Document Jr7OVqYYpa2K0yRr248bDdVMZ

1 COATINGS AS BARRIERS TO PREVENT POLYCHLORINATED BIPHENYL CONTAMINATION OP SILAGE1'2 2 L. B. Willett, Department of Dairy Science 3 Ohio Agricultural Research and Development Center, Wooster 44691 4 5 ABSTRACT 6 l'n past years polychlorinated biphenyls (PCB's) v.-ere incorporated 7 into a coating material used on the inside of many concrete silos. These 8 residues subsequently diffuse into silages and ultimately pass into food 9 products produced by livestock that consume the PCB contaminated silage. 10 Twelve coating materials were evaluated to determine if they would form a 11 barrier to PCB residues. Coating materials were evaluated by coating PCB 12 contaminated stave blocks, on test sections in a contaminated silo and on 13 dairy farm silos that were contaminated. All coatings were not evaluated 14 at all the test locations. 15 When PCB centmi.rated surfaces were treated with various barrier coat- 16 iegs and exposed to silage, 9 of the 12 coatings significantly (P<.05) re- 1 17 '.'.'' T.d the concentration of Aroclor 1254 in silage compared to silage adja- 13 c.;.a`. to control !;- faces. Significant differences in the effectiveness of ,7 >. ; <n-j i.v torials as barriers were also noted. Those coatings that wore 70 carried by water or a solvent in which Aroclor 1254 is not readily i.oluMo, 21 vac .rv.ojig the most effective coatings. Coating materials with a base coat 22 designed to seal the surface prior to application of the surface coating 23 ~ ..... ........ 1 Approved as Journal Article no. /5*J-7jP Ohio Agricultural Research 34 -nd Development Center# Wooster 44691. . 5. 25 ` Suppox tod in part by USDA-AKS Cooperative Agreement no. 12-14-1001--234. DSW 038278 STLCOPCB4022102 2- - 1 were more' effective than two applications of a single formulation. Hydrau 2 lic cement with an acrylic bonder and water-carried epoxy effectively re 3 duced the PCD residues in silage from contaminated dairy farm silos. The 4 resulting concentrations of PCB in the milk from co s d these silages 5 were below the Pood and Drug Administration "temporary tolerance" level. 6 INTRODUCTION 7 Many silos in the Eastern half of the United states have been treated 8 with a coating material that contains polychlorinated biphenyl (PCB) resi 9 dues. These residues appear in the silage as a result of disbdged chips 10 from the contaminated coating and/or the PCB's from the coating being dis n solved by the silage juices (14). This contamination process has continued u ; any years (more than 16 years observed) after the coating was applied 13 ;...i long after all visible traces of coating were gone (1.8), H Tie coating responsible for most, if not all the PCB contaminated 15 silos vas called Cu-.iar . Cumar was formulated in 1941 and was used by 16 several silo companies until 1970. This material contained a mixture of 17 cour;irone-indene resins, a chlorinated rubber, clay, the PCB Arcelor 12,,4 13 . (" .':;.7ito Industrial Chemical Co.,St. Louis, Mo. 63.166), the polychlori \) nated terphenyl (PCY) Aroclor 5460 (Monsanto) and carrier solvents. Simi) h.r fo'.mulntions have been shown to provide excellent protection of concrete /I '-r.. nets (17). Whereas the Aroclors wore rot specifically manufactured for 77 .!neo>poration into coatings (9), their plasticising properties made their 73 ace -.d /.anhageous (6, 11), The Aroclors compr ised about 42% of the cured 74 ^ The Av.'-lor containing si lo <a>nt *ng called "Ce.mar" should not be 75 e-,nf used v. :.h > l J o It-l-GA rosfn th b has 1 he same name. DSW O^8279 STLCOPCB4022103 -3- I Cumar coating. *' 2 Consumption of silage from a PCB contaminated silo, by dairy cattle, 3 i.Y:suits in the deposition of PCB residues in the body adipose tissues and 4 secretion into milk via the fat (4, 6, 7). PCB residues in milk are now 5 considered a chemical adulterant, therefore, the Food and Drug Administra 6 tion in 1970 recommended an "actionable level" for milk at 5 ppm on a fat 7 basis (8). A "temporary tolerance" of 2.5 ppm was established in 1973 (2). 0 The dairyman that has a PCB contaminated silo is confronted with a two 9 fold economic hazards lost income from unmarketable milk and either elimi 10 nation of the residue from the silo structure or lost use of the silo. n Therefore, a research effort was undertaken to evaluate coating materials 12 and systems of application that might be used as a barrier i>reventing fur 13 ther contamination of the silage with PCB's, The principle objective was 14 to offer the dairyman a low cost alternative to the replacement of the silo 15 structure. A preliminary report has been made (19). : 16 I V.TllODS AND MATERIALS ! 17 The coating materials were evaluated on PCB contaminated stave blocks, : J i.'-ist sections in a contaminated silo, and applied to existing silos on , . ;V 'stern Ohio dairy farms. Twelve coatings wore evaluated, however, :) 1 I. .<<> i:ot .luo1 led in all of the trials. Coat! -.'gy v.bich ''demonstrated 21 ; or oi.vr j.-iyo or* wore an ineffective barrier to the PCB residues were 22 eliminated from subsequent trials. New coatings, with similar properties 23 .vi coatings that formed good barriers,'were incorporated into subsequent 24 ! '.i el o. . 25 Coat i t<> ' als. The coding ,.v tcrials, their x>rinciple components OSW 038280 STLCOPCB4022104 1 jj'.d location of testing are shown in Table 1. The coatings that were evalu 2 ated in these studies, with the exception of VII and XIII, were selected 3 on the basis of properties which were hypothesised to form an adequate bar . 4 rier to PCB residues and resist the corrosive action of silage juices. . 5 Those hypotheses were based on the formulation of the coatings and their 1 6 performance when used in other applications. All were either commercially available or currently under development for application to silos. Coatings 7 8 VII and XIII did not contain the properties thought to be necessary for a ' 9 good barrier to I'CB's, but since these had been recommended for use on farm 10. silos they were included in the trials. All coatings were applied to the 11 tr.st surfaces in two coats, however, with coatings I, IV,V, and IX each appli- 12 t lx. a !v.d a different formulation. With these materials, the first coat 13 '.as fji j minted for penetration and sealing of the surface while the second 14 .vp plica Lion was to provide the desired surface. Coating XI was the combi IS nation of a single coat of an organ`o .co.1.vent-ca:o ii.d epoxy nd a r.u;o IS application of a vter~cavxled epoxy* 17 Two cumar-Aroclor coatings were used for .the stave block trials. In ij ' - \ trial 1 the finished cumar coating contained 5$ Aroclor 1254. For i) J V-.k s *.lal 7 some of idle actual Cxnrtar silo coat!t>g was obtained. This :) id coating contained about 32$ Aroclor 1254. . 21 !5ilo tost sections. A silo,3,on x 15.4 m that was built and coated 22 wi th an Aroclor 1254 containing coating in 1954,,was used. Rock fill, to a 23 fa pth of 1; 22 m was placed in the bottom to p. oo-nt i pfiirfeccnce f.i.o. i VOO 24 residues that r.ay have acc'mulated in the dirt floor. The silo was then 25 divided h-fo .seven 1.22 . ,2.44 m i;< L sections which were separated by qSW 038281 t i f i ; | j I STLCOPCB4022105 I'lG. -5- 1 Masonite dividers (Fig. 1). Chips of Masonite analyzed for PCD residues were 2 found to contain .012 ppm. Since this concentration is nearly the came as 3 the lowest levels found in silage, they would not significantly influence con 4 centrations in the silage. The test sections, with the exception of a con 5 trol, were wire brushed to prepare a sound sur.Caco for coating application. 6 Costings were applied at random to five sections. The test coatings were 7 used to seal the junctions between the Masonite and the silo wall. 8 The silo was filled three times so that after each filling the settled 9 si lego level was oven with the top of the sections. .Two fi llings chop 10 ped corn and one a chopped grass-legume mixture. Sections were vertically 11 c.moled four months after each filling at 0, 60, 120, 180 and 240 cm from ; ' a hose and horizontally at 0, 35, 20, 60, and 90 cm from the wall. r> 13 Str.ve block trials. Two trials were conducted on concrete silo stave blocks. In' these (rials the stave blocks (30 x 70 cm) were treated on one U 15 side with a enme.v-vco.clor coating, thou the entice block was reccet-l with 16 the barrier coatings. The blocks need in trial l varo very porous and the 1/ cunar coating contained 5% Aroclor 1254, whereas the blocks in trial 2 were 13 smooth surfaced and treated with 32^ Aroclor 1254. Untreated blocks and c\i' ar-Aroclor blocks were maintained as controls. 19 .0 The blocks '..' re picc-d m c rtd and at one side of polyethylene i * red 21 :.'.'8,2 .1, drums which wore then f U.lr.d with chopped whole corn plant and 'll c.-aled. After standing for four months, they wore campled every 25 cm 7'i .dong the block and at 0, 25 and 45 cm from the block. 24 Dairy r,. ,.i . *i 1 os. Two i; i1 os in *:o on MortV Ohio d.* i r y f , s, 2'j which vi.) ' i r. i 1 o he PCi (;<)!:!' i'. .ted, vino nl Cor field lists of OSW 038282 STLCOPCB4022106 -G- 1 two coating materials. Samples of .* lo wall scrapings, silage and milk from 2 the bulk tanks wore analyzed to verify the existence of PCB residues. 3 The first silo was built in 1957 and coated with tin; PCB containing 4 Cumar at that time. In 1972, this silo was cleaned by wire brush prior to 5 application of two coats of hydraulic cement plus an acrylic bonder (coating 6 VIII). This silo was subsequently filled once with a chopped grass-legume 7 mixture and then once with chopped corn. The second silo was built in 1954 8 and treated with a 1'CB containing coating. In 1563 the pit and lower 2.44 m 9 of this silo ware treated with a furfuryl alcohol resin coating (coat *ng I.). 10 in 1972, this silo was cleaned with high pressure water (51 kg/sq cm) and 11 coated from the base of the pit to 11.3 m above ground level with water- 12 carried epoxy (coating VI). The silo was filled once with chopped legumes .3 cud o.fter emptying was refilled with corn silage. 14 yilngo samples were collected from the farm silos at least biweekly, 15 here fj.V:1 ji.--. it sampling occurred wh in the dairymen hr. d to enter the silo to 16 adjust the meek t'cal. unlcrdcvs. Well sample ooiscintod of a corw osito of 17 ullage collected adjacent to U.o t.v..l.l from the north, south, cast and west i 4 s-ces of the silo. 17 Fxt. reel ion of silage. All solvents used to extract silage rrmpius A) . m wH-ilyi teal .reagent grvdo. These were glass '-ofyihllod bor.oj o until a volume equivalent to the qruikity used for extraction would yield V 72 i.o inter fori jyj peeks when injected into ; lio gas li quid chromatog raph (*'i-C) 7.3 after being .reduced lo 1 ml and 6 ]il wore injected. 24 fti.1v.go sampleg \:;ycc meek w .lee-1 ly chopped until i he !.'-`.t. i< 1 on v; y i:>i about l r.m in sixe. Vy.eid.y - >' i vo g v;ero < > . n :; ir-v;l ed with 250 ml DSW 038283 STLCOPCB4022107 -7- V 1 acetone by mechanical shaking for 15 h. The particulate matter was then 2 .separated by filtering through Whatman No. 1 filter paper {prewashed with 3 w,ter, methanol and acetone) or glass wool. The acetone extract was taken A up in 500 ml of 2% Na2S04 and vigorously extracted with 200 then 150 nl 5 petroleum ether (PE) (boiling range 30 to 60 C). The aqueous phase \:as 6 discarded and the P)2 washed with 100 ml of 2% Nalico^. The PE was concen 7 trated to about 10 ini on a rotary evaporator. 8 Column hromatqgraphy. Organic solvent extracts can be freed from 9 interfering pigments (13) and many pesticides by florisil (.12) and/or silica 10 gc-1 columns (1, 16). Columns to clean the jPE extracts were prepared by ] i placing 6.0 cm (7,5 g) of activated florisil (Kensington, 650 C activation, 12 'YAOO mesh) in the bottom of a 23 mm column fitted with glass wool in the 13 Horn. On top of this was placed 14.0 cm (26 g) of silica gel (Matheron, 14 tv Iw'.un & 'lei3.r grade 923) and 2.5 cm (12 g) of anhydrous Na2S0^. Ool'un 15 p,-eking materials vero stored in an oven at 110 c until used. Vh-> pi < pared 16 columns v.ero pravr-rshod with ICO ml of PE, the extracts were applied and 1/ they were eluted with 250 ml of v>? -scene in PE. The volume of the column 13 ell.ales was reduced in vacuo oh the rotary evaporator (42 c) in prepa- i') /.al icn for GI.C analysis. Care was taken to avoid cent: e'nation of the .) . by reflux during rotary evapor..! ion. 21 Kaponifixation and acid extraction. Selected extracts were saponified :-2 with alcoholic KOII (2.5% w/v) and extracted with H^SO^. (16 normal) by i he 23 method described by Monsanto (10) .-aid modified as follows. Moth nol w.-u 24 used to prepare the alcoholic OH end PE was us>d for o-itri-.o lions, The 25 :}ootrd extracts were refluxed fo.c 45 min in 25 ml of eb ohol.ic KOI1 then ` DSW 038284 STLCOPCB4022108 T l FIG. -8- 1 extracted 2 tiroes with 25 ml of PE. The combined extracts were then ex 2 tracted with 25 ml of H^SO^. The PE extracts were rechromatographed as pre 3 viously described. 4 Gas chromatography. An FfiM model 402 GLC with a Ni detector was used 5 for all analyses. A 2.44 m glass column of 4% DC-200 and 6% QF-1 (1:1) on 6 Gas-Chrom Q (80/100 mesh) was used with Argon-Methane (95:5) as carrier and t, 7 purge. Running conditions were: flash heater 230 C, column oven 210 c, 8 detector 300 C and gas flow 40 to 50 ml/min. All samples were diluted so 9 that they were detected within: one linear attenuation range of the detector. 10 Quantitations. Quantiation of the chromatograms was based on total 11 area under peak F thro1 ugh peak M (Fig. 2). Area was de; termined by Disc inte12 yrator. This quantitation method was used to eliminate the influence of on 13 vni.dontifiedcontaminant with a short retention time, which appeared in some 14 silage samples, i 15 Corrections for method loss.were based on the extraction of silage to 16 v.-hich known quantities of Aroclor 3 254 were added. The so standards ranged 17 from 0 to 2 ppm. Recoveries did not vary significantly among the various l 18 types of silage. . 19 Dry matter doterfn!nation. The water content of the silages were vari 20 able, therefore, the concentrations of Aroclor were expressed on a dry 2] matter basis. Silage dry matters were determined by weight loss of samples 22 oven dried for 48 h at 110 C. 23 Data Analyses. The data from the three silo trials were analyzed by 24 Least-Squares Analysis of Variance (LSANOV) as a split-split plot model. 25 The variables of this model were the Aroclor levels in silage as influenced DSW 038285 STLCOPCB4022109 -91 by tlio five coating treatments pins the untreated cont rol section; the hori 2 zontal and vertical sample collection positions; and the three silo fillings 3 The FOB values in the silage were highly variable among the various sampling 4 locations. Therefore, the data was transformed to the Log (ppm Aroclor) + 1 5 prior to analysis. Similar I.SANOV analyses were conducted for the two block 6 trials without transformation of the data. 7 Hartley's Sequential Range Test (15) was used to test for significant 8 differences among treatment means. 9 INSULTS AND DISCUSSION 10 Relative peak areas for standard Aroclor 1254 were essentially the same 11 an the Aroclor extracted from silage. Typical CLC tracings of silage ex 1C. 3 12 tracted and standard Aroclor are shown in Fig. 3. Results indicated that 13 he microorganisms or juices in the silage did not alter or selectively ex 14 tract the Aroclor components. These findings are confirmed by the work of 15 Fries (6) and Skrontny et al. (14). Since there appeared to bo no appreci 16 able alteration of the f-roclor by the silage, and saponification plus ac.i.d 17 -.traction did not alter the rolo.tionsh.ip between the major peaks, the 13 total area under peak F through peak M was considered a valid quantitation i? .fhod. >0 M.tempts to detect the Fee's that were also a cc.iporont of the Ce- .r 21 silo coating wore not made. Even though they wore probably extracted by 22 l.ho procedures that wore ysed, the I'CT's wore not eluted at the maximum 23 ti-opnr./itnros of the liquid phase of the GLC column (5). 24 The average ppm of Aroclor .1254 in silage from the three silo 1 rials 25 .and two block trials are shown in Fig. 3. Each bar of the histograms re- OSW 038286 STLCOPCB4022110 1 procants the average Aroclor 3 254 concentration of all .samples analyzed re- 2 presenting all sampling locations. The comparisons of significant diffcr- TABLE 2 3 ences among means are shown in Table 2. 4 Generally speaking, all of the coatings that were hypothesized to form 5 1 rviers to PCB residues did so when evaluated on the silo test sections 6 ar.d/or stave blocks. The two commercial coatings that did not have proper 7 ties predicted to be necessary for a good PCB barrier were indeed ineffec 8 tive when tested. The L9AN0V for the silo and block trials indicated that 9 the concentration of Aroclor 1254 in the silage was significantly (P<,01) 10 affected by coating treatments. 11 The coatings applied to the silo sections greatly reduced the PCB con- 12 a ntration when compared to the untreated control section, and significant 13 differences were observed between the individual coatings (Table 2). All 14 of who coalings adhered well to the silo wall. With the exception of the 15 water-carried epoxy in coating XT, coverage was good. This water-carried 16 ipoxy did not provide desirable coverage over the thinly applied rolvent- 17 u'rri.ed epoxy. The thickness of coatings I, IT, and V was about the same 18 1 ranged from .01 to .09 cm. The hydraulic cement material (VIT.3) pro 19 vided a very thick coating ranging between .35 and .72 cm. A film tbick- `0 could not bo determined for coating XI. ' 2J_ , Posults of the silo trials (Fig. 3) suggested that the solvent used to 72 fairy the coating materials may influence effectiveness of the coating. 23 7\.,oevlor 1254 has been shown to bo readily dissolved in the methyl isobutyl 24 ketone (MTl:K), cellosolve and xylene which are found in coatings II, V, and 25 XI (9). The Aroclor has low solubility in isopropanol used in coating I ' 1 DSW 038287 STLCOPCB4022111 -11- 1 > i d is insoluble in the water used to carry coating V'tlI. Tn contrast, 2 coatirajs IV, V and XI with MINK, collor-olve and xylene respoctively, w. vo 3 .u.-.ong the most effective barriers when evaluated on the .stave blocks (fig. 1 i) . 5 The coatIngs maintained their relative effectiveness .throughout the 6 three silo trials. There were no significant differences (P>.05) between 7 the three silages tested, indicating that different types- of silage had no 8 offoot on the l evels of Aroclor in silego nor did the .barriers become less 9 effective with continued usage. 10 The levels of Aroclor 1254 in the silages from block trial 1 were con- 11 :'l;r.-.bly lower than in either block trial 2 or in the silo (Fig. 3). This 12 ^ - obably resulted from the lower concentration of Aroclor 1254 in the cumar 13 '. iw.ir.g and porous surfaces of the blocks of trial 1. The porous surface 14 1 by,..-d the cm,'ar-Aroclor to penetrate, thus reducing the amount of A me l.or 15 that was in close contact with the harrier coating and silage, 16 This experiment indicated that a coating that contains a solvent in which Aroclor is vry soluble (9) should not be used. Coating VII contain 13 ed kcrosenO which resulted in significantly greater contamination of the 19 r.>l-.ge Ilian did kho cur.iar-Arcelor coni rol. ' Vhe ..d/. .lingo of two -co: -ponont coating syntc-ms was shown in the block 21 trials. Tn tln-so studies a two-component coating system utilized a modi.fir.-d 77 formulation to serve as a sealing base coat. Then the second comporiont of 'A wbiilnr material formed the coati.ny surface. Coatings I, IV, V ond IX v vo 24 all two-component systems. These materials, with the exception of coating 25 I, w.-re umong the most effective in this trial (Fig. 3). Coatings II and OSW 038288 STLCOPCB4022112 -12- 1 IT I wore two applications of the single-component equivalents of coatings 2 IV and IX, respectively. The two-eemponont r-yetems wove significantly (P 3 <.OS) more effective than the single--component for mul at ion of tlic same 4 material {Table 2). 5 Coating I v.'as not an effective barrier to the PCB residues nor did it 6 form the desired smooth surface in block trial 1. The surface of the coat- 7. ing was not smooth and solid as it subsequently appeared to be on the silo 8 v:all and in the second block trial. It was suspected that improper formu- 9 lation or application was responsible. 10 In block trial 2, three water-carried systems, two dual-component sys- 11 terns and a commercial silo coating were evaluated on relatively nonporous 12 stave blocks. Coatings I, IV, VI, VII and XII significantly (P<.05) re- 13 duced the Aroclor 1254 residue in the silages. There were no significant 14 differences am.o.ig these coatings (Table 2). The commercial coating XIII 15 was not significantly different from the untreated control. This coating 15 was softened by the silage juices, and consequently did not form an adequate 1/ l.nricr to the PCB residues. ; 13 Coatings I, IV, VI, and XIII showed signs of physical failure when ex- 19 .-.mined at the end of this trial. These coatings cracked or blistered indi- 20 eating that they wvro unable to bond to a smooth Cumur surface. Tin's i\di- 21 cated that those coatings should only be used on silos that no longer have 22 a solid and intact Cuir.ar finish. 23 The Aroclor 1254 concentration of silage was significantly (P<.01) in- 24 fluenced by the distance from the silo wall or the stave block. Significant 25 (p<.01) linear and quadratic effects vere also noted within the silo. DS 038289 STLCOPCB4022113 -13IVG. 4 1 Figure 4 shows the average distribution of Aroclor from the silo test soc- 2 lions. The average from all sections was used. 3 This distribution was as expected since the mechanism by which the 4 residues migrated was probably diffusion. These results agree with those 5 of Skrontny et al. (14) with the exception that beyond 15 cm from the silo 6 wall, higher levels were detected in this study. This may only reflect silo 7 and methodology differences. Also, these workers (14) did not state 8 whether Aroclor levels of silages were on a wet or dry matter basis. 9 Concentrations of Aroclor were significantly (P<.05) higher near the 10 base of the silo test sections. This may be the result of the downward 11 leaching of the silage juices. Leaching would deposit the PCB residues 12 near the base of the silo. This effect was not observed in the drum ex13 pc-rinents. The drums were sealed and contained a relatively small volume 14 of silage, thus extensive leaching would not be expected. 15 Eased on the results of the silo and block trials and commercial a16 vailability, hydraulic cement (VIII) and water-carried epoxy (VI) were 17 selected for use on two dairy farm silos. Both silos were known to contain 18 sufficient PCB's to cause the residue level in the herd milk to exceed .2 19 ppm. The histories and preparations of the silos was previously described 20 (page 5). Concentrations (ppm) of Aroclor 1254 in scraping of the silo 3 2J walls and in silage before and after recoating are shown in Table 3. 22 Concentrations of Aroclor were extremely high both in wall scrapings 23 and silage near the base of silo 1. Unfortunately, this silo was nearly 24 empty when located for experimentation so only limited precoating data was 25 available. The concentrations observed near the base may not be repre- D-SW 038290 STLCOPCB4022114 -14- 1 sentative of the entire silo as the residues may have accumulated near the 2 base, as a result of downward leaching of silage juice. However, the high 3 concentration of Aroclor residue (>.6 ppm) present in the milk produced on 4 that farm indicated that the cows had been consuming considerable quanti 5 ties of PCB. ; 6 The hydraulic cement coating VIII that was applied to this silo, after 7 thoroughly cleaning the walls with a wire brush, provided an effective bar 8 rier between the contaminated silo wall and the silage (Table 3). The con 9 centration of Aroclor 1254 did not reach .5 ppm during the two trials and 10 the PCB residue in milk continually declined throughout the experiment. 11 After three fillings of silage there has been no indication of failure of 12 the coating. 13 The base of silo 2 had been coated by the owner with a furfuryl alco 14 hol resin coating (I) prior to the discovery of the PCB contamination. The 15 concentrations in scrapings of and silage adjacent to this recoated area 16 v:ere considerably less than similar samples collected above the coated area 17 (Table 3). 18 The entire silo was cleaned with high pressure water (51 kg/sq cm) 19 then recoated to the 11.3 m level with the water-carried epoxy (VI). The 20 levels of PCB in the silage collected above the rocoated area were high 21 (Table 3). However, the residues were significantly reduced when collected 22 adjacent to the surfaces coated with the water-carried epoxy. The high PCB 23 concentrations observed near the top of the coated area probably resulted 24 from settling of the silage and the downward leaching of the silage juice. 25 As observed with silo 1 no failure of the coating was evident after two trials. osw o36291 STLCOPCB4022115 -151 GKNPIvAL DISCUSSION 2 The results of those experiments with barrier coatings have domonstra3 ted that a number of coating materials will form an effective barrier to 4 prevent significant PCB contamination of silage. Two coatings Will and VI) 5 have been shown to provide sufficient protection of the silage when used on 6 PCB contaminated silos that were in use on dairy farms. Based on the experi7 mental tests one would expect similar results could be achieved with some 8 of the other coatings that were tested. The vinyl coatings (II, IX) and the 9 organic solvent-carried epoxy coatings (IV,V) were shown to provide a bar10 rier to the PCB residues, but the organic solvents used as carriers may re11 duce their effectiveness as compared to the water-carried systems. Coating 12 I was effective in the silo trials, block trial 2 and remained as a bar13 rier five years after application to the base of silo 2. Coating XII was 14 a water-carried epoxy similar to VI, therefore, may form a successful bar15 rier to PCB's in a farm silo. With the exception of block trial 2, all of the coatings were evalu17 ated on a rough surface. In these trials the bonding of the materials to 18 the surface was good. The poor bonding that was observed on the smooth 19 blocks in trial 2 suggests that barrier coatings may fail to provide an 20 adequate protective barrier in silos having an intact smooth Cumar coating. 21 Likewise, bonding problems should be anticipated on silos that had been wax 22 treated or were improperly cleaned prior to recoating. 23 Results of these studies have indicated that PCB contaminated silos 24 can be effectively decortpminatcd by the application of a barrier coating. 25 The cost of decontamination (labor and materials) ranges from 10 to 18% of DSW 038292 STLCOPCB4022116 -16- 1 the silo replacement cost. Thus, on silos with sound porous surfaces, re- 2 coating is a practical alternative to the total replacement of the silo 3 structure, 4 Careful selection of a coating material is advised. The components of 5 certain commercial coatings are not approved by the Food and Drug Adminis- (, tration for use in livestock food storage containers. Likewise, use of 7 some coatings, particularly those that contain organic solvents, cannot be 8 used in certain areas as they will not meet air quality Standards or occu- 9 pational health standards during application. 10 The effective life span for a barrier coating has not been determined 11 at this time. Continued observation of recoated silos will eventually pro- 12 vide thi6 information. Some silo coatings have remained intact for as long 13 as 10 years when used to seal the inner surfaces of silos. It should be 14 emphasized that the effective life span of a barrier coating will be great- 15 ly reduced if the silo surface is improperly cleaned and prepared prior to 15 recoating. 17 ACKNOWLEDGEMENTS j 18 The author is grateful for the technical assistance provided by T. L. 19 Ayres, B, B. Beam, C. J. Brumm, C. F. Stellwagon and S. L. Welty, 20 This research was partially supported by gifts from Action I Plastic 21 Inc., Monsanto industrial Chemicals and Ohio Milk Producers Federation. 22~ Technical and material support was provided by Standard Dry Wall Inc., and 23 Universal Cooperatives. 24 25 DSW 038293 STLCOPCB4022117 -171 REFERENCES 2 (1) Armour, J. A,, and J. A. Burke. 1970. Method for separating poly 3 chlorinated biphenyls from DDT and its analogs. J. Ass. Offic. Anal. 4 Chem., 53:761. 5 (2) Department of Health, Education and Welfare, Food and Drug Administration. 6 1973. Polychlorinated biphenyls. Federal Register, 38 (29):18096. 7 (3) Fries, G. F. 1972, Degradation of chlorinated hydrocarbons under 6 anaerobic conditions. Adv. in Chem., Ser. 111:256. 9 (4) Fries, G. F. 1972. Polychlorinated biphenyl residues in milk of en 10 vironmentally and experimentally contaminated cows. Environ, Health 11 Perspectives, 1:55, 12 (5) Fries, G. F., and G. S. Marrow. 1972. Polychlorinated terphenyls as 13 potential contaminants of animal products. Presented at AOAC Meeting, 14 Washington, D. C. 10-10-1972. 15 (6) Fries, G. F., G. S. Marrow, Or., and C. H. Gordon. 1971. Similarity 16 in behavior of DDE and polychlorinated biphenyl {Aroclor 1254) resi 17 dues in an environmentally contaminated herd of dairy cows. J. Dairy 18 Sci., 54:796. (Abstr.) 19 (7) Fries, G. F., G. S. Marrow, Jr., and C. H. Gordon. 1972. Similarity 20 of a polychlorinated biphenyl (Aroclor 1254) and DDE in rate of 21 elimination from cows. Bull. Environ. Contamin. Toxicol., 7:252. 22 (8) Kolbye, A. C. Jr. 1972, Food exposures to polychlorinated biphenyls. 23 Environ. Health Perspectives, 1:85. 24 (9) Monsanto, (Undated Report). Aroclor Plasticizers, Monsanto Industrial 25 Chemical Co. Tech. Bull. 0/PL-306A. DSW 038294 STLCOPCB4022118 -18- 1 (10) Monsanto Industrial Chemical Co. 1971. Monsanto Methodology for 2 Aroclor, Analytical Chemistry Method, 71-35. 3 (11) Nisbet, I. C. T., aid A. F. Sarofim. 1972. Rates and routes of trans 4 port of PCB's in the environment. Environ. Health Perspectives, 1:21. 5 (12) Reynolds, L. M. 1969. Polychlorobiphenyls (PCB's) and their inter 6 ference with pesticide residue analysis. Bull. Environ. Contamin. 7 Toxicol., 4:128. 8 (13) Rote, J. W., and P. G. Murphy. 1971. A method for the quantitation 9 of polychlorinated biphenyl (PCB) isomers. Bull. Environ. Contamin. 10 Toxicol., 6:377 . i 11 (14) Skrentny, R. F., R. W. Hemken, and H. W. Dorough. 1971. Silo seal 12 ants as a source of polychlorinated biphenyl (PCB) contamination of 13 animal feed. Bull. Environ. Contamin. Toxicol., 6:409.. 14 (15) Snedecor, G. W. 1956. Statistical Methods. 5th Ed, Iowa State Univ. 15 Press, Ames. p. 253. 16 (16> Snyder, D., and R. Reinert. 1971. Rapid separation of polychlorinated 17 biphenyls from DDT and its analogues on silica gel. Bull. Environ. 18 Contamin. Toxicol., 6:385. 19 (17) Sproul, J. R. 1941. Acid-resistant concrete coatings. Ag. Eng., 22: 70 209 21 (18) Willett, L. B. 1973. Docs your silo contain PCB residues? Hoard's 22 Dairyman, 118:610. : 23 (19) Willett, L. B., and H. R. Conrad, 1973. Coatings as protective barriers 24 to polychlorinated biphenyl residues in contaminated silos. J. Dairy 25 Sci., 56:669. (Abstr.) DSW 038295 STLCOPCB4022119 TABLE 1. The identification, principle components, principle solvents and test locations of the barrier coatings tested. Coating Numeral Coating Type Principle Component'9 Principle Solvent Where Tested Farm Silo Block Silo Name^ I Furfuryl* Furfuryl Isopropanol X X alcohol resin 11 Vinyl Vinyl resin MIBK7 XX III Epoxy Epoxy resin Xylene X IV Epoxy* Epoxy resin Xylene X V Epoxy* Epoxy resin Cellosolve X X ,2 Silenzcrete ,2 Monolite 2 Epoxy 2 Epoxy 4 808-909 VI Water epoxy Epoxy resin Water XX 0094 VII Thermoplastic Alkyl aeromatic Kerosene X Type"0"6 hydrocarbon hydrocarbon VIII IX Hydraulic cement Vinyl* Cement + acrylic Vinyl resin Water MIBK7 X XX X Thoroseal6 2 Monolite X CONTROL Cumar-Aroclor Mineral spirits or Xylol > XI XII XIII Epoxy 4 Water epoxy Epoxy filler Phenolic resin Epoxy resin Epoxy resin Amberol Xylene Water Water Isopropanol Methanol X X X Epoxy2' 3 Waterpoxy Block filler 44C Sealer6 Two component coating system 2 Universal Cooperatives, Alliance, Ohio 3 General Mills Chemicals Co., Minneapolis, Minnesota ^ Action Plastic, Inc., Charlotte, Michigan 6 Standard Dry Wall, Inc., Miami, Florida 6 Whitteker Corp., Wooster, Ohio 7 Methyl Isobutyl Ketone g The use of trade names is only to identify the products used. The use of trade names is not an endorsement of the products used nor meant to discriminate against similar products not used. Q As stated by the manufacturer. DSW 038296 STLCOPCB4022120 TABLE 2. The comparison of differences in mean concentrations of Aroclor 1254 in silages from the barrier coating trials. Significant differences were determined by Hartley's S^uential Range Test.____________ _______ _ Coating Numeral Trial -- --------- ---- -------- ..COATING NUMERAL ...- - ------------------- _ ..... , ,, _ I II III IV V VI VII VIII IX X XI XII XIII Silo I Block 1 Block 2 "<a < >*> nsc > > > < ns ns < << > > ns ns < ns < Silo > II Block 1 < Block 2 ns ns < ns < ns ns > < > > < Silo III Block 1 ns > Block 2 > > > < > > ns Silo IV Block 1 < ns < Block 2 ns ns < ns < ns ns < ns < ns < Silo > ns V Block 1 < ns < ns Block 2 > ns < ns < < > >< Silo VI Block 1 < < < >> Block 2 ns ns | < > i> < ns : < ns < Silo VII Block 1 > > > >>> Block 2 > >> VIII Silo > ns Block 1 < < < Block 2 ns < ns < < < ns ns << ns < < ns < Silo IX Block 1 < < < ns < < < ns Block 2 < Silo >> > > : X Block 1 ns > ns > > > < > > Block 2 > >> > > ns Silo > ns XI Block l Block 2 Silo XII Block 1 Block 2 ns ns ns ns >< DSW 038297 ns < < XIII Silo Block 1 Block 2 > >> > ns STLCOPCB4022121 FOOTNOTES FOR TABLE 2 a Coating on vertical axis is significantly more effective them (P<.05) coating on horizontal axis. j k Coating on vertical axis is significantly less effective than (P<;05) coating on horizontal axis. c Coating effectiveness is not significantly (P>.05) different. DSW 038298 STLCOPCB4022122 TA3LE 3. Levels of PCB (pgm Aroclor 2204) in silage and silo wall surfaces collected before and after recoating. Level silage collected (m) 13.7 12.2 10.7 10.1 9.1 8.2 7.6 6.1 5.2 . 4.6 3.7 .3.1 2.1 1.5 0.3 0.0 -0.6 Scrapings before recoating (ppm) 20155.00 Silo la Silage before recoatingc (ppm) 103.00d 7131.88 Silage after reCOAfIxlge Trial 1 Trial 2 (ppm) (ppm) 0.013 0.06 0.013 0.05 0.08 0.27 0.38 0.42 0.24 0.29 0.07 0.02 0.07 0.08 0.10 0.11 0.16 0.10 0.11 0.07 Scrapings before recoating (ppm) 314.02 175.37 705.27 - 4.90 " 3.60 Silo 2b Silage before recoatingc (ppm) 5.11 8.04 0.99 0.03 Silage after recoatingc Trial 1 Trial 2 (ppm) (ppm) 20.68 58.98 28.80 1.91 0.85 1.06 1.00 13.43 ' 18.23 1.31 0.69 0.40 0.62 0.62 0.50 0.88 0.61 0.35 0.98 0.86 0.48 0.48 1.56 1.19 a Silo was coated with hydraulic cement with an acrylic bonder (coating I). k Silo was coated with water-carried epoxy from the base of the pit to 11.3 m above the ground (coating VI). oc Sampled adjacent to the silo wall. 0 ^ This sample was a blend, not adjacent to the silo wall. oj 03 ro > . vO ' FIG. 1. Dividers made of Masonite were used to separate the coating test sections in a PCB contaminated silo. The test coatings were used to seal the junctions between the Masonite and the silo wall. DSK 038300 STLCOPCB4022124 c DSW 038301 STLCOPCB4022125 Of O 0.4 O 0.2 u < 0.0 BLOCK TRIAL 1 ! BJLBjl fl Jl.n i III x VI II v IV IX VIII COATING NUMERAL FIG. 3. Average concentrations (ppm) of Aroclor 1254 in silage from the various barrier coatings test locations. Each bar of the histograms represents the average from all sampling locations. The X is the un treated control section in the silo and the Aroclor-cumar coatings in the block trials. ! DSW 038302 STLCOPCB4022126 V* in t'. O. t u O < f. o r\ r>. * ........ .... * fc t ' \ 60 90 ."i 'i 120 CM ;vO/A SILO WALL l if:. <5. '.'.v W. i\r, f.'- . t : c.;-.*?.. >.^r of t.;.o 3.i \i r;f.0-3 *n'i cor.'.rol s:fictions. :jbetion of or 12?4 in t!vi y.fi-c-.iT. rv^xc'.'rr.-ts tne evvri^o .'.to.-. OSW 038303 STLCOPCB4022127