir.'(ion of hi;ch-e;';:ciu:u:.y collector''' or filters bached up by absolute or is Ira. high-efficiency designs. E .. sure of service and cb'.fiimir.atio'i ItaswriLs fr.'u ser'icic.g or rpjilaclitg collector or filler . ! jus' the axyer.siv : cquirw.it so offer V.Td cuot collecfcr d dyas in pm.cv of irexpe-i- a: 1 idler;; mu ; s'lira m ..pii.d ;nore safely fir .l iraiy a Cp-du::ii:sb dip ot ;i;i are:' less like1/. Itoverae h'd-vic brne v.-itt be us-*d in ;;iu;e of lass vy.js::->iva conventional fabric because Ibrc a --fewer f. ef ...or o-uls to ) .:d; no;! a-s er chaw ,U to bo r pi fund, .rriiait'g or yrafilccr:. soslsli --f h; s pries i;;::: ne- s ! = f b a r., \.. 'i i iv.u.'.i.. repl'-c eai-'ot cycle, raih:i;s hruifidr ;:, V isle aiapos :: and rose i ale cards -mi. alien ijrcia- .o ... ; : aar, V;.iy ;;o; es:-. 1 : .das shfaad b> fi,Eo.v,.j : lias; ;;is ,1; s.i of hoods for radio.clive r.rd od;h fnvicia/ r.iu- L iy a.;!..;; is abic) rudionctiv" oiad- rial- are haadii-d s'leeUi be aticUiy ! as r inch as pos.-ibh; in ;;revi a.:-' - : imaaii'..rye cir vr-h..',;-is. i`rhe use uf yiove bo:ms iniiiiu'by.eS air vj'.viei oral aw.Uf as ; : - ' * :ne s' pc. Vr x.) . 'v". v-d.;i a c ao..;, -p irc'd-y . ,,fr.a!. pacejp : .sj;.'!.. cm so !iiey may ioasoi; laads;;:' d:u:: and dust a. T a vt. ".a a. o ' .> i v v j d -.on f ro n the i:o,;c am si bp n;--*. Lain fee vobi"n of couhirninutfed gnscs, ,;.|;a; p.,1 ,J-,, ,,-,j . d a;! 1-, `Im "peiTii i.rin rrriaicirr iacye mounts of wet di-o s'ion n:ci vc 1.1 f;Ui:-.rd iscid or solvent treut- a; at ah jem la'ia dinrp in one yj of hoods :o'd !h" ha ad i i ag of cry nad'ain! i:i others. a"; a (h.pap a-r ispi y fih'i'ihl bp icpiovsil !>;' fiifr.itiOu as close to the hood ns pr.icti- .'. : a; ,.; c - ."f uar"a- a -v c o,i,';ic:i;;;dp.-'n of aqs ..pmeut nsai dr.i iiv.j ' f ' a1;:: or ecour,-:..:;;'dry of ihe rrotpriai ;:)ay n^sipn so ihat even !!> sniullest chips and t c. cm.,p c>.c b" v- s',!' V. a.d qa dr s.iy, y ap;or. Is ,a:e the 'u oci iraiy be reccssury, Perianalsy on the ,.yroioric :isiure of /pi". '.'b,;py Up.aaaimiliciiof f.i- !: yj ;,n,i sysfam reus; he made us ousy ns giossibie mid va : a a a.i "if-/ ah' '""'ii at eoi is used tha ma hd j: . ids id iho hr id for ibis- raesori. ' . a ; ' a '. aa: d" u-.-jr-.,' ,..., ppavre's ivithin building : i i nd";- a negufiv--' or-'-idirp. 1 . da lyp- h.a ds, a':' face Vtd irdy o f 125-200 frm e ad a mini mam face vel .a y : ' y . .a s' i,p , a.a . jr<> i.-i.suru tr o ':or,tn:.-'.;c.->at v/ouid i-sa.i;ce inip Ihu room, jn addition, f:;cp CAPCO KIN 0000485 5IC0D data -i-it velocities of laboratory hoods >.vi;h adjustable fronts should be control led within reasonsbk* Urjita in order to reduce the i-.'sfunee* of air-borne materials within the hood. Tliis velocity um.kvl cun be accomplished by eithw proportional bypass (constant volume) or controlled lace velocity (variable volume). Hoods with h 1 : heat loads should have a major portion of the air exhausted through the slot at the lop. In i:i" Utboralnry handbag of hi;;h alpha or beta emitters, enclosed glove boxes .should be used. V-'ith the r.ef-'-sr.ury fight construction, an exhaust volume of from 2f> to EO cbn is usually sufficient for these enclo sures. The air locks tveded with these 'roods should be exhav.slc-tl if they open directly to the room. Adequate quantities of makeup air must be furnished by meclanical supply systems and intelligently disii jbidod with rclution to exhaust points. Supply air distribution mujt be nr.-v igwi to provide ;;er.eral air flow from clean area;; toward more ccnlaminated areas. Filtration of supply air is necessary to reduce air-borne dust concentrations, thus prolonging the life ot uitrahigh efficiency exhaust filters. The use of prefifters in laboratory type hoods for radioactive materials prevents contamination of the ex haust piping. A gauge should be installed indicating pressure drop across the filter, so that the filter will be replaced when pressure drop exceeds design value. Filtration of room supply air will prolong the life of u'.iru high efficiency hcod exhaust filters. Where there is a possibility of spontaneous or continuous release of ioxic icnlcrin's, or where sm-^rnl t -.v.N ere connected to a ;r;<le exhaust .'astern the exhaust fa,, ..houfd !;s operated continuously. Srtimfr-y fan c; p city should be available for breakeio'-m CAPCO KIN 0000486 CAPCO KIN 0000487 iOOD Di-'SICN DATA 4-13 CAPCO KIN 0000488 4-14 INDUSTRIAL VKNTILATION PRINCIPLES OF / .Q*l uo) n CAPCO KIN 0000489 -'iy i< r \ \ />(l / if /f)/ fj '.j . $ rc j ;-j v;, -v; PFWCfPfJzS OF FFFVJST HOOL / t CAPCO KIN 0000490 INDUSTRIAL VENTILATION % 2r Spurs? - Source - FREELY SUSPENDED ROOD 0 - EOXEa }v Refer in Section 4 CjO LAPSE HOOD Largs f.ocJ, X small-- measure X psrpefidicuicr to hood Lace, not tec; then 2X from hood edge. -vY - 4Pf ST \ HOOD C ' as,VCR OR HEDP Q-Q.70( !0X2r A)V Q = 0.75i!0X~-e A)V SUSPENDED HOODS fSmu/J Hdo-rJreR hoods) 0 - Required exhaust voice-;?, cf.n X- Ohtcnre from hood idee to forfresI point of con>cmii.c,:r rot-ease, Her. A ~ Hood face area, sq ft V ~ Srphirn >.>e.!cciiy, fpm, at distance X. Note; A;r fchxne must inc'ruse os the soon? of d'Hcnse of to- coerce from the hood. Lin-rung iy ffanning -m iy /. Cring on renoh. door, cot. ins e LeireficiR effect. X.1- _ - tr.r .J XL O --r CDECRY HOOD d ~ /. : i-'i ; P- perimeter of fee'-} i ' reesmme/,-?:/ if mcleric! is ionic end oortoms most beret o ,cm svcrcee. V ranges PO to rp-n tiep-n dmg on crsccdrcri:. Side cm Irina cm too or fcr.ee Sees in . ' c re s- tmmih or i'onih O'- te-irnbie. Saiiobh do-' stem v-gcr or other innocuous ESEXPCY CCER ACEEX. C? :57,UAl H?G!sMIS7$ HGGD DESiEH DATA at; m- rta P-iE CAPCO KIN 0000491 design data 4-hi `.r >c -Sourea---------- FREELY SUSPENDED SLOT 0=3.7LUX -0 Q = .3 LV> 0 - Required onreuet volume, cfm X=Distance, 7?.at, hood fees to farthest point of scores (usuoily on centerline or heed) V=Ccp;urs veheuy, Err, or dlnfrnce X L=Lo;:prh,fnNf cf iu-od. NN. irbd frd.o. c\ \ 7= Wider, fed, of /EEs, iorf ere fQ ^ v" --L < i-.o !"/ ' .A' 'jf C)=CLW -1 ...... f,! NT ON TO. NX n-.-. C:, in.'if 0 in D .'/ ' :.A' mil h ; c.r. < S rl.sr^GEO :;\or n- c? w ;i : ' V' / ;'r . . . top '? ON'S f NN/'Or. rr.p.r WXY.D. :.:.; ; Al. ..-l-' : V. fo.n r z~ '.'/.i; o -i-- i 1 ; ~ J v/ --- '... ~ c-*'* . t -! :~On ! hip. CAPCO KIN 0000492 - r{ . i i J ?.?k { i t;DVOTiu.\v ij>:r.i.A'rio>; :`f.n f-' Eg i: hi i \ \ * i ) CAPCO KIN 0000494 )N' t Vl'ilTj LATIG.M 7 h: t'C a/ i ('. oo l r CAPCO KIN 0000495 SPECIFIC OPERATIONS I>-o7 "5!AND !DL Ef\ :fr, VO :VA'Cr!. CAPCO KIN 0000496 Cement Asbestos Products Company Woodward, Alabama MAKING ASBESTOS-CEMENT PIPE Introduction Asbestos-cement, as the product is called, is made from three prin cipal ingredients: asbestos fibre, cement, ar.d silica. Mixed in preset proportions, the ingredients are consolidated under pressure to form pipes having dense, uniform walls. After formation, the pipes are subjected to a steam-curing process that improves their stability ar.d structural strength. The resulting product is a strong, corrosion-resistant pipe suitable for under ground piping and industrial lines. For example, such pipes are used for water and sewer systems, irrigation, electrical conduit, ducts, vents, flues, and stacks. In 1904 when asbestos-cement was introduced in the United States, it was in its simplest form, a plain gray slate, cured under natural room con ditions, but it has since progressed from this simplicity. Most people who use asbestos-cement products consider them as a masonry product, but the manufacturer of asbestos-cement knows that there are two major classifications of asbestos-cement products--normal cure and autoclaved or steam cure-- and two distinct manufacturing processes--the wet method and the dry process--which give definite characteristics and determine where the asbestos-cement products are used. The method used by Capco is the wet method for pipe forming and then autoclaving or steam curing. Composition and Basic Materials In normal curing the product, as it comes from the manufacturing machine, is allowed to air cure at atmospheric pressure or in a moist cham ber. There are those who have the mistaken idea that the cement has to dry in order to cure. The opposite is true, not only for asbestos-cement but also for all products made with hydraulic Portland cement. It is necessary at all times to keep masonry products moist to hydrate the cement for at least 28 days, a period at which the composition has approximately 90 per cent of its theoretical strength. In work done at the Portland Cement Association it goes even further and states that in atmospheres of under 50 per cent relative humidity cement fails to hydrate. In normal cure manufacture asbestos-cement pipes leave the machine with a water content of 20 to 25 per cent, thus insuring adequate water for hydration. CAPCO KIN 0000497 2- - In concrete work subjected mainly to compression, only a.bout 15 per cent cement is required, but with normal cure asbestos- cement as much as 75 per cent cement is used for the strength. that is required for these relatively thin members. For an autoclave product the formula is similar to a normal cure product except that silica, 200 mesh, replaces part of the Portland cement in a silica/cement ratio of .6; or, the silica is 40 per cent of the total weight of the cement and silica. The other difference of an autoclave mix is the cure; an autoclave mix must be autoclaved at high steam pressures. After forming, the auto clave product is precured first in moist heat oven for one to one and a half hours, next air cured for four to eight hours, and then steamed in an auto clave at 100 - 150 p.s.i., about 350 degrees Fahrenheit for eight to sixteen hours, depending on the pressure in the autoclave and also on the pipe being manufactured. Usually thicker pipes require longer steaming. The quantity of asbestos in the mix has a bearing on the strength of the product. Each pipe size and service may require a different percentage of fibre, determined from experience and the strength necessary for a satis factory performance. For_many years it was thought that long-length fibre was necessary for good strength and that the longer the length the better the product. For pipe this is partially true, but openness, degree of fiberization, and freedom from grit are more important than just length alone. The strong asbestos fibres behave similarly to the steel bars used in reinforcing concrete. The fibres used involve Groups 4, 5, and 6 of the Canadian classi fication. These grades of chrysotile asbestos are generally classified as medium length fibre; they are used extensively in the manufacture of asbestoscement pipes. One basic requirement for the asbestos is that it must be fully fiberized prior to mixing it with cement in order to obtain the best properties in the final product. It is also important to remove or minimize such impurities as dust and grit. The mixing of the asbestos and cement slurry is highly important in the wet mechanical process, because the slurry must be distributed to form a thin film across the entire width of the machine. The open fibres from Kollergang are combited with the cement and mixed with water in a turbopulper fitted with rotors in order to open ^remaining clusters of fibres. The relatively heavy paste mixture in the turbopulper is delivered to a stirring CAPCO KIN 0000498 -3- vat where it is pumped into overhead containers for delivery to pipe machine or recirculated to this mixer. It is important that agitation, be constant and effective in order to prevent separation and settling of the solids in the slurry. The slurry flows to cylinder vats of pipe machine which are fitted with paddle agitators to prevent settling of the stock. There are nwo of these vats on the machine. Each vat contains a horizontal cylinder covered with a fine wire mefch screen.and fitted with seals at its ends so that flow can occur out of the vat and only through the wire, thus leaving a thin, even film of stock deposited on its surface while removing the major part of the water. The thickness of the film depends on the slurry level in the. vat, its consistency, and the speed of rotation of the cylinder. The machine is usually operated so that the film deposited is approximately . 002 to .010 Inches thick. The continuous woven felt travels above these cylinders with its hairy side toward them; it is kept in firm uniform contact with them by heavy rubbercovered rolls. At the contact surface, the film of stock is transferred to the felt and some water is removed. Each cylinder adds its film thickness to the web of stock on the felt. Additional water is drawn from the web by means of a vacuum box placed under the felt as it travels toward the cast iron or steel mandrel. There is a vacuum box between the vats to seat the stock web firmly on the felt. , As__the web of stock passes under the mandrel, it is transferred to the mandrel in a continuous operation until the pipe is built up to the desired thickness. The water removed during this operation is returned to the mixing area of the machine. This water contains a small quantity of asbestos and cement from the stock that has passed through the screens and the felts. It is first retained for a period of time in settling tanks to clarify it. In addition the water very rapidly becomes saturated with soluble materials from the Portland cement. This latter operation is generally beneficial because it eliminates fur ther leaching of lime from the cement as the process continues. The solids separated from the water in the settling tanks are returned to the mixing cham bers separately from the clarified water. When the felt is returned toward the vats, it is cleaned by means of shower sprays and vacuum to remove any adhering stock particles. It is sub jected to considerable strain and wear; usually it has an effective life of only six to twelve days. Similarly, it is necessary to prevent the cylinder screens from clogging. They are cleaned contiguously during operation with a shower spray immediately after the film of stock has been released and before it is dipped into the vat for a new film. The process needs to be controlled closely. Attention to cleanliness is important; otherwise, there may be clogging of the cylinder screens and the felt, and an inferior product may result. CAPCO KIN 0000499 4- The experimectal manufacture o asoestos cement pressure pipes was started in Italy in 1913. Progress was rapid, and oy 192.1 .asbestoscement pipes had bear, accepted l.c. Europe. At v>at time tue Brinish Ministry of Health approved nke use of the p'pe for watermains. They provided for loans for these pipes with a repayment period of thirty years; this period represented the same period .allo wed for cast iron pipes. This type of pipe gradi ally superseded both metal, and ceramic, piping in. a large number of applications because of the fact that they are resistant to corrosion, impervious to and free from electrolytic action, when, buried in the earth, light-weight, elastic, strong, resistant to com pression, economical to install, and 'unaffected by iemperature changes. Tests have been conducted on pipes after thirty years in service with the conclusion that they had retained their original properties. These pipes have a smooth, glossy, cylindrical internal surface, and offer very low hydraulic frictional, resistance to the flow of liquids. The Ital.it Mazza asbestos-cement pipes manufactured by Efcernit, Genoa, Italy, are still in operation throughout the world. Their experimental data shows that the carrying capacity of pipe is on an average of 25 per cent greater than that of new cast iron pipes and 30 to 60 per cent greater than that of old cast iron pipes, all being of the same internal diameter. Asbestos-cement pressure pipes are manufactured on costly and complex machines which are automatically operated by means of hydraulic and electrical controls. The pipes are built up of a continuous, uniformly thin and highly compressed film of asbestos-cement. The Mazza process is the most important commercial process used in the manufacture of pipes. The diameter of mandrels varies from three to fifty inches. Because of their weight, the larger diameter mandrels are more difficult to handle. These large mandrels are usually mounted in pairs, one attached to each side of the machine. The machine permits wrapping on one mandrel as the previously wrapped pipe is withdrawn from the other mandrel. CAPCO KIN 0000500 MIAINC. Op MAieClALS MANDREL. LOVJcXlU <. F^- I*: W mandrel RETU RN MANDREL e>T*x<.^er Wat OVEN <eisvl cumoiR. P\?E P6ivA\>tG a vkts _______wHim C AlEnq (1) Asbestos Fibers (2) Cement (3) Silica flour (4) Water ?lov diagram illustrates major equipment items used in forming asbestos-cement pipes. A mixture of asbestos fibers, cement, silica, and water is formed on metal mandrels in pipe forming machine. After calendering to loosen pipe from mandrel, pipe and mandrel then move through an oven for precuring, then to a mandrel extractor. Prom the extractor, mandrels are returned by conveyor to the pipe forming machine, and pipe are stacked in curing trays, The pipe stac'-rsd in curing trays are moved to auto clave area and~allowed to air dry for several hours. The pipe on curing trays are then placed in auto-claves which are high pressure steam curing vessels. After curing in the auto-claves the pipe are first subjected to a bending or flexural test, then machined on each end, then tested with internal water pressure and finally pacvaged for storing and shipping. 0 -=FLex - Te*r 1 INTERNAL PRE^ORE T6Vf STORvuc. 4 CEMENT ASBESTOS PRODUCTS CO. RAGLAND. ALABAMA "Dl AOO.A kAX-p C Pipfc MANO^C,XvSt. DRAWN: APPROVED: SCALE: -- | DATE: 4 11 -5* | DWG. NO. A- r CAPCO KIN 0000501 ASBESTOS PRODUCTS COMPANY Sales Offices, Woodward, Alabama S5189 / Phone 205 i28-12il / Plant, Ragland, Alabama 85181 MAKING ASBESTOS-CEMENT PIPE Introduction Asbestos-cement, as the product is called, is made from three principal ingredients: asbestos fibre, cement, and silica. Mixed in preset proportions, the ingredients are consolidated under pressure to form pipes having dense, uniform walls. After formation, the pipes are subjected to a steam-curing process that im proves their stability and structural strength. The resulting product is a strong, corrosion-resistant pipe suitable for underground piping and industrial lines. For example, such pipes are used for water and sewer systems, irrigation, electrical conduit, ducts, vents, flues, and stacks. In 1904^when asbestos-cement was introduced in the United States, it was in its simplest form, a plain gray slate, cured under natural room conditions, but it has since progressed from this simplicity. Most people who use asbestos-cement products consider them as a masonry product, but the manufacturer of asbestos-cement knows that there are two major classifications of asbestos-cement products -- normal cure and autoclaved or steam cure -- and two distinct manufacturing processes -- the wet method and the dry process -- which give definite characteristics and determine where the asbestoscement products are used. The method used by Capco is the wet method for pipe forming and then autoclaving or steam curing. Composition and Basic Materials In normal curing the product, as it comes from the manufacturing machine, is allowed to air cure at atmospheric pressure or in a moist chamber. There are those who have the mistaken idea that the cement has to dry in order to cure. The opposite is true, not only for asbestos-cement but also for all products made with hydraulic Portland cement. It is necessary at all times to keep masonry products moist to hydrate the cement for at least 28 days, a period at which the composition has approximately 90 per cent of its theoretical strength. In work done at the Portland Cement Association, it goes even further and states that in atmospheres of under 50 per cent relative humidity, cement fails to hydrate. In normal cure manufacture, asbestos-cement pipes leave the machine with a water content of 20 to 25 per cent, thus insuring adequate water for hydration. Manufacturers of PERMAFLEX Water and Sewer Pipe CAPCO KIN 0000502 2" - Ia concrete work subjected mainly to compression, only about 15 per cent cement is required; but with nomai cure asbesto6-cement, as much as 75 per cent cement is used for the strength that is required for these relatively thin members. For an autoclave product, the formula is similar to a normal cure product except that silica, 200 mesh, replaces part of the Portland cement in a silica/cement ratio of .6; or, the silica is 40 per cent of the total weight of the cement and silica. The other difference of an autoclave mix is the cure; an autoclave mix must be autoclaved at high steam pressures. After forming, the autoclave product is pre cured first in moist heat oven for one to on^ and a half hours, next air cured for four to eight hours, and then steamed in an autoclave at 100 - 150 p.s.i., about 350 degrees Fahrenheit for eight to sixteen hours, depending on the pressure in the autoclave, and also on the pipe being manufactured. Usually thicker pipes require longer steaming. The quantity of asbestos in the mix has a bearing on the strength of the product. Each pipe size and service may require a different percentage of fibre, determined from experience and the strength necessary for a satisfactory performance. For many years it was thought that long-length fibre was necessary for good strength and that the longer the length the better the product. For pipe, this is partially true; but openness, degree of fiberization, and freedom from grit are more important than_just length alone. The strong asbestos fibres behave similarly to the steel bars used in reinforcing concrete. The fibres used involve Groups 4, 5, and 6 of the Canadian classification. These grades of chrysotile asbestos are generally classified as medium length fibre; they are used extensively in the manufacture of asbestos-cement pipes. One basic requirement for the asbestos is that it must be fully fiberized prior to mixing it with cement in order to obtain the best properties in the final product. It is also important to remove or minimize such impurities as dust and grit. The mixing of the asbestos and cement slurry is highly important in..the wet mechanical process, because the slurry must be distributed to form a thin film across the entire width of the machine. The open fibres from Kollergang are combined with the cement and mixed with water in a turbopulper fitted with rotors in order to open remaining clusters of fibres. The relatively heavy paste mixture in the turbo pulper is delivered to a stirring vat where it is pumped into overhead containers for delivery to pipe machine or recirculated to this mixer. It is important that agitation be constant and effective in order to prevent separation and settling of the solids in the slurry. The slurry flews to cylinder vats of pipe machine which are fitted with paddle agitators to prevent settling of the stock. There are two of these vats on the machine. Each vat contains a horizontal cylinder covered with a fine wire mesh screen and fitted with seals at its ends so that flow can occur out of the CAPCO KIN 0000503 -3- vat and only through the wire, thus leaving a thin, even film of stock deposited on its surface while removing the major part of the water. The thickness of the film depends on the slurry level in the vat, its consistency, and the speed of rotation of the cylinder. The machine is usually operated so that the film dfposited is approximately .002 to .010 inches thick. The continuous woven felt travels above these cylinders with its hairy side toward them; it is kept in firm uniform contact with them by heavy rubbercovered rolls. At the contact surface, the film of stock is transferred to the felt and some water is removed. Each cylinder adds its film thickness to the web of stock on the felt. Additional water is drawn from the web by means of a vacuum box placed under the felt as it travels toward the cast iron or steel mandrel. There is a vacuum box between the vats to seat the stock web firmly on the felt. As the web of stock passes under the mandrel, it is transferred to the mandrel in a continuous operation until the pipe is built up to the desired thickness. The water removed during this operation is returned to the mixing area of the machine. This water contains a small quantity of asbestos and cement from the stock that has passed through the screens and the felts. It is first retained for 'a period of time in settling tanks to clarify it. In addition, the water very rapidly becomes saturated with soluble materials from the Portland cement. This latter operation is generally beneficial because it eliminates further leaching of lime from the cement as the process continues. The solids separated from the water in the settling tanks are returned to the mixing cham bers separately from the clarified water. When the felt is returned toward the vats, it is cleaned by means of shower sprays and vacuum to remove any adhering stock particles. It is subjected to considerable strain and wear; usually it has an effective life of only six to twelve days. Similarly, it is necessary to prevent the cylinder screens from clogging. They are cleaned continuously during operation with a shower spray immediately after the film of stock has been released and before it is dipped into the vat for a new film. The process needs to be controlled closely. Attention to cleanliness is important; otherwise, there may be clogging of the cylinder screens and the felt, and an inferior product may result. The experimental manufacture of asbestos-cement pressure pipes was started in Italy in 1913. Progress was rapid, and by 1921 asbestos-cement pipes had been accepted in Europe. At that time, the British Ministry of Health approved the use of the pipe for watermains. They provided for loans for these pipes with a repayment period of thirty years; this period represented the same period allowed for cast iron pipes. CAPCO KIN 0000504 -4- This type of pipe gradually superseded both metal and ceramic piping in a large number of applications because of the fact that they are resistant to corrosion, impervious to and free from electrolytic action when buried in the earth, light-weight, elastic, strong, resistant to compression, economical to install, and unaffected by temperature changes. Tests have been conducted on pipes after thirty years in service with the conclusion that they had retained their original properties. These pipes have a smooth, glossy, cylindrical internal surface, and offer very low hydraulic frictional resistance to the flow of liquids. The Italit Mazza asbestos-cement pipes manufactured by Eternit, Genoa, Italy, are still in operation throughout the world. Their experimental data shows that the carrying capacity of pipe is on an average of 25 per cent greater than that of new cast iron pipes and 30 to 60 percent greater than that of old cast iron pipes, all being of the same in ternal diameter. Asbestos-cement pressure pipes are manufactured on costly and complex machines which are automatically operated by means of hydraulic and electrical controls. The pipes are built up of a continuous, uniformly thin and highly compressed film of asbestos-cement. The Mazza process is the most important commercial process used in the manufacture of pipes. The diameter of mandrels varies from three to fifty inches. Because of their weight, the larger diameter mandrels are more difficult to handle. These large mandrels are usually mounted in pairs, one attached to each side of the machine. The machine permits wrapping on one mandrel as the previously wrapped pipe is withdrawn from the other mandrel. CAPCO KIN 0000505 Cement Asbestos Pipe Company Asbestos Cement Pipe Manufacture CAPCO KIN 0000506 TABLE OF CONTENTS Subiect Summary I Mixing Plant A. Raw Materials B. Fiber Preparation C. Batch Weight D. Mixing E. Process Water F. Stock Feed to the Machine II Pipe Machine Operation A. Vats and Molds B. Bottom Felt and Vacuum Dewatering Boxes C. The Press D. Bottom Felt Cleaning Devices E.. Top Felt F. The Press Hydraulic System G. The Calender III Pipe Curing A. Pre-cure Oven B. Wet Room C. Autoclaving Pages 1-3 4 4 6 6 6 6 7 7 7-11 11 12 13 14 14 15 16 16 17 18 CAPCO KIN 0000507 SUMMARY Cement, silica flour, and asbestos fiber are batched by weight and mixed in water to form a slurry. This slurry is pumped into the two vats of the pipe machine, where two cyl inders covered with a fine mesh screen are mounted. Because the cylinder ends are sealed, the water pressure forces the slurry through the immersed screen, thereby depositing asbestos fibers - which in turn trap a cake of cement and silica flour. In a way closely analogous to pouring slurry into a bucket having only a wire screen for a bottom, the thickness of the film on the wire will vary with the pressure head, the consistency and viscosity of the slurry, time, the compressibility of the cake, and the number of fibers available to close the openings in the screen. Over the top of the cylinders passes a cloth belt made of a woven felted material containing wool and nylon. The felt is held tightly against the cylinder by weighted rolls so that the felt drives the cylinders as it moves. Because of water's surface tension the wet film is picked up by the smoother felt from the rough wire. After the felt picks up both stock films CAPCO KIN 0000508 2 to form a sheet, it passes over a suction box which partially dewaters the sheet prior to roll-up. The sheet is rolled up to the required pipe wall thickness on a metal pipe or mandrel in a press which consists of a large roll underneath and a pair of smaller, hydraulically loaded rolls above the mandrel. Between the mandrel and the upper press rolls is a second felt which prevents transfer of the sheet to the top rolls and which has voids in the weave for acceptance of water pressed from the pipe wall. After roll-up is completed, the felts are stopped, the upper press rolls are raised and the old mandrel is replaced by a new, bare mandrel for the next roll-up cycle. The newly formed pipe is then loosened from the mandrel, or calendered, by blowing compressed air under the pipe wall next to the mandrel and rolling to complete the loosening. Next the mandrel with pipe is conveyed through a heated tunnel where a combination of curing and drying hardens the pipe enough to permit stripping without damage. After stripping, the pipe are loaded by vacuum cups into a metal tray. In these trays the pipe are stored in a warm room where overhead spray showers return moisture lost in the pre-cure CAPCO KIN 0000509 3 tunnel. From the wet room the trays are transferred to auto claves for final curing. At approximately 350F the high pressure steam brings about an accelerated cure of the cement and causes unstable products of hydrated cement to combine with the free silica to form a strong bond around the reinforcing strands of asbestos. CAPCO KIN 0000510 4 I Mixing Plant A. Raw Materials 1. Cement a. Properties (1) Set time: The cement should be designed to set as rapidly as possible after roll-up in order to minimize mandrel inventory and wet-end handling damage. If the cement sets before roll-up, water retention increases, build-up occurs in the wet portion of the operation, and strength is lost. (2) Strength* The ultimate strength of the cement is affected by the chemical composition, the fineness of grind, k __ and the water retention. (3) Fineness of grind: While a finer grind improves early strength in concrete, the increase in water retention in the pipe wall associated with a fine grind may result in an overall weakening of the pipe. (4) Importance of uniformity: In order to produce pipe of consistent quality, it is mandatory that the cement properties remain constant. For a uniform cement, other manu facturing variables may be adjusted to give optimum results. 2. Silica flour (a) Chemical requirements: The silica should be in a pure crystalline form. (b) Physical properties: Chemical reactivity in- CAPCO KIN 0000511 5 creases with fineness, but at the expense of higher water re tention. 3. Asbestos Fiber (a) Chrysotile or white fiber: In general as fiber grade or length increases - strength increases, filtering time decreases, water retention is relatively constant, and bulk increases. As a particular grade is opened to a higher sur face area - strength increases moderately, filtering time decreases but with more water retained, and bulk increases moderately. _ (b) Crocidolite or blue fiber: For a given grade of blue fiber, additional opening results in - considerably in creased strength, reduced filtering time, considerably increased water retention, and a rapid increase in bulk. 4. Reclaimed scrap pipe (a) Method of preparation: After primary crushing the scrap is fed to a closed circuit consisting of a hamraermill and screen. Above the screen an air suction duct lifts the fine reclaim product while the oversize is returned to the hammermill. (b) Benefits: The reclaim reduces material costs and improves filtration by rendering the stock less compressable. (c) Limitations: The reduced compressability of the CAPCO KIN 0000512 6 stock results in lower pipe density. B. Fiber Preparation 1. Kollergang The Kollergang, which is an edge-runner, opens the crude bundles of fiber and mixes the blue and white fibers. A small amount of water is added to aid in opening the blue and to reduce dust. 2. Turbopulper The turbopulper has a horizontal shaft turning a pair of vertical discs having radial slots which open into curved scoops. When water and fiber are violently agitated in the pulpers, final mixing and opening is achieved. Fiber opening is a function of time and slurry viscosity. C. Batch weights Fiber and reclaim are weighed in a hopper on beam scales controlled by electric eye scanners at the scale head. At present, the cement and silica are weighed on belt scales but beam scales will replace them when delivered. D. Mixing The turbopulper serves to mix the entire batch into a slurry as well as to open the fiber. E. Process water Process water variables which influence pipe manu facturing are temperature, which influences cement set time CAPCO KIN 0000513 7 and filtering - and disolved minerals, which alter cement re actions. Process water is recirculated in a closed system in order to conserve water and to maintain stable water properties. To prevent too fast a set of the cement when starting up with fresh water, hydrated lime is added to raise process water alkalinity. F. Stock feed to the machine After each batch is mixed a pump transfers it to a holding chest containing a ribbon agitator. A small stock pump constantly pumps stock from the holding chest to a small stock chest. When a tapered plug in the small stock pump is raised, the stock flows to the machine; when lowered, the stock overflows back into the holding chest. In the piping to the machine, a tee mixes process water with the stock to dilute the slurry. This thinned slurry discharges into a mixing cone and overflows into three troughs to the vats. II Pipe Machine Operation A. Vats and molds In the bottom of both vats are two flat-bladed agitators which maintain the solids in suspension and aid in aligning fiber circumferentially around the molds - thereby giving the CAPCO KIN 0000514 8 hoop strength needed in pressure pipe. The paddles must turn fast enough to provide a uniform slurry consistency but not so fast that the film is swept from the mold wire. The mold is covered first with a spirally wound wire, next a ten mesh stainless wire cloth and finally a 30 or 40 mesh stainless face wire. The wire weave is normally "wrong way" which means the crimped wires run axially across the face. The 30 mesh screen provides a more rugged cover than the 40 mesh and the larger openings do not seem to affect strength adversely. i __ Variables which affect the thickness of the film on the cylinder wire are as follows: (1) The thickness of the film increases as the proportion of asbestos increases - first be cause without the asbestos the cement and silica would pour through the wire and second because the asbestos reduces the compressibility of the film, thereby leaving voids for the passage of more water. (2) The thickness increases for an increase in slurry temperature, since slurry viscosity drops rapidly as the temperature rises. (3) The thickness decreases as the consistency or CAPCO KIN 0000515 9 viscosity of the slurry increases. For a given blend the con sistency increases as the concentration of solids increases. For a given blend and concentration, the consistency increases as the asbestos surface area increases. (4) The thickness of the film increases with time, but at a decreasing rate. There are two times to consider: First, the time that a given part of the screen is under the slurry while the machine is running - an inverse function of felt speed; second, the time that the machine is stopped, a direct function of mandrel change time. _ Although the formation of the film on the mold gives the appearance of being elementary, the precentage, types, and degree of opening of the asbestos fibers charged into the vats is vital to the machine operation. The production rate of the machine may be determined by the rate of film pickup on the molds, but a high production rate is costly unless the fiber strength and opening is balanced with cement and silica pro perties to produce a sheet which the pipe machine felts, vacuums, and press can sucessfully convert into a sound pipe wall. In general, as asbestos fiber is progressively opened. QAPCO KIN 0000516 10 the strength increases, the filterability decreases, the bulk increases (thereby decreasing density), and the water retention increases. As compared to white fiber, the blue asbestos ex hibits a more rapid increase in strength but also a much higher water retention increase. As an aid to the agitators in maintaining uniform vats, an overflow system is in use. The flow over a weir to ward the front of the machine flows down a trough to a pump which returns it to the mixing cone at the rear of the machine. A high volume overflow may also aid in aligning fiber for greater hoop strength. Because of the mixing which takes place with the overflow in the cone, water may be allowed to flow into the machine during mandrel changes to replace the water lost from the vats through the molds. For some random alignment of fibers to increase flexual strength, a rake having long blades immersed in the slurry next to one of the molds is slowly oscillated. There is some question about the rake's effectiveness, but if it does promote flexual strength it should not be used for hydro pipe i.e., 10" or larger pipe, which requires no flexual strength test. The film width is controlled by applying an adhesive CAPCO KIN 0000517 11 or other coating to fill the face wire openings outside the desired film width - these coated areas are known as deckles and are 13'-2" apart. B. Bottom felt and vacuum de-watering boxes After the bottom felt passes over the first cylinder mold it passes under a vacuum slit box which pulls the stock into the felt and partially dewaters both the felt and the sheet before the second mold. After the second film is picked up, the two-layered sheet is carried back toward the front of the machine with the sheet still on the outside but now on the top,instead of the bottom of the felt loop. Sheet and felt are again dewatered while passing over a larger vacuum box pulling from 10 to 16 inches of mercury. The flow of air varies as the square root of the pressure difference across the felt - so that increasing the vacuum 50% only changes the air flow by 22% with other conditions constant. The moisture remaining in the sheet will vary as follows: The moisture decreases as fiber content increases, as temperature increases, and as the sheet thickness decreases; the moisture increases as a given content of fiber is opened, as cement and silica fineness increase, and as water contact time with the stock increases. CAPCO KIN 0000518 12 Also, affecting moisture release are the dust content of the fibers, the degree of hydration of the cement, and the design and cleanliness of the felt. There is a limit to what can be accomplished with higher vacuums because as the vacuum increases the accompanying increase in felt tension tends to reduce the felt weave openings. C. The Press The roll-up of the sheet on a mandrel is probably the most critical operation in pipe making - for at this point the thin, tender sheet must be compacted into a dense, thick mass to form the pipe wall. High densities and strength require low moisture content after roll-up, and it is the press which must reduce the moisture to an acceptable level. While in creasing the press roll loading will squeeze out more water, pressures cannot be increased beyond a point which causes the pipe wall to shift or tear. Once shifting or tearing occurs, the bond between the plies or between fiber and cement is permanently weakened. The factors limiting pressures are water content of the sheet, sheet thickness, drainage capacity of the felts, the lubricity or slipperiness of the stock, and the uniformity of CAPCO KIN 0000519 13 pressure across the mandrel. For a given pressure curve the moisture in the pipe wall will vary as follows: Moisture will decrease as temperature increases, as water contact time decreases, and as sheet thick ness decreases? moisture will increase with more opened fibers, with finer grind cement and silica and with faster setting cement. Blue fiber as compared to white permits the use of higher pressure but retains more water and reduces density. D. Bottom felt deeming devices . _ After leaving the bottom press roll, an inside, high volume shower floods the felt immediately before an inside worm roll. The left and right hand helixes on this roll knead and stretch the width of the felt and at the same time force shower water through the weave to flush out the imbedded stock. Next a face shower is directed 45 into the felt travel dir ection to wash the loosened stock away. The final shower is inside the felt at a right angle and again drives solids to the lowersface. Next a whipper turning against the felt travel strikes the felt with a series of sharp raps to jar away re maining solids - much like the action of a rug beater. CAPCO KIN 0000520 14 Finally, before reaching the first mold, the felt passes over a fan suction box which pulls out the soiled washing water. E. Top Felt The top felt transmits and cushions the press roll forces to the pipe wall. Since the press forces are spread over more pipe area than on the bottom felt, and since the sheet carrying job is reserved to the bottom felt - the physical wear and filling is far less a problem on the top felt. Consequently, cleaning on the top felt is limited to three worm rolls, a single intermittent spray shower, and a single slit vacuum box. The DC drive speed control permits the operator to set the top felt speed at a ratio greater than one to the bottom felt - this is termed overdrive. By using a slight amount of overdrive the top felt drive carries an increased share of the press power load and is thought to assist in rolling up a tighter pipe. F. The press hydraulic system At the present time, the two press rolls are moved up and down by hydraulic cylinders connected to the press roll bearing housings and guided by a pair of four parallelogram CAPCO KIN 0000521 15 linkages connected with two torque tubes. In order to com pensate for deflection in the center of the rolls, a pair of dolly rolls transmits force from two other cylinders. When a bare mandrel is loaded in the press, a closed center hydraulic valve shifts to move the outboard and dolly roll cylinders down against the press rolls to load the mandrel at a preset pressure. When the proper pressure is reached, the fill valve centers and the pipe machine is started. During roll-up the hydraulic circuit is isolated from any oil source. The pressure curve is controlled by a cam _ operated relief valve - which drains excess oil to sump as the cylinder pistons are pushed up by the increasing wall thick ness. Physically the press should impart smooth, uniform, and reproducible pressures across the pipe wall and should permit a rapid mandrel change. By keeping mandrel change times low the excess build up of stock on the molds during machine pauses will be minimized. This heavier mold pickup is termed a slug and may be positioned in the pipe wall by varying layer thickness and felt speed. G. The Calender At the calendering station, an air lance is inserted CAPCO KIN 0000522 16 between mandrel and pipe wall to open a gap across the pipe. By subsequent rolling the pipe is loosened around its cir cumference. Although a pressure roll is sometimes used on small pipe, over-opening may result. If the mandrel is too smooth, the compressed air cannot easily penetrate across the pipe. Accordingly, the mandrels are periodically sand or shot blasted to leave a textured surface. Every effort should be made to prevent over-opening, since an increase in pipe diameter weakens the bonds between _ fiber and cement. Resistance to over-opening increases with lower moisture content and with higher fiber level. The tendency to over-open increases as pipe diameter and wall thickness increase. Ill Pipe Curing A. Pre-cure Oven The purpose of the pre-cure oven is to harden the pipe enough to permit stripping the mandrel as quickly as possible for return to the pipe machine - thereby reducing mandrel inventory. The hardening can result from cure of the cement or from drying the pipe. Ideally, all the hardening should be derived from curing rather than drying, but in practice CAPCO KIN 0000523 17 drying predominates. When a pipe is rolled up in the press, some air is trapped in its wall, primarily between layers. As the pipe is rapidly heated, this blocked air expands more than the solid phase and causes the pipe to swell. As compaction or density decreases, the swelling increases rapidly and can greatly weaken the pipe. Wetting the newly rolled up pipe will also result in destructive swelling, but as the pipe is allowed longer curing times before wetting the damage decreases. In fact, after enough strength is obtained to prevent swelling, an increase in strength will result because of the additional water available for hydration. B. Wet Room Pipe is placed in the wet room after pre-cure in order to replace moisture lost through drying in the oven. This room is heated and sprinkled by overhead showers, which provides uniform cement hydration regardless of outside temperature and humidity. Regulating the minimum hold time in the wet room assures that pipe will be strong enough to withstand rapid autoclave heating. CAPCO KIN 0000524 18 C. Autoclaving There are two important advantages to an autoclave cure as compared to a normal cure. First, greater strength is reached by autoclaving for a day than by normal curing for a month. This greatly reduces in-process inventory and allows flexibility in scheduling production to meet shipments. Secondly, autoclaving imparts improved resistance to chemical attack in the ground by sulfate salts, aggressive C02, soft waters, and acid. At the high pressure and tem perature in the autoclave, calcium hydroxide - a vulnerable hydration product of cement - combines chemically with silica flour to form a stable calcium silicate hydrate called tobermorite. Properties which are not improved by autoclaving are permeability, brittleness, and stiffness. These undersirable tendencies may be minimized by holding curing temperature at approximately 350F, by an adequate pre-cure, and by avoiding too rapid an increase or decrease of pressure. The reactivity of silica increases rapidly as the particle size decreases and the strength falls sharply for particles coarser than 200 mesh (74 microns). For this CAPCO KIN 0000525 19 reason silica flour should be 98% passing 200 mesh - which would be equivalent to a 3500-4000 Blaine. Scientific studies indicate that the maximum strength will be obtained with a 70:30 or 65:35 ratio of cement to silica flour but a slightly higher proportion of silica may be used to reduce uncombined calcium hydroxide or to compensate for too low a water to cement ratio in the pipe wall. CAPCO KIN 0000526 Cement Asbestos Pipe Company Asbestos Cement Pipe Manufacture CAPCO KIN 0000527 TABLE OF CONTENTS Subject Summary I Mixing Plant A. Raw Materials B. Fiber Preparation C. Batch Weight D. Mixing E. Process Water F. Stock Feed to the Machine II Pipe Machine Operation A. Vats and Molds B. Bottom Felt and Vacuum Dewatering Boxes C. The press D. Bottom Felt Cleaning Devices E. Top Felt F. The Press Hydraulic System G. The Calender III Pipe Curing A. Pre-cure Oven B. Wet Room C. Autoclaving Pages 1-3 4 4 6 6 6 6 7 7 7-11 11 12 13 14 14 15 16 16 17 18 CAPCO KIN 0000528 SUMMARY Cement, silica flour, and asbestos fiber are batched by weight and mixed in water to form a slurry. This slurry is pumped into the two vats of the pipe machine, where two cyl inders covered with a fine mesh screen are mounted. Because the cylinder ends are sealed, the water pressure forces the slurry through the immersed screen, thereby depositing asbestos fibers - which in turn trap a cake of cement and silica flour. In a way closely analogous to pouring slurry into a bucket having only a wire screen for a bottom, the thickness of the -- film on the wire will vary with the pressure head, the consistency and viscosity of the slurry, time, the compressibility of the cake, and the number of fibers available to close the openings in the screen. Over the top of the cylinders passes a cloth belt made of a woven felted material containing wool and nylon. The felt is held tightly against the cylinder by weighted rolls so that the felt drives the cylinders as it moves. Because of water's surface tension the wet film is picked up by the smoother felt from the rough wire. After the felt picks up both stock films CAPCO KIN 0000529 ( 2 to form a sheet, it passes over a suction box which partially dewaters the sheet prior to roll-up. The sheet is rolled up to the required pipe wall thickness on a metal pipe or mandrel in a press which consists of a large roll underneath and a pair of smaller, hydraulically loaded rolls above the mandrel. Between the mandrel and the upper press rolls is a second felt which prevents transfer of the sheet to the top rolls and which has voids in the weave for acceptance of water pressed from the pipe wall. After roll-up is completed, the felts are stopped, the __ upper press rolls are raised and the old mandrel is replaced by a new, bare mandrel for the next roll-up cycle. The newly formed pipe is then loosened from the mandrel, or calendered, by blowing compressed air under the pipe wall i next to the mandrel and rolling to complete the loosening. Next the mandrel with pipe is conveyed through a heated tunnel where a combination of curing and drying hardens the pipe enough to permit stripping without damage. After stripping, the pipe are loaded by vacuum cups into a metal tray. In these trays the pipe are stored in a warm room where overhead spray showers return moisture lost in the pre-cure CAPCO KIN 0000530 3 tunnel. From the wet room the trays are transferred to auto claves for final curing. At approximately 350F the high pressure steam brings about an accelerated cure of the cement and causes unstable products of hydrated cement to combine with the free silica to form a strong bond around the reinforcing strands of asbestos. CAPCO 0000531 4 I Mixing Plant A. Raw Materials 1. Cement a. Properties (1) Set time: The cement should be designed to set as rapidly as possible after roll-up in order to minimize mandrel inventory and wet-end handling damage. If the cement sets before roll-up, water retention increases, build-up occurs in the wet portion of the operation, and strength is lost. (2) Strength* The ultimate strength of the cement is affected by the chemical composition, the fineness of grind, *_ and the water retention. (3) Fineness of grind: While a finer grind improves early strength in concrete, the increase in water retention in the pipe wall associated with a fine grind may result in an overall weakening of the pipe. (4) Importance of uniformity: In order to produce pipe of consistent quality, it is mandatory that the cement properties remain constant. For a uniform cement, other manu facturing variables may be adjusted to give optimum results. 2. Silica flour (a) Chemical requirements: The silica should be in a pure crystalline form. (b) Physical properties: Chemical reactivity in- CAPco KIN 0000532 5 creases with fineness, but at the expense of higher water re tention. 3. Asbestos Fiber (a) Chrysotile or white fiber: In general as fiber grade or length increases - strength increases, filtering time decreases, water retention is relatively constant, and bulk increases. As a particular grade is opened to a higher sur face area - strength increases moderately, filtering time decreases but with more water retained, and bulk increases moderately. (b) Crocidolite or blue fiber: For a given grade of blue fiber, additional opening results in - considerably in creased strength, reduced filtering time, considerably increased water retention, and a rapid increase in bulk. 4. Reclaimed scrap pipe (a) Method of preparation: After primary crushing the scrap is fed to a closed circuit consisting of a hammermill and screen. Above the screen an air suction duct lifts the fine reclaim product while the oversize is returned to the hammermill. (b) Benefits: The reclaim reduces material costs and improves filtration by rendering the stock less compressable. (c) Limitations: The reduced compressability of the CAPCO KIN 0000533 6 stock results in lower pipe density. B. Fiber Preparation 1. Kollergang The Kollergang, which is an edge-runner, opens the crude bundles of fiber and mixes the blue and white fibers. A small amount of water is added to aid in opening the blue and to reduce dust. 2. Turbopulper The turbopulper has a horizontal shaft turning a pair of vertical discs having radial slots which open into curved scoops. When water and fiber are violently agitated in the pulpers, final mixing and opening is achieved. Fiber opening is a function of time and slurry viscosity. C. Batch weights Fiber and reclaim are weighed in a hopper on beam scales controlled by electric eye scanners at the scale head. At present, the cement and silica are weighed on belt scales but beam scales will replace them when delivered. D. Mixing The turbopulper serves to mix the entire batch into a slurry as well as to open the fiber. E. Process water Process water variables which influence pipe manu facturing are temperature, which influences cement set time CAPCO KIN 0000534 7 and filtering - and disolved minerals, which alter cement re actions. Process water is recirculated in a closed system in order to conserve water and to maintain stable water properties. To prevent too fast a set of the cement when starting up with fresh water, hydrated lime is added to raise process water alkalinity. F. Stock feed to the machine After each batch is mixed a pump transfers it to a holding chest containing a ribbon agitator. A small stock pump constantly pumps stock from the holding chest to a small stoc k c_hest. When a tapered plug in the small stock pump is raised, the stock flows to the machine; when lowered, the stock overflows back into the holding chest. In the piping to the machine, a tee mixes process water with the stock to dilute the slurry. This thinned slurry discharges into a mixing cone and overflows into three troughs to the vats. II Pipe Machine Operation A. Vats and molds In the bottom of both vats are two flat-bladed agitators which maintain the solids in suspension and aid in aligning fiber circumferentially around the molds - thereby giving the CAPCO KIN 0000535 8 hoop strength needed in pressure pipe. The paddles must turn fast enough to provide a uniform slurry consistency but not so fast that the film is swept from the mold wire. The mold is covered first with a spirally wound wire, next a ten mesh stainless wire cloth and finally a 30 or 40 mesh stainless face wire. The wire weave is normally "wrong way" which means the crimped wires run axially across the face. The 30 mesh screen provides a more rugged cover than the 40 mesh and the larger openings do not seem to affect strength adversely. Variables which affect the thickness of the film on the cylinder wire are as follows: (1) The thickness of the film increases as the proportion of asbestos increases - first be cause without the asbestos the cement and silica would pour through the wire and second because the asbestos reduces the compressibility of the film, thereby leaving voids for the passage of more water. (2) The thickness increases for an increase in slurry temperature, since slurry viscosity drops rapidly as the temperature rises. (3) The thickness decreases as the consistency or CAPCO KIN 0000536 9 viscosity of the slurry increases. For a given blend the con sistency increases as the concentration of solids increases. For a given blend and concentration, the consistency increases as the asbestos surface area increases. (4) The thickness of the film increases with time, but at a decreasing rate. There are two times to consider: First, the time that a given part of the screen is under the slurry while the machine is running - an inverse function of felt speed; second, the time that the machine is stopped, a direct function of mandrel change time. -- Although the formation of the film on the mold gives the appearance of being elementary, the precentage, types, and degree of opening of the asbestos fibers charged into the vats is vital to the machine operation. The production rate of the machine may be determined by the rate of film pickup on the molds, but a high production rate is costly unless the fiber strength and opening is balanced with cement and silica pro perties to produce a sheet which the pipe machine felts, vacuums, and press can sucessfully convert into a sound pipe wall. In general, as asbestos fiber is progressively opened. CAPCO KIN 0000537 10 the strength increases, the filterability decreases, the bulk increases (thereby decreasing density), and the water retention increases. As compared to white fiber, the blue asbestos ex hibits a more rapid increase in strength but also a much higher water retention increase. As an aid to the agitators in maintaining uniform vats, an overflow system is in use. The flow over a weir to ward the front of the machine flows down a trough to a pump which returns it to the mixing cone at the rear of the machine. A high volume overflow may also aid in aligning fiber for greater hoop strength. Because of the mixing which takes place with the overflow in the cone, water may be allowed to flow into the machine during mandrel changes to replace the water lost from the vats through the molds. For some random alignment of fibers to increase flexual strength, a rake having long blades immersed in the slurry next to one of the molds is slowly oscillated. There is some question about the rake's effectiveness, but if it does promote flexual strength it should not be used for hydro pipe i.e., 10" or larger pipe, which requires no flexual strength test. The film width is controlled by applying an adhesive CAPCO KIN 0000538 11 or other coating to fill the face wire openings outside the desired film width - these coated areas are known as deckles and are 13*-2" apart. B. Bottom felt and vacuum de-watering boxes After the bottom felt passes over the first cylinder mold it passes under a vacuum slit box which pulls the stock into the felt and partially dewaters both the felt and the sheet before the second mold. After the second film is picked up, the two-layered sheet is carried back toward the front of the machine with the sheet still on the outside but now on the top,instead of the bottom of the felt loop. Sheet and felt are again dewatered while passing over a larger vacuum box pulling from 10 to 16 inches of mercury. The flow of air varies as the square root of the pressure difference across the felt - so that increasing the vacuum 50% only changes the air flow by 22% with other conditions constant. The moisture remaining in the sheet will vary as follows: The moisture decreases as fiber content increases, as temperature increases, and as the sheet thickness decreases; the moisture increases as a given content of fiber is opened, as cement and silica fineness increase, and as water contact time with the stock increases. CAPCO KIN 0000539 12 Also, affecting moisture release are the dust content of the fibers, the degree of hydration of the cement, and the design and cleanliness of the felt. There is a limit to what can be accomplished with higher vacuums because as the vacuum increases the accompanying increase in felt tension tends to reduce the felt weave openings. C. The Press The roll-up of the sheet on a mandrel is probably the most critical operation in pipe making - for at this point the thin, tender sheet must be compacted into a dense, thick mass to form the pipe wall. High densities and strength require k ____ low moisture content after roll-up, and it is the press which must reduce the moisture to an acceptable level. While in creasing the press roll loading will squeeze out more water, pressures cannot be increased beyond a point which causes the pipe wall to shift or tear. Once shifting or tearing occurs, the bond between the plies or between fiber and cement is permanently weakened. The factors limiting pressures are water content of the sheet, sheet thickness, drainage capacity of the felts, the lubricity or slipperiness of the stock, and the uniformity of CAPCO KIN 0000540 13 pressure across the mandrel. For a given pressure curve the moisture in the pipe wall will vary as follows: Moisture will decrease as temperature increases, as water contact time decreases, and as sheet thick ness decreases; moisture will increase with more opened fibers, with finer grind cement and silica and with faster setting cement. Blue fiber as compared to white permits the use of higher pressure but retains more water and reduces density. D. Bottom felt cleaning devices After leaving the bottom press roll, an inside, high volume shower floods the felt immediately before an inside worm roll. The left and right hand helixes on this roll knead and stretch the width of the felt and at the same time force shower water through the weave to flush out the imbedded stock. Next a face shower is directed 45 into the felt travel dir ection to wash the loosened stock away. The final shower is inside the felt at a right angle and again drives solids to the lower:'face. Next a whipper turning against the felt travel strikes the felt with a series of sharp raps to jar away re maining solids - much like the action of a rug beater. CAPCO KIN 0000541 14 Finally, before reaching the first mold, the felt passes over a fan suction box which pulls out the soiled washing water. E. Top Felt The top felt transmits and cushions the press roll forces to the pipe wall. Since the press forces are spread over more pipe area than on the bottom felt, and since the sheet carrying job is reserved to the bottom felt - the physical wear and filling is far less a problem on the top felt. Consequently, cleaning on the top felt is limited to three worm rolls, a single intermittent spray shower, and a single slit vacuum box. The DC drive speed control permits the operator to set the top felt speed at a ratio greater than one to the bottom felt - this is termed overdrive. By using a slight amount of overdrive the top felt drive carries an increased share of the press power load and is thought to assist in rolling up a tighter pipe. F. The press hydraulic system At the present time, the two press rolls are moved up and down by hydraulic cylinders connected to the press roll bearing housings and guided by a pair of four parallelogram CAPCO KIN 0000542 15 linkages connected with two torque tubes. In order to com pensate for deflection in the center of the rolls, a pair of dolly rolls transmits force from two other cylinders. When a bare mandrel is loaded in the press, a closed center hydraulic valve shifts to move the outboard and dolly roll cylinders down against the press rolls to load the mandrel at a preset pressure. When the proper pressure is reached, the fill valve centers and the pipe machine is started. During roll-up the hydraulic circuit is isolated from any oil source. The pressure curve is controlled by a cam -operated relief valve - which drains excess oil to sump as the cylinder pistons are pushed up by the increasing wall thick ness. Physically the press should impart smooth, uniform, and reproducible pressures across the pipe wall and should permit a rapid mandrel change. By keeping mandrel change times low the excess build up of stock on the molds during machine pauses will be minimized. This heavier mold pickup is termed a slug and may be positioned in the pipe wall by varying layer thickness and felt speed. G. The Calender At the calendering station, am air lance is inserted CAPCO KIN 0000543 16 between mandrel and pipe wall to open a gap across the pipe. By subsequent rolling the pipe is loosened around its cir cumference. Although a pressure roll is sometimes used on small pipe, over-opening may result. If the mandrel is too smooth, the compressed air cannot easily penetrate across the pipe. Accordingly, the mandrels are periodically sand or shot blasted to leave a textured surface. Every effort should be made to prevent over-opening, since an increase in pipe diameter weakens the bonds between _ fiber and cement. Resistance to over-opening increases with lower moisture content and with higher fiber level. The tendency to over-open increases as pipe diameter and wall thickness increase. Ill Pipe Curing A. Pre-cure Oven The purpose of the pre-cure oven is to harden the pipe enough to permit stripping the mandrel as quickly as possible for return to the pipe machine - thereby reducing mandrel inventory. The hardening can result from cure of the cement or from drying the pipe. Ideally, all the hardening should be derived from curing rather them drying, but in practice CAPCO KIN 0000544 17 drying predominates. When a pipe is rolled up in the press, some air is trapped in its wall, primarily between layers. As the pipe is rapidly heated, this blocked air expands more than the solid phase and causes the pipe to swell. As compaction or density decreases, the swelling increases rapidly and can greatly weaken the pipe. Wetting the newly rolled up pipe will also result in destructive swelling, but as the pipe is allowed longer curing times before wetting the damage decreases. In fact, afte'r enough strength is obtained to prevent swelling, an increase in strength will result because of the additional water available for hydration. B. Wet Room Pipe is placed in the wet room after pre-cure in order to replace moisture lost through drying in the oven. This room is heated and sprinkled by overhead showers, which provides uniform cement hydration regardless of outside temperature and humidity. Regulating the minimum hold time in the wet room assures that pipe will be strong enough to withstand rapid autoclave heating. CAPCO KIN 0000545 18 C. Autoclaving There axe two important advantages to an autoclave cure as compared to a normal cure. First, greater strength is reached by autoclaving for a day than by normal curing for a month. This greatly reduces in-process inventory and allows flexibility in scheduling production to meet shipments. Secondly, autoclaving imparts improved resistance to chemical attack in the ground by sulfate salts, aggressive C02, soft waters, and acid. At the high pressure and tem perature in the autoclave, calcium hydroxide - a vulnerable hydration product of cement - combines chemically with silica >_ flour to form a stable calcium silicate hydrate called tobermorite. Properties which are not improved by autoclaving are permeability, brittleness, and stiffness. These undersirable tendencies may be minimized by holding curing temperature at approximately 350F, by am adequate pre-cure, and by avoiding too rapid an increase or decrease of pressure. The reactivity of silica increases rapidly as the particle size decreases and the strength falls sharply for particles coarser than 200 mesh (74 microns). For this CAPCO KIN 0000546 - 19 reason silica flour should be 98% passing 200 mesh - which would be equivalent to a 3500-4000 Blaine. Scientific studies indicate that the maximum strength will be obtained with a 70:30 or 65:35 ratio of cement to silica flour but a slightly higher proportion of silica may be used to reduce uncombined calcium hydroxide or to compensate for too low a water to cement ratio in the pipe wall. CAPCO KIN 0000547 BARON WHITAKER. PRESIDENT DONAL BRETING. VICE PRES- LABEL SERVICE W. A. FARQUHAR. VICE PRES. ELECTRICAL NORMAN H. DAVIS. JR. Assistant Vice President 2t7 C. onto ST 3 2 J PFINGSTEN ROAD CHICAGO. ILL 60611 NORTmOROOK ILL. 60062 FOUNDED t894 ]for m>icr - aot forprofif SPONSORED BY Amrrtran titsuraurp Assnriation K. S. GEIGES. Senior Vice President E. N. DAVIS. Vice Pres. Fire Protection W. s. AUSTIN. Vice pres, and secretary T. F. RAMSEY. JR.. TREASURER 1265 WALT WHITMAN ROAO 1t>5S SCOTT BLVD MELVILLE. L l , N.Y. 11746 SANTA CLARA. CALIF 95050 Pile Ex2456 Assignment 66K1715 June 17, 1966 REPORT on PIPE AND COUPLINGS - ASBESTOS CEMENT Cement-Asbestos Products Co. Ragland, Alabama CAPCO KIN 0000549 Pile Ex2456 Page 1 Issued: 6-17-66 PRODUCT COVERED: DESCRIPTION Asbestos-cement pressure pipe and couplings in 4 to 12-in. sizes, inclusive, 150-psi pressure class. The pipe is 13 ft in length. Service connections in 3/4-in. size for use with pipe sizes 4 to 10 in-,, inclusive, 150-psi pressure class. GENERAL CHARACTER: The asbestos-cement pressure pipe and couplings covered by this Report are manufactured from a mixture of asbestos fibers, Portland cement, and silica flour. A description of the method of fabrication is given in a latter section of this Report. Construction features of the pipe couplings and ring gaskets are shown by Pig. 1. , _The design of the pipe and couplings will permit slight angular deflection at the joints so that a pipe line may belaid in curves of large radii. USE: The pipe and couplings covered by this Report are intended for use in underground water service where the working pressure does not exceed that for which it is rated and when installed in accordance with the manufac turer's installation instructions. MARKING: Pipe - Each length of pipe is marked as follows: 1. Manufacturer's trade name - "Cement-Asbestos Products Co." 2. Nominal inside diameter, pressure class. 3. Test pressure "T-350 PSI" for Class 100 and "T-525 PSI" for Class 150. CAPCO KIN 0000550 Pile Ex2456 Page 2 Issued: 6-17"66 4. Date and shift of manufacturer. 5. Underwriters1 Laboratories, Inc. label reading: UNDERWRITERS' LABORATORIES, INC. LISTED NONMETALLIC PIPE FOR WATER MAINS Couplings - Each coupling is stenciled with the following marking 1. Manufacturer's trade name - "Cement-Asbestos Products Co." 2. Nominal inside diameter, pressure class. 3. Test pressure "T-350 FSI" for Class 100 and "T-525 PSI" for Class 150. Rubber Sealing Rings - Each ring is marked with the following information molded into it. /y 1. Ring manufacturer's mark, " ." 2. Year of manufacture (may be indicated by a code letter). 3. The size and pressure class for which its use is intended. TRANSPORTATION AND INSTALLATION OP PIPE: TRANSPORTATION Pipe is normally loaded on skids, secured by steel straps, and transported in flat-bodied trucks, or railroad cars. CAPC0 KIN 0000551 Pile Ex2456 Page 3 Issued: 6-17-66 UNLOADING Unloading is by hand or with the aid of ropes. Skids and hoisting equipment are employed for excessive drops and larger sizes. DISTRIBUTION After unloading, the pipe is distributed along the trench site, leaving the couplings and rubber rings in a central storage point until used, in such a manner as to protect the rubber from exposure to sun. The pipe and cou plings may also be delivered assembled with one gasket in place. TRENCHING AND LAYING The trench is dug to allow proper clearances for working space at the sides of the pipe and for coupling clearance under the pipe. ._ ASSEMBLY OP "PERMAFLEX" The parts forming the joint are the pipe ends, a coupling, and two rubber sealing rings. Before making the joint, the pipe ends, rubber rings, and interior of the couplings are thoroughly cleaned. - 1. The rubber sealing rings are fitted inside the coupling in the gasket recesses. The outside surface of the pipe is lubricated with a hydrogenated vegetableoil lubricant.2 2. Tine coupling is then placed over the last pipe laid, and pulled on the pipe until stopped by a shoulderon the pipe. In those cases where the pipe is delivered with the coupling and one gasket in place, the other gasket is inserted and the plain end of the next pipe is assembled into the coupling. CAPCO KIN 0000552 Pile Ex2456 Page 4 Issued: 6-17-66 3. The new pipe length to be laid is then brought up so that it is in alignment. The pipe is pulled into the coupling until the shoulder of the pipe comes in contact with the sealing ring. In the larger sizes, it may be necessary to aid the assembly of pipe and couplings by using a steel bar as a lever, pushed into the ground and acting against a wooden block inserted between the steel bar and the pipe or coupling. A jack and chain may also be used. In some in stances the pipe can be pushed by hand. 4. After the joint is made, deviations in align ment can be adjusted and slight angular deflections may be made by lifting and moving the end of the last laid pipe. 5. Disassembly can be accomplished by lifting the end of the pipe or moving it from side to side and at the same time pulling the pipe from the coupling. Capck,n 0005s3 CAPCO KIN 0000555 EX 2456 FIG. 3 RESTRADED JOINT TEST LINES Pile Ex2456 Page Tl-1 Issued: 6-17-66 TEST RECORD NO. 1 SAMPLES: Representative production samples of asbestoscement pipe and couplings in sizes and types covered by this Report were used in the following tests, except as noted. EXAMINATION OF PIPE AND COUPLINGS: METHOD The sample pine, couplings, and rubber rings were examined to check the dimensions and design features against the manufacturers drawings and manufacturing tolerances. The production methods and facilities at the manufacturer's plants were reviewed to develop information regarding the uniformity of production and the inspection program followed in production. *- RESULTS The dimensions of the pipe and couplings examined were found to be within the tolerances established by the manufacturer. The manufacturing procedures followed and the manufacturer's inspection and test program are conducive to the production of uniform pipe and couplings, and the elimination of products not measuring up to the shop standard. BURSTING TESTS: METHOD Individual lengths of pipe were installed in the plant hydrostatic test machines. See Pig. 2A. The assembly was filled with water, vented of air, and subjected to gradually increasing pressures until a value of four times the rated pressure was obtained. This was held for 5 sec, whereupon the pressure was increased until the pipe burst or until the maximum of the apparatus was attained. CAPCO KIN 0000557 Pile Ex2456 Page Tl-2 Issued: 6-17-66 RESULTS The results of these tests are recorded in the following table. The pressures at which the pipe burst were, in all cases, in excess of requirements. Pipe Size, In. Pressure Class Bursting Pressure PSI 4 4 ........ 6 6 8 8 10 10 12 . _ 12 150 150 150 150 150 150 150 150 150 150 980 t 1000 t 905 950 740 730 810 810 670 700 t - These samples did not burst maximum of test apparatus. Hydrostatic test samples are required to sustain a pressure of at least four times the rated pressure or 5 sec. PTEXURE TEST: METHOD Two full-length samples of the 4, 6, and 8-in. size pipe were placed on "V" block load supports in a tension and compression testing machine and loaded at the third points. See Pig. 2B. Each sample was loaded at a uniform rate until failure occurred. Note was made of the maximum load applied and the character of the failure. CAPCO KIN 0000558 File Ex2456 Page Tl-3 Issued: 6-17-66 RESULTS The following table presents the results of these tests in comparison with the minimum flexure load requirements. Pipe Size, In. Pipe Length, Ft Test Load Span, Span, Pressure Ft Ft Class Required Minimum Load, Lb Load at Failure Lb 4 13 12 4 150 4 13 12 4 150 6 13 12 4 150 6 13 12 4 150 8 13 12 4 150 8 13 12 4 150 1000 1000 2800 2800 5700 5700 1330 1410 3110 2990 6140 6060 RING CRUSHING TESTS: SAMPLES Unmachined samples, 12 in. long, of each size pipe were selected from production stock for these tests. METHOD Each ring was placed in a Horizontal position be tween wooden-block cearings in a tension and compression testing machine and loaded to failure. See Fig. 2C. Obser vations were made to note the maximum load. RESULTS The following table presents the results of these tests in comparison with the required minimum crushing load. Pipe Size, ____In. Pressure Class Required Minimum Load, Lb Actual Load, Lb 4 150 5400 9720 4 150 5400 9130 6 150 5400 7890 6 150 5400 7300 CAPCO KIN 0000559 File Ex2456 Page Tl-4 Issued: 6-17-66 (Table Cont'd) Pipe Size, In. Pressure Class . Required Minimum Load, Lb Actual Load, Lb 8 150 5500 9130 8 150 5500 9300 10 150 7000 7030 10 150 7000 7090 12 150 7600 8380 12 150 7600 9350 HYDROSTATIC TESTS OF COUPLINGS: SAMPLES Samples of each size of coupling were used in these tests. METHOD >_ Samples of each size of coupling were installed in the plant coupling tester and subjected to a hydrostatic proof test of four times the rated pressure for 5 sec, where upon the pressure was increased to burst the coupling. RESULTS The couplings burst at the pressure indicated in the following table. Pipe Size, In. Pressure Class Bursting Pressure, _________PSI ______ 4 150 900 4 150 930 6 150 900 6 150 900 8 150 790 8 150 870 10 150 820 10 150 770 12 150 730 12 150 630 CAPCO KIN 0000560 me EX2456 Page Tl-5 Issued: 6-17-66 SERVICE CONNECTION (CORPORATION STOP) TESTS: At least two full-length samples each of pipe sizes 4 to 10 in., inclusive, in the 150-psi pressure class, were used. Three-quarter-inch service connections were also used. METHOD Each pipe sample was cut in two, one-half placed aside as a control sample and the other half was drilled and tapped for attachment of a 3/4-in. service connection. The service connection was attached following the manufac turer's installation instructions. Each sample including the control samples, was subjected to a pressure of four times the rated pressure for 5 sec. The pressure was then increased until the pipe burst. RESULTS The results of this test are recorded in the following table: Pipe Size, In. __________ Sample Maximum Pressure, PSI Remarks 4 A, control 4 A, with connection 4 B, control 4 B, with connection 4 Cj control 4 c. with connection 6 A, control 6 A, with connection 6 B, control 6 B, with connection 6 c. control 6 c. with connection 900 620 950 890 970 770 1000 630 950 770 950 750 Pipe burst Pipe cracked across stop Maximum of apparatus Pipe cracked across stop Maximum of apparatus Pipe cracked across stop Maximum of apparatus Pipe cracked across stop Maximum of apparatus Pipe cracked across stop Maximum of apparatus Pipe cracked across stop CAPCO KIN 0000561 Pile Ex2456 Page Tl-6 Issued: 6-17-66 (Table Cont'd) Pipe Size, In. Sample Maximum Pressure, PSI Remarks 8 A, control 8 A, with connection 8 B, control 8 B, with connection 10 A, control 10 A, with connection 10 B, control 10 B, with connection 10 c. control 10 c. with connection 750 Pipe burst at end connection 700 Pipe cracked across stop 700 Pipe cracked at end 655 Pipe cracked across stop 730 Pipe burst 675 Pipe cracked across stop 620 Pipe burst 600 Burst at 6 sec 610 Pipe burst 610 Pipe cracked across stop ASSEMBLY AND DISASSEMBLY TESTS: SAMPLES Samples of the S-in. Class 150 and 12-in. Class 150 pipe and couplings specially machined to the minimum cou pling and-maximum pipe dimensions permitted by the manufac turer's tolerances were used in these tests. METHOD The spigot ends of the pipe were given a coating of lubricant and the couplings were provided with the sealing ring and spacer gaskets. After the pipe and couplings were aligned, the assembly was made, following the manufacturer's installation instructions. RESULTS The assembly of two lengths of pipe and one coupling was accomplished with reasonable ease in all sizes. Dis assembly of the pipe was also accomplished without undue difficulty. Examination of the disassembled samples showed no damage to the pipe, coupling, or gaskets. CAPCO KIN 0000562 File Ex2456 Page Tl-7 Issued: 6-17-66 RESTRAINED JOINT TESTS: SAMPLES Full-length samples of the 8-in. Class 150, and 12-in. Class 150 pipe with couplings of like sizes and classes were used in these tests. Some of the pipes were machined to the minimum dimensions permitted by the manufacturer's tolerances, while some of the couplings were machined to the maximum dimensions, and these were used to form the joints. METHOD Test lines of the pipe and couplings, together with rubber-ring gaskets consisting of four joints and' five lengths of pipe were assembled in accordance with the manu facturer's installation instructions. The joints were de flected as shown in the test record. The pipeline was filled with water, vented of air, and subjected to increas ing pressures in 50-psi increments up to twice the maximum rated pressure. Each increment of pressure was maintained until the_Laboratories engineer was satisfied as to the equi librium of the joint. Each test line was cycled twice in this manner from 0 to 300 psi to 0. Following this, the pressure was increased until failure occurred. The test assembly is shown by Figs. 3A and 3B. RESULTS In the tests with the assembled line of pipe and couplings, no leakage occurred at a pressure of twice the rated pressure of the test line. Specific test data are shown in the following table. Pipe Size, In. Pres sure Class Maximum Joint Maximum Deflection, Pressure, Deg PSI Remarks 8 150 12 150 5.42 5.33 550 End cap leaked at maxi mum pressure 390 End pipe began moving and fourth coupling broke CAPCO KIN 0000563 Pile Ex2456 Page Tl-8 Issued: 6-17-66 PHYSICAL TESTS OF SEALING RINGS: METHOD Representative samples of the gaskets were subjected to an accelerated oxygen pressure aging test for 96 hr in an oxygen bomb having a temperature of 70 C with oxygen at a pressure of 300 psi. The tensile strength and elongation of the samples were determined before and after the aging period. The hardness was measured before aging with a Shore-Type A durometer hardness gauge which has a scale graduated from 0 to 100. Two-inch gauge marks were stretched to 6 in., held for 2 min, then released and measured 2 min later. RESULTS Before After Aging Aging Per Cent of Original Average Tensile Strength, PSI 259^- Average Elongation, Per Cent 455 Hardness Sample recovered to 2.10 in. 55 2031 355 78 78 FACTORY METHODS: The factory of Cement-Asbestos Products Co. was visited by a representative of Underwriters' Laboratories, Inc. for the purpose of obtaining general information re garding the manufacture of asbestos-cement pipe and couplings covered by this Report and detailed information relative to the features of factory equipment and inspection that have a bearing on the quality of materials employed, character of the workmanship, the uniformity of the finished product, and practicability of handling and shipping the pipe and couplings. The following information covers briefly the manufacture of asbestos-cement pressure pipe and couplings. CAPCO KIN 0000564 Pile Ex2456 Page Tl-9 Issued: 6-1J-66 Manufacturing Process - These asbestos-cement pipe and couplings are manufactured by the Mazza Process from an initimate mixture of asbestos fiber, Portland cement * and silica flour. A mixture of asbestos fiber, cement, silica flour, and water is conveyed to a vat provided with a hollow rotating cylinder, sheathed with a fine-metal gauze. A thin uniform layer of the mixture adheres to the sheath, and is transferred to an endless belt of felt equipped with two suction chambers to draw off excess water. The film of asbestos cement, approximately 0.005 in. thick then passes over a polished-steel mandrel onto which the required thickness is built up. While winding the pipe, a pressure is exerted on the mandrel to insure a homogenous compact product. Coupling stock is made in the same manner as the pipe, but is built up to a greater thickness for a given size. After forming to the required size, the mandrel is immediately removed and the pipe is passed through a precured oven of steam for approximately 1-1/2 hr. The mandrel is then removed and the pipe is stored for at least 8 hr in a moist atmosphere. The pipe is then given a final cure by autoclave with steam at 115 psi for 16 hr. After curing, the pipe is cut to the proper length and the ends machined to accommodate the couplings. Coupling stock is cut and machined to proper dimensions before auto claving. Each finished pipe and coupling is subjected to a hydrostatic test of three and one-half times rated pressure and each pipe in the 4, 6, and 8-in. size is given a flexural test at the proof test loads specified in the Laboratories 1 requirements. Automatic recorders on the pipe and coupling hydrostatic testers and on the pipe flexural tester record each test for review by quality-control personnel. MRS CAPCO KIN 0000565 Pile Ex2456 Page Cl Issued: 6-17-66 CONCLUSIONS The following conclusions apply to the pipe and couplings covered by this Report when used in public and private water-work systems and connections to such systems, for the rated working pressures of the pipe and couplings (150 psi). PRACTICABILITY: The pipe and couplings can be properly handled and installed under conditions ordinarily met in service by those reasonably familiar with the installation of asbestoscement pipe. STRENGTH: The pipe, couplings, and service connections covered by this Report, when installed according to the methods advocated, are capable of withstanding the working pressures for which they are designed and the stresses to which they are likely to be subjected in service. These pipe and couplings meet the strength require ments, as evidenced by the results of the bursting test, ring crushing tests, restrained joint test, and flexural tests. The service connection features meet the strength requirements as evidenced by the results of the service connection tests. UNIFORMITY: The facilities and methods employed in the manu facture of the pipe and couplings covered by this Report are such as to insure an accurate and uniform product. Examination of the pipe and couplings show that a high degree of uniformity is maintained in the manufacture of this product. The manufacturer maintains a rigid in spection program to insure uniformity of the product within established manufacturing procedures. CAPCO KIN 0000566 File Ex2456 Page C2 Issued: 6-17-66 CONFORMITY: The pipe and couplings covered by this Report are in conformance with the requirements of the Laboratories1 Outline of Proposed Investigation for Asbestos-Cement VJater Pipe and Couplings (Subject 107). FOLLOW-UP SERVICE: The asbestos-cement pipe and couplings covered by this Report will be placed under the Label Service. Report by: t / Reviewed by: MILES R. SUCEOMEL Project Engineer Fire Protection Department xs. E. AUCK Associate Managing Engineer Fire Protection Department k ____ MRS:pe CAPCO KIN 0000567 UNDERWRITERS' LABORATORIES, INC. CHICAGO NORTHBROOK, ILL. - MELVILLE, N.Y. SANTA CLARA. CALIF. an independent, not-for-profit organization testingfor public safety File Ex2 56 Assignment 60HK328A December 2, 1968 REPORT on ASBESTOS -CEMENT PIPE AND COUPLINGS Cement-Asbestos Products Co. Ragland, Alabama CAPCO KIN 0000569 File Ex2456 Page 1 Issued: 12-2-68 DESCRIPTION PRODUCT COVERED: Asbestos-cement pressure pipe and couplings in 4-l4 in. sizes, pressure Class 200 and 14 and 16 in. sizes, pressure Class 150. The pipe is 13 ft in length. GENERAL CHARACTER: The asbestos-cement pressure pipe and couplings covered by this Report are manufactured from a mixture of asbestos fibers, Portland-cement, and silica flour. The design of the pipe and couplings will permit slight angular deflection at the joints so that a pipe line may be laid in curves of large radii. USE: ` The pipe and couplings covered by this Report are intended for use in underground water service where the working pressure does not exceed that for which it is rated and when installed in accordance with the manufacturers installation instructions. MARKING: Pipe - Each length of pipe is marked as follows: 1. Manufacturer's trade name - "Cement-Asbestos Products Co." 2. Nominal inside diameter, pressure class. 3. Test pressure "T-700 PSI" for Class 200 and "T-525 PSI" for Class 150. 4. Date and shift of manufacture. 5. Underwriters' Laboratories, Inc.- label reading: UNDERWRITERS' LABORATORIES, INC. LISTED NONMETALLIC PIPE FOR WATER MAINS CAPCO KIN 0000570 Pile Ex2^56 Page 2 Issued: 12-2-68 Couplings - Each coupling is stenciled with the following marking. 1. Manufacturer's trade name - nCement-Asbestos Products Co." 2. Nominal inside diameter, pressure class. 3. Test pressure "T-700 PSI" for Class 200 and "T-525 PSI" for Class 150. CAPCO KIN 0000571 File Ex2456 Page Tl-1 Issued: 12-2-68 TEST RECORD NO. 1 SAMPLES: Representative production samples of asbestos-cement pipe and couplings in sizes and types covered by this Report were used in the following tests, except where noted. EXAMINATION OF PIPE AND COUPLINGS: METHOD The sample pipe, couplings, and rubber rings were examined to check the dimensions and design features against the manufacturer's drawings and manufacturing tolerances. The production methods and facilities at the manufacturer's plants were reviewed to develop information regarding the uniformity of production and the inspection program followed in production. ._ RESULTS The dimensions of the pipe and couplings examined were found to be within the tolerances established by the manufacturer. The manufacturing procedures followed and the manufacturer's inspection and test program are conducive to the production of uniform pipe and couplings, and the elimination of products not measuring up to the shop standard. HYDROSTATIC TESTS OF PIPE AND COUPLINGS: METHOD Individual lengths of pipe and coupling were installed in a hydrostatic test machine. The assembly was filled with water vented of air, and subjected to a gradually increasing pressure up to a value of four times the rated pressure (600 psi for Class 150 and/or 800 psi for Class 200). This pressure was maintained for 5 sec, whereupon it was increased until either failure occurred or the capacity of the test apparatus was reached. RESULTS The results of these tests are recorded in the following tabulations: CAPCO KIN 0000572 File Ex2456 Page Tl-2 Issued: 12-2-68 HYDROSTATIC TEST RESULTS Size, In. 4 4 6 6 8 8 10 10 12 12 14 14 16 16 Pressure Class Pressure At Burst Or Maximum Pressure PSI "T>ipe Coupling Reauired Pressure PSI Pipe Coupling 200 200 200 200 200 200 200 200 . 200 200 150 150 150 150 930 1000 1000 t 1000 t 1000 910 940 875 875 840 t 725 650 640 665 1000 t 1000 t 1000 t 1000 t 960 860 960 t 1060 t 960 t 1010 t 600 600 960 t 960 t 800 800 824 840 800 800 838 874 833 . 773 635 629 600 600 800 800 800 800 83? 784 800 800 859 801 600 600 600 647 t - No burst limit of apparatus. FLEXURE TESTS: METHOD Two full lengths of the 4, 6 and 8 in. sizes, were placed on supports 12 ft apart. The load was applied by the manufacturer's production testing machine at a uniform rate at the third.points, 4 ft apart and located 4 ft from the lower supports. Each sample was loaded in this manner until failure occurred and note was made of the maximum load applied and the character of the failure. RESULTS The following table presents the results of these tests in comparison with the minimum flexure-load requirement for a 12 ft span. CAPCO KIN 0000573 File Ex2456 Page Tl-3 Issued: 12-2-68 FLEXURE TEST RESULTS Pipe Size Pressure In. Class Minimum Required Load, Lb______ Maximum Load Obtained Lb 4 200 4 200 6 200 6 200 8 200 8 - 200 1400 1400 3700 3700 7600 7600 1410 1410 3700 3700 7640 7600 RING CRUSHING TESTS: SAMPLES The 12 in. samples were cut from each size pipe used in these tests. METHOD ' Each ring was placed on two lower bearings consisting of two straight wooden strips having their interior top edges rounded to a radius of approximately 1/2 in. Load was applied by an upper bearing of a straight wood block. The load was applied until failure occurred and note was made of the maximum load at failure. RESULTS The following table presents the results of these in comparison with the minimum required crushing load. Pipe Size Pressure Minimum Required In. Class Load, Lb Maximum Load Obtained Lb 4 4 6 6 8. 8 10 10 12 12 200 200 200 200 200 200 200 200 200 200 8700 8700 9000 9000 9300 9300 11000 '11000 11800 11800 9220 10800 12950 12950 11590 . 12750 12850 13350 15950 16150 CAPCO KIN 0000574 File Ex2456 Page Tl-4 Issued: 12-2-68 (Table Cont'd) Pipe Size In. Pressure Minimum Required Class Load, Lb Maximum Load Obtained Lb 14 200 14 200 16 200 16 200 14 150 14 . 150 16 150 16 150 13500 13500 15400 15400 8600 8600 9200 9200 15900 15700 18860 18700 9430 11400 11590 11690 ASSEMBLY AND DISASSEMBLY TESTS: SAMPLES Samples of the 16 in. Class 200 pipe and couplings specially machined to the minimum coupling and maximum pipe dimensions permitted by the manufacturer's tolerances were in thesd tests. METHOD The spigot ends of the pipe were given a coating of lubricant and the couplings were provided with the sealing ring and spacer gaskets. After the pipe and couplings were aligned, the assembly was made, following the manufacturer's installation instructions. RESULTS The assembly of two lengths of pipe and one coupling was accomplished with reasonable ease in all sizes. Disassembly of the pipe was also accomplished without undue difficulty. Examination of the disassembled samples showed no damage to the pipe, coupling, or gaskets. CAPCO KIN 0000575 File Ex2456 Page Tl-5 Issued: 12-2-68 RESTRAINED JOINT TESTS: SAMPLES Full length samples of the 12 in. Class 200, and 16 in. Class 150, and 16 in. Class 200 pipe with couplings of like sizes and classes were used in these tests. Some of the pipes were machined to the minimum dimensions permitted by the manufacturer's tolerances, while some of the couplings were machined to the maximum dimensions, and these were used to form the joints. METHOD The pipe and couplings, together with rubber ring gaskets were assembled in accordance with the manufacturer's installation instructions. Some of the joints were deflected as shown in the test record. The pipeline was filled with water, vented of air, and subjected to increasing pressure. Each increment of pressure was maintained until the Laboratories engineer was satisfied as to the equilibrium of the joint. Each test-line was cycled three times in this manner from 0 to twice the rated pressure to 0. Following this, the pressure was increased until failure occurred. Four separate tests were conducted on the 16 in. Class 200 pipe and couplings. RESULTS In- the tests with the assembled line of pipe and couplings, no leakage occurred at a pressure of twice the rated pressure of the test line. Specific test data are shown in the following table. Pipe Size In. Maximum Joint Pressure Deflection ClassDeg Maximum Pressure, _________ PSIRemarks 12 200 5 16 150 0 16 200 4 16 200 0 600 No failure - no leaks 450 No failure - no leaks 450 Chain holding pipe broke 600 No failure - no leaks (three separate tests) WAW CAPCO KIN 0000576 Pile Ex2456 Page Cl Issued: 12-2-68 CONCLUSION The product covered by this Report has been found to comply with the requirements covering the class and is judged to be acceptable for listing under the Label Service of Underwriters' Laboratories, Inc. Report by: Jh. i.JfoU' W. A. WEBB Project Engineer, Fire Protection Department Reviewed by: R. MILES R. SUCHOMEL Senior Project Engineer Fire Protection Department WAW:JA CAPCO KIN 0000577 CAPCO KIN 0000579 Every Good SAFETY RECORD is a CHALLENGE for a BETTER ONE CAPCO KIN 0000580 PREFACE These rules are made primarily for the purpose of promoting the safety of the employees of the Cement Asbestos Products Company, and the Company ex pects each and every employee not only to observe and obey the rules himself but to do all in his power to prevent their violation by others, as the carelessness of one employee is very apt to result in injury not only to himself but to others as well. A violation of any of the rules will subject the of fender to disciplinary action. The method of discipline will be left to the local management Every violation, no matter how slight should be noted and steps taken to prevent a repetition. Every employee in and around the plant is urgently requested to report any dangerous condition which he may see to the foreman. CEMENT ASBESTOS PRODUCTS COMPANY CEMENT ASBESTOS PRODUCTS COMPANY PLANT SAFETY RULES August 1, 1965 The Safety Rules in this book apply to all em ployees in and around the plant and copies of these rules may be obtained from the superintendent's office. The following rules and regulations are printed for your benefit, see that you obey them, and take nec essary steps to see that your fellow workmen know and are obeying these rules. To know the rules of the department reflects your interest in your work, and to comply with the rules means you are an asset to the company. Never take anything for granted, it is your duty to see conditions for yourself. Your own safety and that of your fellow workmen will be endangered by guess work. Your pride should make your work look neat; your interest in safety should make a safe job. Strict compliance with the rules of this book shall be the first duty of each employee at all times. Vigilance and watchfulness promote safety. To avoid danger, adopt the safe course. Employees must not trust to the care exercised by another when their own safety is involved. __ _ GENERAL RULES 1. Each employee shall know all the special rules covering his work, all the general rules, and should always report to the foreman any unsafe condition or practice he thinks may cause accidents. 2. If in doubt as to the meaning of any rules, an employee shall apply to his foreman for explanation. 3. Employees are forbidden to take short cuts over dangerous places. You must not leave your work to go 1 CAPCO KIN 0000581 to other parts of the plant except upon Company gerous weapons, intoxicating liquor, or possession of business. illegal goods of any kind. 4. Do not ride on any burden being carried by a 13. Injuries, including those of a minor nature, crane. must be reported to your foreman before the shift is 5. No one is allowed to operate any machinery, completed. unless duly authorized by the proper authority. 14. Wrestling, throwing of material, or "horseplay" 6. All gears, sprockets, saws, belts, etc., and all projections on revolving shafts, such as set screws, keys, couplings, bolts, oil cups, etc., shall be properly * of any kind, is positively prohibited. Fighting in, or around the plant property and buildings thereon is strictly prohibited. guarded. Any employee removing any guard or safety 15. Be ever watchful of loads carried by cranes or device from any mechanical equipment for any reason suspended in the air, and keep out from under them. shall see that such guard or safety device is replaced, before the machine is put in operation. . 16. Removing or replacing electric light bulb or socket with the current on is prohibited. 7. Never work on any electrically driven ma chinery until the control switch has first been locked in the off position and the operator notified. 17. Do not play with compressed air, never blow the air on anyone. It may enter the body and injure or cause death. The working on air lines while the pres 8. Do not turn on any electricity, gas, steam, air sure is on is prohibited. or water, or set in motion any machinery, or throw 18. It shall be a violation of the rules to sleep down any material without first seeing if any one is in while on duty in or about the plant. position to be injured. 19. Goggles shall be worn when grinding, cutting, 9. All persons not authorized by the Electrician welding, or striking where particles may fly, including are forbidden to work upon any electrical apparatus. You are warned against touching wires of any kind, as employees exposed to possible eye injury as a result of work being performed by other employes. it may result in death. Before doing any work where 20. Oiling, greasing of machinery, or cleaning of there is danger of coming in contact with electric belts or conveyors while in motion is not permitted, wires, notify the Electrician, who will advise concern except where protection is provided against moving ing the work. Do not try to fix electric lights, but call T parts. your foreman or electrician. 21. Loose clothing must not be worn by em 10. Hand tools must be kept in good condition, ployees who are required to work around moving mushroomed heads, or other dangerous conditions of , machinery. drills, hammers, cutters, and other tools will not be 22. Empty soft drink bottles must be placed in permitted. racks provided. Lunch papers, paper cups, etc., must 11. All work must be done in a neat and orderly be placed in trash cans. manner. No repair or construction job will be con 23. When products are being loaded or unloaded sidered complete until all refuse and excess material from railway cars, workmen shall see to it that car has been stored in its proper place. brakes are properly setup and car or cars well secured 12. No employee shall bring upon the plant prop to prevent movement. erty, or in or around any building thereon, any dan- 24. Respirators and goggles must be worn by each 23 CAPCO KIN 0000582 employee when the particular circumstances make either of them needed. 25. Additional protective apparel or equipment re quired for the personal protection of any employee exposed to a special hazard by reason of a special occupation or work shall be worn or used by the em ployee subjected to such hazard. 26. Oil and grease kept in the plant shall be in substantial covered metal containers. 27. Employees shall use care in placing ladders before using them. If there is danger of the ladder slipping, have someone hold it. Do not use an unsafe or make-shift ladder. 28. Do not go up or down a ladder without the free use of both hands. If material is to be handled, use a rope. Do not reach more than an arms length from ladder. 29. All scaffolds, whether swinging or otherwise, when higher than six (6) feet above the ground shall be provided with railings of substantial strength. Floor boards of scaffold must be fastened to prevent slipping. 30. Employees removing the cover from any open ing in the floor, ground, valve pit, or sewer, must take steps to guard that opening so no one will fall into it. 31. Any employee reporting to work under the influence of intoxicating liquor will be discharged. 32. Employees performing work under elevated equipment or machinery, etc., must have the same securely blocked in addition to lifting jacks, hydraulic systems, chain blocks, etc. 33. Employees are forbidden to run on the job except to protect himself or others from personal injury. 34. Riding on the running boards or on the outside of fork trucks is prohibited. 35. Employees shall use a brush to clean metal shavings frqpi drill presses and lathes and the cement asbestos shavings from machines and machine tools. 4 36. Supplies and material should be stored in bins and racks in such a manner that it will not obstruct aisleways. 37. Storing of supplies and material in walkways, aisleways, and on stairs is prohibited. 38. Work benches and the front of work benches shall be kept free of excess material and oils. 39. When there is any doubt as to the best and safest method of doing work, and when instructions are not complete or thoroughly understood, the fore man must be consulted and his direction followed. LATHE OPERATORS A lathe is not an especially dangerous machine, but it must be intelligently operated if accidents are to be prevented. 1. Wear eye protection, guard against flying chips. 2. Do not hand brake the machine. 3. Do not caliper or gauge the job while machine is in motion. 4. Do not leave chuck wrench in chuck. 5. Do not wear loose clothing. 6. Do not leave machine running unattended. 7. Use a hooked rod for handling chips. 8. Use file with protected tang. 9. Use stick to hold emery cloth against work. 10. Keep the work area dean around the machine. GRINDING WHEELS 1. When grinding, eye protection must be used in addition to eye shield mounted on grinder. 2. Work rest must be adjusted to within %" of wheel. 3. Do not grind on side of wheel. 4. Do not use gloves when grinding small work. 5. Report grinder defects to your foreman. 5 CAPCO KIN 0000583 DRILL PRESS 1. Be sure the work is securely clamped. 2. Wear eye protection if work is throwing off chips. 3. Do not wear loose clothing that could be caught in revolving parts. 4. Keep the work area dean and dear of stum bling hazards. 5. Do not leave machine running unattended. 6. Report any machine defects to your foreman. TOOLS Because of the widespread use of hand and power tools and the severity of many tool injuries, it is im portant that control of tool accidents be made a part of every safety program. 1. Workmen are expected to select the right tool for the job. 2. Tools must be kept in good condition. 3. Tools must be used in the right way. 4. Tools must be kept in a safe place. 5. Do not use a wrench for a hammer, pliers for a wrench. 6. Do not use tools with split or broken handles or mushroomed chisels. 7. Do not carry tools or lav tools down where they may fall on someone. 8. Report defective tools to your foreman. ELECTRIC WELDING 1. Be sure the work setup is such that the work is grounded. Exercise care or the welder or operator can easily become grounded. 2. Do not dip hot electrodes in water. 3. Never change electrodes with bare hands or wet glove^ or_when standing on wet floors or grounded surfaces. 6 4. Report any defects in the welding equipment to your foreman. 5. Welding cables and cutting hose must be neatly stored with machines when not in use. BURNING AND CUTTING 1. Shut off gas at the pressure-reducing regulators before changing torches, do not crimp hose. 2. If welding or cutting is stopped for sometime (lunch or overnight) dose oxygen and acetylene cyl inder valves, then open torch valves to relieve gas pressure from hose and regulator. 3. Do not use matches to light torches. 4. Point torch away from others when lighting. 5. Never put torch down until the gases have been completely shut off. 6. Do not hang lighted torch over regulators. 7. When burning or cutting in an area containing combustible or flammable material, fire extinguishers or their equivalent must be readily available. 8. Keep hose wound around regulators or cart when not in use. Protect hose when in use from falling sparks. OXYGEN AND ACETYLENE 1. Oxygen and acetylene cylinders should be kept in an upright position and secured against accidently being knocked over. Empties must be returned to storage area and replaced with full one. 2. Never use oil or grease as a lubricant on valves or attachments of oxygen cylinders. Keep oxygen cyl inders and fittings away from oil and grease, and do not handle such cylinders or apparatus with oily hands, gloves, or clothing. 3. Never use oxygen as a substitute for com pressed air in pneumatic tools, in oil preheated burn ers, to start internal combustion engines, or to blow 7 CAPCO KIN 0000584 out fuel lines. Oxygen under presseure will explode when in contact with oils or grease. POWER TRUCKS AND FORK LIFTS 1. Operators must give proper signal when turn ing. 2. Slow down at intersections and doorways. 3. Look in direction of travel and obey all signs. 4. Do not travel with load too high. 5. Report defective equipment to your foreman. 6. Do not ride on fork trucks. No one but the operator is permitted to ride. 7. Do not run over loose material on floor such as cables, hose, boards, and other obstacles. We believe we should all be proud of our plant, and we think most of us are. The management wants the plant kept neat and clean and orderly, as attrac tive and comfortable a place to work in as possible. Management cannot do the entire job. Unless we all help, we're up against a tough proposition. Sure, the other fellow can do his best, but if we fail to do our part, the job will not be done. Let's each one of us keep our own job in order, thus maintaining a clean safe plant and safeguarding our future. No. I hereby acknowledge receipt of a copy of the Cement Asbestos Products Company Safety Rules for CAPCO Plant. As a condition of my employment, I agree to study and learn these rules and to abide by all of them. To be careful to protect myself and fellow workmen from injury. Name Badge No__________________________________________ Occupation Witness Date, 19 CAPCO KIN 0000585 CAPCO KIN 0000586