Document JNNewrv1bGvp33e6drLZQ3v5K

\ ^ T5' physical r properties and A suggested 0221971 TOWOLDMONOQ26592 FOREWORD The Aroclors*, chlorinated biphenyl and chlorinated poly-phenyls, possess unique properties which enable the fulfillment of requirements not met by other materials. This has won a prominent place for Aroclors. particularly, in the electrical insulating field and in such widely differing applications as nonflammable hydraulic media, high* temperature and high-pressure lubricants, heat-transfer and expansion media, sealing compounds, adhesives and protective coatings, including plastics, pigments, lacquers, paints and varnishes. This booklet describes the properties of thirteen Aroclors, each of which is representative of a series. For almost every Aroclor described there is a dark-colored grade of other wise approximately the same physical and chemical char acteristics. These darker products arc less pure but lower in price. The Aroclors are efficient and very economical, both when used alone to accomplish results not attainable by other materials and when used as extenders to enhance the properties of other products. They arc produced exclusively by Monsanto Chemical Company. . *Regiilered in L\ S. Patent Office. . .. 0221972 TOWOLDMONOQ26593 INDEX - Page No. GENERAL PROPERTIES................................ 3 General Physical Properties of Some of the Aroclors............................................4-5 Resistance of Structural Materials to Aroclors................................................... 6 Adhesiveness....................................................7 Specific Volume................................................7 Average Coefficients of Expansion, Aroclor 1248................................................7 Corrosion...................................... 7 Density............................................................... 9 Electrical Properties........................................9 Non-drying Properties.................................... 9 Nonflammability............................................... 9 Solubility........................................................... 9 Specific Ileal and Thermal Conductivity . 9 Electrical Properties........................................9 Thermal Conductivity of Aroclor 1248 . . 10 Stability .......................................................... 10 Toward Alkalies..........................................10 Toward Acids..............................................10 Toward Heat................... 10 Toward Oxidation...................................... 10 Surface Tension..............................................10 Therinoplasticity.............................................. 10 Vaporization Loss.......................................... 13 Vapor Pressures..............................................13 APPLICATION OF AROCLORS...................15 Adhesives................... 15 Electrical Equipment...................................... 15 Expansion Medium.......................................... 15 Page No. Hydraulic Medium..........................................15 Power Transmission.................................. 15 Hydraulic Pressure Medium...................... 15 Liquid Heating Medium.......................... 16 Lubrication...................................................... 17 Air Compressors..........................................17 Cutting Oils..................................................17 High Temperature...................................... 17 Extreme Pressure...................................... 17 Submerged Lubrication.............................. 18 Gaskets and Packing Materials...................... 18 Dermatology and Toxicology.......................... 19 Suggested Uses for Aroclors in Plastics, Pig ments, Lacquers, Paints, Varnishes and . Waxes......................................................... 20 Compatibility with Various Materials . . 20 Ethyl Cellulose..........................................20 Graphic Arts.............................................. 20 Impregnation................................... .... . 21 Moisture Proofing ...................................... 21 Pigment......................................................21 Paints and Varnishes..................................21 Rubber and Rubber Substitutes .... 22 Modified Rubber Finishes..........................22 Vinyl Resins................................................. 22 Nitrocellulose Coatings..............................23 Waxes............................................................. 23 Diagrams Showing Practical Composi tion of Lacquers Using Aroclors 1254 and 1262 ........................................24-25-26 Other Literature on Aroclor Applications......................................27 i 2 0221973 TOWOLDMONOQ26594 General Properties The Aroclors range in form and appearance and Aroclor 5460 is insoluble in the lower from mobile oily liquids to fine white crys molecular weight alcohols. Aroclor 4465 is tals and hard transparent resins. They arc only partly soluble in the lower alcohols. non-oxidizing, permanently thermoplastic, of low volatility and non-corrosive to metals. They arc not hydrolyzed by water, alkalies or acids. The viscous liquids and the resins will not support combustion when heated alone. The excellent electrical properties, fire resistance and inertness of the Aroclors make them useful in many applications. The properties imparted by the Aroclors and their usefulness for particular applica The crystalline Aroclors are relatively insol tions vary in regular gradients over the uble, but the liquid and resinous products series so that the selection of the right are soluble in most of the common organic Aroclor for a specific use can generallv be solvents, thinners and oils. All Aroclors are made simply by a comparison of the physi insoluble in water, glycerine or the glycols. cal properties of the several Aroclors. 0221974 TOWOLDMONOQ26595 TAB. GENERAL PHYSICAL PROPERTIE! Form................................................................... Aroclor 1221 Colorless mo* bile oil Color.................................................................. 50 Max. (APUA) Aroclor 1232 Aroclor 1212 Arcolor 1248 Fracticallv Practically Yellow tinted colorless mobile colorless mobile mobile oil oil oil 60 Max. 100 Max. 100 Max. (APIIA) (APIIA) (APIIA) Aroclor 12' Light vellnw viscous oil 150 Max. (APIIA) Acidity--Maximum (Mgm. KOH per Gm.).. 0.015 0.015 0.015 0.015 0.015 Average Coefficient of Expansion........................................cc/cc/C Typical Density Specific Craviiv 25/25C (77/77F).......... Pounds per Gallon--25UC (77*T')................. 0.00071 (15-40C) 1.182 9.85 0.00073 (25-100C) 1.266 10.55 0.00068 (25-65C) 1.380 11.50 0.00070 (25-65C) 1.445 12.04 0.00066 (25-65C) 1.538 12.82 Distillation Rancf.--ASTM D-20 (Mod.) Coer. C.......................................................... 275-320 Evaporation toss--%--ASTM D*6 Mod. 163C..................................................... 5 hr*. -- 100C..................................................... 6 hrs. 1.0 to 1.5 290-325 -- 1.0 to 1.5 325-360* 3.0 to 3.6 0.0 to 0.4 340-375 3.0 to 4.0 0.0 to 0.3 365-390 1.1 to 1.3 0.0 to 0.2 Flash Point--Cleveland Open Cup.........C 141-150* F 286-302 152-154 305-310 176-180 348-356 193-196 379-384 None Fire Point--Cleveland Open Cup.............*C 176 F 349 Pour Point--ASTM D-97..........................C F Softening Point--ASTM E-28................. C CrvstaU at 1C CrvataU at 34*F -- F -- Refractive Index--D-linr--20C................. 1.617-1.618 Viscosity'--Savboh Universal 210F (08.09C) Sec. (AS 1 M-Lmw) 130.f (5, 4oC) 100F (37.8*0 30-31 35-37 40-12 238 460 -35.5 -32 -- -- 1.620-1.622 31-32 39-41 47-50 None* -19 2 -- -- 1.627-1.629 34-35 49-56 80-93 None --7 19.4 -- -- 1.630-1.631 36-37 69-78 185-240 None 10 50 -- -- 1.639-1.641 44-48 260-340 1800-2500 NONK imtiralr* -"No fire point up to boiling lrmj*rrulrc" 4 ql* TOWOLDMON0026596 I OF SOME OF THE AROCLORS Aroclor 1260 Light yellow oft sticky resin 150 Max. (AP11A) 0.015 Aroclor 1262 Light vcllnw sticky clear resin 150 Max. (API1A) 0.02 0.00067 (20"-100"C) 1.620 15.50 0.00064 (25-65C) 1.646 13.72 S85M20" 0.5 to 0.8 0.0 lo 0.1 None 400"-430" 0.5 to 0.6 0.0 to 0.1 None None None SI* 88* -- 1.617-1.649 72-78 3200-1500 37" 99" - 1.6501-1.6517 90-103 600-850 (l6U*F<tr7l*C) Aroclor 1268 White opaque resin 1.5 Max. NPA 0.05 Aroclor 4465 Yellow transparent brittle resin 2.0 Max. NPA 0.05 Aroclor 5442 Yellow trans-a parent sticky resin 1.5 Max. NPA 0.05 0.00067 (20"-100"C) 1.810 15.09 0.00061 (25"-65C) 1.670 13.91 0.00123 (25"-99C) 1.470 12.24 435"-450" 0.1 to 0.2 0.0 to 0.06 None None 135" lo 160" (hold pt.) 275 to 320 (hold pt.) -- 230-320 at 4 mm. Hg. 0.2 to 0.3 0.0 to 0.02 None None 60" to 66" 140" lo 151" 1.664-1.667 90-150 (*6*F or 1S0*C| `-- 215-300 at 4 mm. llg. 0.2 0.01 247" 477" >350" >662" 46" 115" 50" to 61" 113" to 122" -- 300-400 Aroclor 5460 Yellow transparent resin 2.0 Max. NPA 0.07 Aroclor 2565 ttrown-black opaque resin -- 1.4 0.00179 (25"-124"C) 1.670 13.91 0.00066 (25"-6ScC) 1.734 14.44 280-335 at 5 mm. Hg. 0.03 1.5 to 1.7 (I 260*--$ kr.) None 0.2 to 0.3 None None None 100"tol0S.5" 212" to 222" 1.660-1.665 - 66" to 72" 149" to 162" -- - 5 012l<nb TOWOLDMONOQ26597 TABLE II--Resistance of Structural Materials to Arodors Metals 1248 25C 125C Aluminum......................................................................... Copper............................................................................... Magnesium....................................................................... Nickel................................................................................. Silver.................................................................................. Tin...................................................................................... Zinc..................................................................................... Mild Steel......................................................................... Phosphor Bronze............................................................ Red Brass......................................................................... Stainless Steel (Type 316)............................................ Yellow Brass.................................................................... R R RR RR R R R RR R D RR R Plastics Alkyd Resin No. 46594-12........................................... Alkyd Resin No. 46594-13A....................................... Cellulose Acetate (Fibcstos)....................................... Duritc Phenol Furfural Resin..................................... Formvar Highly Plasticized........................................ Formvar Low Plasticized............................................. Glyptal 1276.................................................................... Clyptal 7136.................................................................... Maleic Resin No. 46594-13B...................................... Maleic llcsin No. 46594-13C...................................... Plexiglas (Methyl Methacrylotc).............................. Polystyrene (Lustron B).............................................. Resinox Mineral Filled Melamine Resin................. Resinox Rood Flour Filled Melamine Resin......... Resinox Mineral Filled Phenol Formaldehvde.... Resinox R ood Flour Filled Phenol Formaldehyde Resinox Rug Filled Phenol Formaldehvde............. Urea Formaldehvde Resin (Plaskon Co.)............... *P D D D De PS R D P P D P *D D D *D *D *D R D R R R R R R D D RR Re P P P P T T P T P P P T P P D P D P Anocixm Number 1254 25C 125X RR RD RR R RR RK RR RR RR RR RR RD RR UR R De *P D D R Pe PS D R P R 1> P *R *R D D D D P P P P T T P T P P P T R D D R D P 4465 125*C RR D RR RR R R R R R R RR Re P P P D T T P T P P P T P R R D D P 5460 125*C RR D RR R R R RR RR R De RR Re P P P P T T P T P P P T D P P P P P Meaning of Abbreviations: " *--Based on weight gain calculated as penetration value shown. RR--Excellent resistance--less than 1.0 x 10~* cm/day penetration or .60014 in/vr. R--Good resistance--has penetration between 1.0 x 10-4 and 10 x 10~4 cm/day or between 0.00014 and 0.0014 in/yr. D--Doubtful resistance, penetration between 10 x 10"4 cm ''day and 100 x 10 4 cm/day or between 0.0014 and 0.014 in/yr. P--Poor resistance--penetration greater than 100 x 10*4 cm/day or 0.014 in/yr. PS-^Poor resistance due to visible local action although weight change indicates greater resistance, e -- Following the letter indicating resistance signifies material may be better than indicated if totailv immersed since weight loss is believed to come from oxidation of the part of test strip exposed to air. T--Material atone will not stand temperature. ` , . 6 0221977 TOWOLDMONOQ26598 ADHESIVENESS The Aroclor resins ahdere strongly to smooth surfaces* such as glass, metal and varnished or lacquered coatings. The softer Aroclors are indicated where a flexible* non-drying, water-resistant strongly adhesive ma* terial is required. The Aroclor adhesives are thermoplastic; are readily applied hot without solvent; do not require high temperatures for easy application, and are set immediately upon cooling. SPECIFIC VOLUME The specific volume of Aroclor 1248 at different temperatures is as follows: Temp. F Aroclor 1248 Specific Volume ml/gm 0 0.674 100 0.699 200 0.726 300 0.755 400 0.790 500 0.828 600 0.870 FIG. I AVERAGE COEFFICIENTS OF EXPANSION, AROCLOR 1248 The average coefficient of expansion of Aroclor 1248 per degree F. within the various temperature ranges indicated in the table below was deter* mined by using the simple formula Vt -- Vtl [1+a (t-ti)]. The coefficient, a, has been calcu lated at 100F increments, as follows: Temp. Range F 0 to 100 100 to 200 200 to 300 300 to 400 400 to 500 500 to 600 Average Coefficient of Expansion cc/cc/ F 0.00037 0.00039 0.00040 0.00046 0.00048 0.00051 CORROSION The Aroclors show practically no corrosive effect on metals within normal ranges of temperature. They do attack many plastics materials of con struction as shown in Tabic II. r fo jo u /r e D s w r r ((?M5./ c c ) 40 SO /20 /60 200 240, 260 320 360 400 440 TMPPArO Dt}S C 7 OZZ^76 TOWOLDMONOQ26599 FIG. 2 l TOWOLDMON0026600 DENSITY AH the Aroclors are heavier than water, a valuable property for many applications. Densities are shown in Figure 1. ELECTRICAL PROPERTIES ^ The Aroclors have extremely interesting electri cal characteristics: high resistivity and dielectric strength and low power factor. The dielectric con stant ranges from 3.4 to 5.0 at 100C. and 1000 cycles, depending upon the particular Aroclor. The dielectric constants of Aroclors 1242 and 1254 at various temperatures are shown graphically in Figure 2. The electrical properties of the Aroclors arc shown in Table 111. NON-DRYING PROPERTIES The Aroclors are non-drying, and when they are exposed to the air, even in thin films, no notice able oxidation or hardening takes place. How ever, w'hen used as ingredients of lacquers, they do not retard the rate of drying of the lacquer fi)m6. Quick drying varnishes and paints may be made with Aroclor resins. ______ NONFLAMMABILITY The viscous Aroclor oils and the resins do not support combustion when heated alone, even at their boiling-points -- temperatures above 350C Most of the Aroclors flux readily with resinous and pitch-like materials to give a product hav ing a decreased Are hazard. When incorporated in nitrocellulose films and rubber foams the Aroclors retard the rate of burning. SOLUBILITY All Aroclors are insoluble in water. Solubilities of some of the Aroclors in the more common sub stances are shown in Table VI. The Aroclor oils and resins are readily soluble in most of the common organic solvents and drying oils. The hard crystalline materials are in general less soluble than the Aroclor oils or softer resins. Compatibility data on Aroclors in nitrocellulose lacquers are shown on page 18. SPECIFIC HEAT AND THERMAL CONDUCTIVITY The specific heat at different temperatures of - several of the Aroclors is shown in Figure 3. This, together with the thermal conductivity data given in Tabic IV, enable calculations involved in the use of Aroclors as high-temperature, low pressure, fluid heat-transfer media. TABLE ///--Electrical Properties Dielectric Constant at 1,000 Cycles (1) Aroclor 25C 100C Volume Resistivity (2) Ohm--cm at 100C, 500 Volts D.C. Dielectric Strength (3) 1232 1212 124B 1251 1200 1268 54-12 5454 5460 4465 5.7 5.8 5.0 5.0 4.3 2.5 3.0 2.7 2.5 2.7 4.6 4.9 Above 500x10 Greater than 35KV 4.6 Above 500x10 Greater than 35K\ 4.3 Above 500x10 Greater than 35K.V 3.7 Above 500x10 Greater than 35KV -- 4.9 Above 500x10 4.2 3.7 3.3 (1) astm nno.vrr (2) ASTM D.2.>?-U< (3) ASTM IM40.1I (4) ASTM U-150-trr Power Factor (4) 100C, 1,000 Cycles <0.1% <0.1% <0.1% <0.1% 9 0221980 TOWOLDMONOQ26601 CALORIES ( 1 5 * 0 PER GRAM PER *C FIG. 3 HEAT CAPACITY OF AROCLORS of varSot/s tomptrofvres Table IV Thermol Conductivity of Aroclor 1248 Temperature IITU./jlr./Sq. Ft./ Calories, gram/Sec./ *C. *F.F./Ft.Sq.Cm./C./Cni. 30 90 0.0680 281 x1(T` 60 140 0.0687 284 xl<r* 100 212 0.0697 288 x10"* STABILITY Toward Alkalies The Aroclors arc remarkably resistant to the action of either hydrolyzing agents or high tern|crattire. They are not affeeted by boiling with sodium hydroxide solution. Toward Acids K\|KTimonts were made to determine whether hydrogen chloride is evolved during the treat ment of Aroclors with sulfuric acid. Aroclor 1251 (elected as typical) was stirred with an equal vol ume of ten per cent sulfuric acid for a jH'riod of 150 hours. Any gases escaping from the reaction flask had to pass through a trap filled with silver nitrate solution, which solution would give a precipitatc of silver chloride if any 1IC1 cainc in con* tact with it. After 150 hours of treatment, neither the trap solution nor the acid layer in the treat ing flask showed any hydrogen chloride present. Even prolonged treatment (255 hours) with con centrated sulfuric acid indicated only a slight trace (too small for quantitative measurement) of hydrogen chloride in the acid layer. Toward Heat Because of their stability to heat, the Aroclors are useful heat-transfer media. Aroclor 1254 and particularly the less viscous Aroclor 1248 arc recommended for this purpose because they may be heated at temperatures up to 315C (600F) in a closed system for long periods without appreciable decomposition and are at the same time nonflammable. Toward Oxidation WheuAroclors are subjected to a bomb lest atl40C with 250 pounds oxygen per square inch oxygen, there is no evidence of oxidation as judged by development of acidity or formation of sludge. SURFACE TENSION The surface tension of Aroclor 1254 in dynes per centimeter is as follows: Temperature Surface Tension- 25C 80C 100C 50.3 44.0 42.0 THERMOPLASTICITY The Aroclors are permanently thermoplastic. They apparently undergo no rondcnsalion or harden ing upon repeated melting and cooling. The clear Aroclor resins are now being produced with soft ening |M>iiits up to I05C. The opaque crystalline solids are produced with initial melting points up to approximately 290C. 10 TOWOLDMONOQ26602 TABLE VI--Solubility of Arodors in 100 Milliliters of Various Solvents Aroclor Type of Srlvcnt 1212 2.VC Hot 1248 25C Hot 12.VI 23C Hot 1270 Cold Hot Acetic Arid.,,.. .................. S Oleic Acid................................. s Rename Acid............................ 10.0 *'*C s s* __ -- -- 10.0 _ -- -- sS sS ---- -- -- -- Aldrhvde 40* f Formaldehyde............... 1 I Furfural..................................... VS vs Amine ss Pvridine.................................... 132.5 *c 4io w.: Chloro--fieriva tivet (lariton Tetrachloride........... Chloroform............................... s s s __ s s s __ Monochlnroltenrrnr.............. s s __ s s __ s s Trichlorethylcne..................... s Drying Oil s Linnecd Oil............................... s Ester Amyl Acetate.......................... s Butvl Acetate.......................... s Cellosolve Acetate................. s Cottonseed Oil........................ s Dihutvl Phthalatc................. s l>iethyl I'hlhulatr.................. s Ethyl Acetate.......................... s Ethvl Lactate.......................... s Kthvlcne Glvcol Diacetatc.. s Methyl Acetate...................... s Tricresvl Phosphate.............. s Ether: Ethvl Ether................... s Ether Alcohol Carhitol..................................... MA i*o Cellosolve................................. s Uiethvlene (rlvcol.................. -- p*p' Dihvdroxy Ethvl Ether . 16.9 <: Ilvdrocarlton nenzrne..................................... VS Gasoline.................................... VS Kerosene................................... vs Mineral Spirit*........................ vs *> 0 ST.S'C s s s s s s s s s s s s s s s s s 307 s -- 19 "*c vs vs vs vs s Pine Oil..................................... s Toluene..................................... vs Turpentine............................... vs Xylene....................................... vs Hydros v--derivatives Amvl Alcohol.......................... s n-Hutvi Alcohol .................... s Ethvl Alcohol (3*\).............. 23.3 ***`- Glycerine.................................. 1 Methyl Alcohol...................... .l* s SST Phenol--90r#.......................... 191 Ketone Acetone..................................... s Miscellaneous tJarlson Disullide.................... Nitrohenrene. ...................... s s s vs vs vs s s 80.0 1 88.5 s s s s I1 VS vs ---- ---- ss ss ss __ -- ss ss __ -- ss ss ss ss ss ss ss ss ss ss ss ss ss ss ss ss ss vs vs ss ---- SS SS vs vs vs vs 2.0 *C vs vs vs vs vs vs vs vs s vs vs vs vs --_ ---- ---- I1 ---- __ -- __ -- -- -- -- -- 1T vs VS ss 114S1*C 425 sS sS ss ---- ss ss ---- ss ss ss ss ss ss ss ss ss ss ss ss ss ss ss ss ss 173 s -- 8 x>*c 259 ** s -- 10 twe vs vs vs vs vs vs vs vs --s ss vs vs vs vs vs vs s s 10 *rc I 15*c SS s s 28 TS*C I 22.2 s ss ss ss I SS -- -- -- 3.7 -- 3.0 -- 2.9 -- -- 3.3 -- -- -- -- -- -- -- -- -- -- -- -- -- -- S -- -- -- -- 3.5 -- -- -- -- -- -- -- " -- -- -- I -- -- -- -- -- Rater........................................ 1 1 11 1 1 -- Insoluble S - Soluble SS Slightly Soluble VS Very Soluble Figures show grams of Aroclor jut 100 milliliters of solvent at 21>CC. miles* other* ior indieated. -- -- -- I SS -- -- -- -- -- -- -- -- -- -- -- -- -- -- -- -- -- -- -- -- -- -- -- -- -- s -- -- -- -- -- -- -- -- -- -- -- -- -- -- -- -- 1 -- -- __ -- -- I 4165 Cold Hot SS" s s vs ---- II vs vs vs vs vs vs vs vs vs .vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs vs V8 vs VS vs VS s vs s vs s vs s vs vs vs vs vs ss SS s s-- SS -- s-- s-- SS -- vs vs vs vs <5.0 s vs vs vs vs vs vs vs s s vs vs vs ss SS s SS -- 11 SS -- ss ss vs vs vs -- 1I S160 25C -- -- -- -- -- -- -- -- 156 -- -- -- -- -- ~ -- -- -- -- -- -- -- -- -- -- -- -- -- -- -- -- -- .-- -- M3 -- -- -- -- -- M2 -- 178 -- -- -- -- -- -- 260 -- -- 11 OZilfBZ TOWOLDMONOQ26603 TOWOLDMONOQ26604 VAPOR PRESSURE -- m m MERCURY FIG. 5 VAPORIZATION LOSS The low vaporization loss of Aroclors is indicated in the following Table VII. * It is concluded that the vaporization rates of Aroclors--especially 12.>4 and 1260 which are the most widely used members of the Aroclor family in the plasticizer field, compare most favorably with the similar constants of other plasticizers selected specifically for these tests because of their low vaporization rates. VAPOR PRESSURES The vapor pressures of several Aroclors arc indi cated in Figure I over the temperature range. 150 to 300C. The following estimated vapor pressures of several Aroclors at 100F shown in Table VIII were determined by extrapolation from the values shown in Figure l. 13 0221984 TOWOLDMONOQ26605 Sample Aroclor 1221................................... Aroclor 1232................................... Aroclor 1242................................... Aroclor 1248................................... Clorafin-42-S.................................. FlexoI-DOP (dioctyl phthalate). . Dutrex 25....................................... Aroclor 1254................................... Dutrex 20....................................... Aroclor 1262................................... Aroclor 1260................................... Aroclor 4465................................... Aroclor 1270................................... Aroclor 5442................................... Aroclor 5460................................... Tricresyl phosphate....................... TABLE VII Vaporization Rates Wt. Loea Cm*. ... 0.5125 ... 0.2572 ... 0.0995 ... 0.0448 ... 0.0745 ... 0.0686 ... 0.0156 ... 0.0064 ... 0.0039 ... 0.0032 ... 0.0010 lloura Exposure 24 24 24 24 48 48 24 24 24 24 24 72 72 72 72 24 Surface Area Cm* 12.28 12.28 12.28 12.28 12.28 12.28 12.28 12.28 12.28 12.28 12.28 12.28 12.28 12.28 12.28 12.28 Vaporisation Rate Zms./cm^hr./lOO^C 0.00174 0.000874 0.000338 0.000152 0.000126 0.000117 0.000087 0.000053 0.000016 0.000013 0.000009 0.000007 0.000005 0.000004 0.000004 0.000003 TABLE VIII Approximate Vapor Pressures Calculated at 100 F (37.8 C) Aroclor 1232.............. ..............0.005 Aroclor 1242.............. ..............0.001 Aroclor 1248.............. ..............0.00037 Aroclor 1254.............. ..............0.00006 mm. Hg. mm. Hg. mm. Hg. mm. Hg. 077X985 TOWOLDMONOQ26606 APPLICATIONS ADHESIVES Liquid and resinous Aroclors are noted commer cially in the adhesives field for their usefulness in preparing synthetic adhesives and as additives in protective coatings to improve adhesion. This quality of the Aroclors is related to their plasti cizing action on the plastics materials commonly used in adhesives and coatings. Interesting examples are the use of Aroclors in adhesives and coatings based on polystyrene, vinyl polymers, ethylccllulose, chlorinated rubber and other plastics materials, usually polymers. Aroclor adhesives are thermoplastic and can be prepared either with or without solvents. Hotmelt Aroclor adhesives do not require high tem peratures for easy application and are set immedi ately upon cooling. Aroclors strongly resist attack by water, acids, alkalies, and other common corrosive influences as well as organisms. By proper selection of materials, adhesives utilizing Aroclors can be made to possess outstanding resistance against all of these destructive influences. The most widely used Aroclors in the adhesives field are 1254, 1260, 4465 and 5460. ELECTRICAL EQUIPMENT Because of their nonflammability, high resistivity and dielectric strength and low power factor, the liquid and resinous Aroclors are extremely useful materials for the electrical industry. Aroclors are used to impregnate capacitors or condensers and transformers. Since the liquid Aroclors will absorb sufficient moisture from the atmosphere to impair the electrical characteristics, it is customary to treat Aroclor intended for this application before use with a dehydrating clay. An effective product for this purpose is Attapulgus clay 80/300 mesh dried for 4 hours at 400C. and used at the rate of 0.125% based on the w'eight of Aroclor, followed by filtration. Treatment is improved if the Aroclor is heated to 80-85C. Another important use of Aroclors in the electrical field is the use of Aroclors 1260, 4465 and 5460 in wire or cable coatings and as impregnants for cotton and asbestos braided insulation. Aroclor 5460 is useful as an iinpregnant for carbon radio resistors to reduce the influence of moisture. EXPANSION MEDIUM Because of their stability under variations in temperature and freedom from gum formation from oxidation, the Aroclors are useful as expand ing media in bellows controls and in thermostats. HYDRAULIC MEDIUM Power Transmission The Aroclors are superior hydraulic media for power transmission. Because of their greater den sity and E. P. characteristics they approach more closely the theoretical transmission values for mechanical power as illustrated in Figure 6. This greater efficiency makes possible a reduction in the size of the hydraulic coupling design. In order to meet extremely low-temperature weather conditions, it is necessary to adjust the freezing point of the Aroclor selected by the addi tion of a pour point depressant. Suitable adjust ments can be made in the composition to reach a pour point of minus 65F. The steepness of the viscosity-temperature curve of the Aroclors is a handicap to the application of Aroclors to many types of fluid transmission. This curve can be flattened to a marked degree by introduction of a viscosity-index corrector. By proper choice of viscosity modifiers and pour point depressants, the viscosity-temperature curve can be made to coincide with any standard hydro carbon oil viscosity curve. Information will be gladly furnished. Hydraulic Pressure Medium Use of D.T. Light Oil (mineral base) or other flammable oils as hydraulic media in the operation of pressurized systems in the vicinity of open flames or metallic surfaces heated to elevated temperatures has resulted in substantial property damage and also serious burns including loss of 15 0211986 TOWOLDMONOQ26607 life as a remit of fire. Zinc ami aluminum alloy die-casting machines and hydraulic mechanisms used to operate doors and other equipment around industrial furnaces arc excellent examples of operations where it is prudent to use a noncumbustiblc hydraulic medium for safety reasons. Some of these systems operate under pressures as high as 2000 pounds per square inch. ^ hen a line ruptures under these conditions, the hydraulic medium is emitted in the form of a spray or a fine mist over a wide area. Such a mist presents un usual requirements with reference to the non* combustible qualities of the hydraulic medium. For safety under these conditions, it is essential that the oil must have a relatively high oxygen requirement in order not to support combustion when impinged on a hot metal surface or when in contact with fire. Ability to fulfill this requirement 16 not adequately reflected merely by the factors that an oil does not possess a flash point, and a fire point in conjunction with a high spontaneous ignition temperature. Spray flammability to a large degree seems to be a separate consideration. Tests conducted by the Navy indicated that high boiling liquids requiring more than approximately 45 percent oxygen in the spray flammability tests failed to cause a Arc in the incendiary firing tests also conducted by the Navy. The percent of oxygen requirement for Aroclor 1218 combustion in the spray flammability limit study was established at 64 percent. This result firmly establishes the nonflammable and noncombustiblc qualities of Aroclor 1248 and in this respect strongly recommends Aroclor 1248 as an unusually safe hydraulic medium. Other desirable qualities of Aroclor 1248 for this specific use arc its extremely high order of stability under heating and pressure, lubricating qualities, noncorrosivcncss, moisture resistance and relative freedom from odor. Aroclor 1248 is used commercially in centralized tine and aluminum die casting systems. Such installations may involve operation with as much as 2000 gallons of Aroclor 1218 distributed to about 15 die-casting machines. Under proper operating conditions the Aroclor make-up in the system is very low. Normal ojn*rating tempera tures of the hydraulic medium may be in the range of 70 to 120F. Centralized systems utilize piston-type pumps and an accumulator is used for smooth operation. In some instances, Aroclor 1248 is used in combi nation with a high lubricity oil in the proportions of 20 gallons of Aroclor and not more than one gallon of the oil. The hydraulic medium is kept clean and free of suspended particles by passage through a centrifugal or by filtering it through a properly prepared bed of Attapulgus earth. Aroclor 1248 is also used in individual or unit die casting systems usually equipped with vanc-tvpe pumps. Frequently these individual die-casting machines have built-in filters. However, if the machine is not already' provided with a filter, either a portable or permanent filter should be provided in order to keep the hydraulic medium clean. Liquid Heating Medium Aroclors 1242, 1248 and 1251 are used as a circulating heating medium with great success. Good circulation and a well designed heating sys tem arc necessary to prevent local overheating of the Aroclor heating medium. Aroclor 1248 is roe- 16 TOWOLDMONOQ26608 omntended for universal use up to 315C (600F) because of its fluidity at low temperatures and its nonflammability. In processes where a cooling cycle must also be introduced, provision can be easily made for shunt* ing circulating Aroclor through a water cooled heat exchanger, thus employing one medium for both heating and cooling. In special cases, Aroclors 1242 and 1254 can be substituted for the Aroclor 1248. If extremely low outside temperatures are encountered, the less vis cous Aroclor 1242 can be used, but it has the disad vantage of being flammable above 330C (626F). Higher temperatures up to 325C (617F) can be attained in the heating medium if Aroclor 1254 is used. Provision can easily be made for warm ing the Aroclor after a shut-down so that it can be pumped. Design for a simple, effective liquid Aroclor heat ing system for small unit operations is available and described in Monsanto Technical Bulletin No. P-130. LUBRICATION Air Compressors The presence of oil, oil vapors or mixtures of oxygen and oil fractions in the discharge lines and receivers of air compressors presents a constant hazard which needs only a particle of hot carbon to create a serious explosion. This problem has been solved by engineers of one large user of this typo equipment by employing Aroclor 1254 as the internal lubricant for high compression air compressors. Their experience with more than 15 high-pressure compressors of various types is reported in the American Machinists Magazine, September 28, 1044. This use of Aroclors is described in Monsanto Technical Bul letin No. P-128. Cutting Oils Aroclors arc used commercially in high quality cutting oils of the "straight" oil and "soluble** oil types. High Temperature The heat-resisting, nonflammable characteristics of the Aroclors make them attractive as lubricants under conditions of high temperature, as, for ex ample, in governor systems of central power sta tions. Aroclor 1248 is well suited to this application. Straight Aroclor 1254 gave excellent results on a roller bearing test operating at 255-260F with much less carbonization or decomposition than the usual spindle oil under the same conditions. Extreme Pressure It is a well accepted hypothesis in the lubrication industry that by the addition of certain elements such as chlorine, sulfur and others in the proper form to a lubricating oil, a certain chemical com bination takes place with the iron or steel metal bearing surfaces. These surface compositions tend to prevent seizure of the rubbing surfaces under extreme loads and under which loads, if the sole lubricant were a pure mineral oil, seizure or scor ing would result at once through film failure. As an extreme pressure (E. P.) lubricant base added to a petroleum hydrocarbon oil in amounts up to approximately 15% by weight, Aroclors 1248 and 1254 materially increase the load-carry ing properties without reducing the viscosity of the resulting composition. These Aroclors repre sent one of the more adequate carriers for the element chlorine as an extreme pressure base, possessing the following advantages: 1. Stability. They are stable, even at higher temperatures, which permits neither separation of components nor appreciable change in physical or chemical properties during long periods of operation and should not cause continued chem ical action on metal parts except the particular chemical metal surface combination which is nec essary to effect high load-carrying capacities. 2. Non-volatile. Many other types of chlorine bearing compounds are so volatile as to render them unfit for long periods of service because of the escape of the elements from the lubricant. The ; Aroclors are non-volatile at normal temperatures. 17 0221988 TOWOLDMONOQ26609 3. Non-oxidizing. Aroclors do not oxidize or thicken up to an objectionable degree. 4. Non-corrosivo. Aroclors are non-corrosive toward metal surfaces. 5. Non-abrasirr. Aroclors exert no abrasion on the machined surfaces. 6. Non-hydtolysi*. Aroclors do not hydrolyze in the presence of water, thus avoiding the genera tion of hydrochloric acid. 7. Conijmlibility. Aroclors are completely misci ble with mineral oils. 8. Color. Aroclors do not darken or change the color of the lubricating oil. Submerged Lubrication Under conditions of lubrication subjected to expo sure to water displacement such, for example, as lubrication of bridge rollers, a hcavier-thanwater lubricant can be prepared from mixtures of Aroclor and oil, of which the following arc typical examples: Mix No. <-% by Wt.-- Aroclor Oil* 124 Pour Point Gravity at )5.5C 1 50 50 0F 1.1263 2 25 75 +5F 1.2703 Bright Stock: Gravity API 22-23 Approx. Iba./gal. 9.4 10.6 Viscosity 210 F--160 Sayholt Secs. Color ASTM--'7-8 Flash Point--545F Pour Point--15F GASKETS AND PACKING MATERIALS Particularly in the use of Aroclors at elevated temperatures, as encountered in Aroclor heattransfer installations, and to a lesser extent in the use of Aroclors as hydraulic' media careful selec tion of gasket anti packing materials is required. Hot Aroclors plasticize anti swell "rubber** materials ineluding Ilyrar P. Koroseal. Perhunan anti Neoprene. Although materials of this type are used as gaskets in certain Aroclor installa tions. careful eonsiderution must Ik* given them in light of expected operating condition to assure that satisfactory performance will hr obtained. Thiokol is not attacked hy Aroclors at ordinary temperatures hut cannot he recommended for use with Aroclors at elevated temperatures. This is apparent from the following temperature ranges indicating the maximum temperature beyond which various types of Thiokol are not stable: Thiokol Type A..............150 to 200F. max. Thiokol Type FA........... 150 to 200F. max. Thiokol Type ST............250 to 300F. max. Kcsistoflex, polyvinyl alcohol, resists attack bv Aroclors but since tins polymer is soluble in water, its consideration for practical use involves drastic limitations where water or moisture must be considered. Silastic (Dow Coming's Silicone 180) is remark ably resistant to deterioration from contact with hot Aroclors and is suggested for gaskets. The follow ing changes in physical properties were noted when Silastic was immersed in Aroclor for seventy hours at 150C. 1. Hardness was lowered about 20 points. 2. Elasticity was improved several points. 3. Practically no change in tensile strength. 4. An appreciable increase in the ultimate elongation. Teflon (duPont's poly tetra fhioroethyleno) is not attacked by hot Aroclor (130C.) and is to be recommended as a gasket material. So far attempts to make Teflon diaphragms for valves have not been very successful in some cases because the Teflon seems to lack the desired flexibility. It is indicated that leather gaskets ami leather packing compositions arc satisfactory for use with Aroclors. Frequently, thin sheets of aluminum are used satisfactorily as gaskets at flanged joints. Garlock Packing Company's No. 7021, inch aslw'stos fiber shed is used at the flange connec tions in' several of Monsnnto*s Aroclor heatexchange units. Garlock's braided No. 117 packing is used in the valves and Garlock's No. 234 ma terial is used for packing the Aroclor pumps. Also, Durametallic Cor|K>ralion's Type B-7 Dura Plastic is used as packing for Aroclor pumps. It is also understood that Garloek No. 431 and Chet run No. 7050-C materials are satisfactory as 18 OZZ^89 TOWOLDMONOQ26610 packing. Likewise Durametailic's Spiral Asbestos Fiber may be used. Doubtless. Johns-Manville and others have comparable parking materials which would be suitable. The following materials are being used satisfac torily as pipe thread compounds in Aroclor units; 1. Plastic Lead Seal, Durametallic Corporation. 2. Ordinary white lead. 3. Glyptal No. 2, General Electric Company. DERMATOLOGY AND TOXICOLOGY Skin patch tests with a polyvinylchloride free film plasticized with 11.5 percent by weight of Aroclor 1254 (about 25 per cent based on the weight of the vinyl resin) and a similar amount of dioctyl phthalate showed that this film was not a pri mary irritant or a sensitizer. Also, skin patch tests on Aroclor 1254 alone applied to gauze and placed in contact with the skin showed no primary irritancy or sensitization. Other skin patch tests using canva6 coated with Aroclor 5460 and an oil modified alkyd resin, in such a manner that the Aroclor concentration in the paint film on the fabric was about 17 percent by weight of paint solids and the finished coated fabric contained approximately seven percent by weight of Aroclor 5460 showed that this painted fabric did not produce primary irritancy or sen sitization of the skin. If Aroclors are spilled on the skin, the skin should be washed in the usual manner witli soap solu tions. If accidental burns occur from contact with hot Aroclors, the burn should be treated the same as any ordinary burn. Aroclor adhering to the burned area need not be removed immediately unless treatment of the burn demands it, in which case use soap and water or repeated wasiiings with a vegetable oil. At ordinary temperatures Aroclors have not pre sented industrial toxicological problems. If Aroclors are used at elevated temperatures such as 200or 300 C. in open systems, methods must be designed to exhaust any vapors arising from these open systems. This applies especially to lower chlorinated Aroclors where experimental work on animals indicates that the maximum safe concentration of vapors in workrooms is in the range of 0.5 to 1.0 milligrams per cubic meter of air. In the case of more highly chlorinated Aroclors such as Aroclor 1268, the allowable limit is about 10 milligrams per cubic meter of air and accord ingly, Aroclors of this type are believed to be of a much lower order of toxicity. Where Aroclor vapors may be encountered in workrooms, local exhaust ventilation together with general workroom exhaust is recommended. 19 0221990 TOWOLDMONOQ26611 SUGGESTED USES FOR AROCLORS In PLASTICS, PIGMENTS, LACQUERS, PAINTS, VARNISHES and WAXES The Aroclors are compatible with most of the common plastics materials (see compatibility table on this page). The degree of flexibility imparted by the Aroclors diminishes progressively in the order of liquid Aroclor -- 6oft resin -- hard resin. The hardness of the resulting compositions increases in the same order. Usually a satisfactory balance between flexibility and hardness can be obtained either by selecting the Aroclor of proper physical characteristics or by using a mixture of two or more Aroclors. ETHYL CELLULOSE The Aroclors are very compatible with ethyl cel lulose, the liquids imparting great flexibility and the resinous products great hardness. 75 parts by weight of Aroclor 1242 with 100 parts of ethyl cellulose produces great flexibility and just a slight tackiness. Aroclor 5460 in the same propor tion produces a very hard and somewhat brittle composition. Aroclor 4465 produces hard films which are not brittle at ordinary temperature. Compatibility With Various Materials Asphalt........................................................ C Benzyl Cellulose......................................... C Carnauba Wax............................................ C Cellulose Acetate........................................ I Cellulose Aceto Butyrate.......................... C Chlorinated Rubber................................... C Coumarone and Indene Resins................. C Dammar Resin........................................... C Ester Gum.................................................. C Ethyl Cellulose....................................... C Manila Gum............................................... t Nitrocellulose............................................... C Paraffin........................................................ C Phenolic Resins........................................... Varies.* Polystyrene Resins..................................... C Polyiso-Butylcne........................................ C Rosin........................................................... C Rubber........................................................ C Sulfur.......................................................... C Styrene-Butadiene Co-polymers.................. C Vinyl Resins............................................... C C -- Indicates compatibility to a degree sufficient to be of value. I -- Indicates incompatibility. Not compatible in final stage. For coatings of high gloss and exceptional weath ering qualities to be applied to rigid surfaces, compositions containing equal parts by weight of Aroclor 5460 and ethyl cellulose are suggested. If greater flexibility is required, one of the softer Aroclors should be used, cither alone or as a replacement for part of the Aroclor 5460 and the proportion of Aroclor should be decreased. A typical formula is as follows: ! Ethyl Cellulose................................. .. 15% Aroclor 1260........................................... 15% Toluene.................................................... 56% Butanol................................................... 14% GRAPHIC ARTS 100% The Aroclors are used as vehicles for carrying pigments employed in glass decoration. When the decorations have been applied and the glass is fired, the Aroclors volatilize without carboniza tion and thus avoid discoloration of the glass. Aroclors 1254 and 4465 are used. Aroclor 4465 is a useful resin for compounding rotogravure inks. 20 OZ21"1 TOWOLDMONOQ26612 A mimeograph ink suitable for use on bond paper contains the following ingredients: Aroclor 4465 ........................................... 40% Lubricating Oil (SUV 1200 <> 100F).. 35% Paraffin Oil (SUV 76 @ 100F)............ 20% Carbon Black................................'____ 4% Oil Soluble Dye...................................... 1% Aroclor 4465 may also be used in the preparation of imitation gold leaf. A thin coating of the Aroclor is applied hot to one side of paper. While it is still hot, bronze powder is spread upon the coating. The bronze powder adheres to the Aroclor completely covering the paper. This product is used in making the "gold leaf* letters on books, etc. The paper treated with Aroclor and bronze powder is placed upon the book binding. A hot die is pressed upon it. The Aroclor softens and sticks the bronze to the binding and forms a coat ing over it to protect it from tarnishing. IMPREGNATION The Aroclors may be used to impregnate cloth, paper, wood or asbestos in order to impart mois ture and gas resistance, adhesion, insulating prop erties, alkali or other chemical resistance, flame resistance, or lubricating qualities. For this type of work they are used in combinations with other materials such as waxes, inorganic pigments, asphalt, tars, aluminum stearate, sulphur, etc., in order to obtain exactly the physical character istics desired for the specific purpose. Aroclors 1254, 4465 and 5460, or the corresponding darkcolored products, arc suggested as most applicable. Wood impregnated by vacuum-pressure method with the following mixture: Aroclor 4465...................................... 70% Microcrystalline Wax....................... 20% Sulfur..................................................10% is definitely tougher, harder and more moisture resistant than untreated wood. This coating is very resistant to acids and alkalies but will be attacked by aromatic, aliphatic or chlorinated hydrocarbons. The surface is not appreciably dis colored and can be painted. Various degrees of hardness and adhesion can be obtained by vary ing the Aroclor: wax: sulfur ratio. MOISTURE PROOFING For use as moisture proof coatings on wood, paper, concrete and brick, the Aroclors are best com bined with waxes, especially paraffin or carnauba, oils such as mineral oil or drying oils, and syn thetic resins including modified alkyds, phenolics, chlorinated rubber, polystyrene, styrene-buta diene co-polymers, ethylccllulosc, cellulose aceto butyrate, benzyl cellulose or vinyl resins. Selec tion of materials for use in combination with Aroclors will depend on the end use requirements of the specific application. The simplest compositions contain only Aroclor and paraffin. A moisture proofing compound com posed of 96% (by weight) of Aroclor 5460 and 4% of paraffin (melting point 54C) has an ASTM soft ening point of about 82 C and is very efficient. Substituting Aroclor 4465 for Aroclor 5460 pro duces a compound with a softening point of about 58C. Softening point and viscosity when melted may be further decreased by using mixtures of Aroclors. For example, a composition containing 40% of Aroclor 1260, 56% of Aroclor 5460 and 4% of paraffin will be very soft at ordinary temperatures. Increased proportions of paraffin will also pro duce softer compounds. PIGMENT Aroclor 1270 is a hard, white crystalline product of high melting point, insoluble in most solvents, resistant to chemicals and to oxidation. When ground to a fine powder it makes an excellent organic pigment for use will) the various plastics. It may be used alone or with conventional pigments. PAINTS AND VARNISHES The Aroclors arc soluble in paint and varnish oils and impart properties corresponding to the phys ical character of the particular Aroclor. The hard resinous Aroclors tend to give increased hardness to the films while the viscous resins imparl flexibility. 21 TOWOLDMONOQ26613 The Aroclors do not react chemically with oils, hence there is no advantage in heating together in making a varnish. They are best added as a "chill hack*' or as a cold cut in the thinning operation. As far as incorporation of the Aroclors is con cerned, the only reason for heating is to make the Aroclors liquid so that they can be readily mixed with the oils. Aroclors 446S and 5460 will produce paints that are very quick drying and yet have excellent durability. The weight of Aroclor used should be from 30% to 50% of the weight of the oils. Aroclor 1260 is best for short oil varnishes that are required at the same time to be flexible. The Aroclor may be considered to play the same role as oil, uifh the difference that it does not oxidize and lose its flexibility on exposure. Resins of the alkyd. phenolic or ester gum type, or a harder Aroclor such as 5460, may be used in making varnish formulations. It is suggested that for two parts by weight of oil, one part of Aroclor 1260 and one part of other resin be used. These pro portions can be varied as required. The Aroclors impart water and alkali resistance and in these qualities enhance the value of the other resins used in the varnish. Aroclors arc excellent grinding and dispersing media for pigments used in paints and varnishes. Aroelor 1254 is used to disperse aluminum powder in a paste form which can he incorporated easily into paints and varnishes. The Aroclor imparts exeellent leafing qualities, brightness or luster and docs not tarnish the aluminum pigment on aging. Moreover, the composition does not support com bustion. RUBBER AND RUBBER SUBSTITUTES The liquid Aroclors, 1221. 1232, 1242 and 1218 have a strong plasticizing action on rubber, both natural and synthetic. Aroclors 1254 and 1260 are milled into rubber in order to impart perma nent tackiness and adhesion. A small amount of Aroclor 1200 added to hard rubber acts as a plasticizer ami reduces the brittleness. Aroclor 1270, being a bard crvstaliiuc material of high inching point, can be ground to a powder and then milled into rubber. The milling tem perature being below the melting point of the Aroclor, the latter is dispersed through the mass of rubber and acts as an efficient flame reducer. This same procedure can be used with synthetic .rubbers to impart fireproofness. From 5% to 25% of Aroclor 1270 based on the weight of the resin is required. Aroclor 1262 is recommended as a plasticizer for crepe rubber resin in paint compositions. Used in concentrations of 5% to 50%, based on the weight of the ruhber resin, it increases the gloss and alkali resistance of the film and increases its ad hesiveness toward steel. Aroclor 1268 used at a level of about three pounds per 200 pounds of Neoprene has excellent working qualities as a plasticizer at 225-325F. in injec tion moldings. MODIFIED RUBBER FINISHES Chlorinated rubber (Parlon) and copolymers of styrene-butadiene (Pliolite S-5) are used widely as protective and decorative coatings for concrete and masonry structures, steel structures, railway tank and gondola cars, wood and metal maritime equipment. Aroclor 1254 is used as a plasticizer and Aroclor 5460 is used as a resin fortifier in these coatings which are used where flame resistance, corrosion resistance, chemical resistance, i.e., resistance to acids, alkalies and water and good electrical insu lating properties are required. The use of Aroclors in making these protective coatings is described in Monsanto Technical Bul letin No. P-124, "Aroclors as Used in Chlorinated Rubber," and Monsanto Technical Bulletin No. P-126, "Aroclors as Used in Pliolite S-5." VINYL RESINS The Aroclors are compatible with all the vinyl resins and are used mainly as co-plasticizers with tricrcsyl phosphate, dioctyl phthalate, dibuty) phthalatc and other plasticizers for vinyls to im part good plasticizing action, chemical and corro sion resistance ami excellent electrical properties at a substantial reduction in cost. This use of Aroclors is described in Monsanto Techniral Bulletin No. P-131, "Aroclors as Co Plasticizers for Polyvinylchloride" and Technical Bulletin No. P-134, "Aroclor 1251 Co-Plasticizer with 1)01* for Vinyl Organosols and Pastes." 22 TOWOLDMONOQ26614 Aroclor plasticizers are very attractive for use with dioctyl phthaiate in preparing organosols, plastisols or pastes of vinyl plastics used for making free films, textile coatings and coatings for paper. In many of these applications the fire-resistant quality of Aroclors is important. Also, the Aroclors serve as excellent media for grinding and dispers ing the pigments used. It is interesting to note that the vaporization rates of Aroclors, especially Aroclors 1254 and 1260 which are the most widely used members of the Aroclor family in the vinyl plasticizer field, com pare most favorably with the similar constants of other commonlv used vinvl plasticizers. (See Table VII, Page 14.) It is also important to note that a free film made up of polyvinylchloride containing 11.5 percent by weight of Aroclor 1254 and a similar amount of dioctyi phthaiate along with standard white pig ments was found free from irritating or sensitizing the skin in accordance with commonly used skin patch tests. Moreover, similar studies made with Aroclor 1254 alone indicate that this plasticizer is neither a 6kin irritant nor sensitizer. While this indicates safety in using Aroclor 1254, the use of the plasticizer is not suggested for such items as baby pants or other items that are intimately in contact with the skin. Another excellent use for Aroclors in vinyl plastics is in the preparation of adhesives. The Aroclors imparl outstanding adhesive qualities and give good resistance against water and corrosive in fluences. Moreover, the Aroclors are resistant against organism attack and when used in com bination w ith other properly selected ingredients, vinyl adhesives can he prepared which strongly resist attack hv organisms. NITROCELLULOSE COATINGS The Aroclors function both as plasticizers ami resins and may he used alone with the nitro cellulose or in combinations with other plasti cizers or resins. They impart weather resistance, luster, adhesion and decreased hurtling rate. Their excellent electrical characteristics (high dielectric strength ami resistivity ami low power factor) and their property of retarding the passage of moisture and gases through nitrocellulose, chlorinated rub ber, and other similar plastics films make the Aroclors of special value in coatings for electrical insulating materials. The accompanying trilinear diagrams show the practical compatibility limits of Aroclors 1254 and 1262 when used in conjunction with some other resins and plasticizers. Aroclor 1260 gives values almost the same as those shown for 1262. The less viscous Aroclors have greater and the more res inous ArocLrs less compatibility than for those shown. (See trilinear diagrams that follow.) To illustrate the differences possible to obtain by changes in formulation, three formulas are given below'. All have excellent durability but the third is much softer and more flexible than the other two. Only the solids contents are given. The amounts tabulated arc parts by weight. Aroclor Lacquers No. 1 y2 second Nitrocellulose (dry)i 100 Dammar resin....................... 80 Ester Gum............................. -- Aroclor 1260.......................... 20-39 Dibutyl Phthaiate................ 20- 0 Tricresyl Phosphate............. No. 2 100 -- 80 20 _20 No 3 100 -- -- 80-70 -- 39-70 No. 1 and No. 2 have excellent sanding and polishing qualities. No. 3 is very flexible but too soft for sanding. Where extremely high flexibility is desired, as for example in lacquers for high tension automotive cables, the following composition is suggested: 15 -- 20 sec. U. S. Nitrocellulose....................... 100 parts by weight Tricresyl Phosphate............. 120 parts by weight Aroclor 1242......................... 80 parts by w-eight WAXES The use of Aroclors to extend or substitute Carnauba Wax and reduce the cost of the wax formu lation is described in Bulletin No. P-132. This bulletin gives several practical formulas using Aroclors in wax blends possessing the qualities of Carnauba Wax for automobile, wood, leather and linoleum polishes. Selected Aroclors such as 5460 used in conjunction with various waxes make excellent impregnating compounds for furniture drawers, etc., to prevent sticking. Resinous Aroclors used in combination with waxes make excellent and inexpensive sealers for concrete and masonry surfaces, wood, fiber board and paper products. 23 0*2199* TOWOLDMONOQ26615 DIAGRAMS SHOWING PRACTICAL COMPOSITION OF LACQUERS USING AROCLORS 1254 AND 1262 In the trilincar diagrams tiic compositions, represented by any point in the unshaded areas, are those which produce homogeneous lacquer films. On the other hand compositions represented by points in the shaded areas produce impractical, segregated, brittle or soft films. For detailed information as to the derivation and use of these diagrams reference is made to the following articles: Jenkins & Foster, "Compatibility Relationships of the Aroclors in Nitrocellulose Lacquers," Ind. Eng. Chem. 23, 1362 (1931). Hofmann & Reid, "Graphical Methods in Lacquer Technology," Ind. Eng. Chem. 20, 431 (1928); "Formulation of Nitrocellulose Lacquers," Ind. Eng. Chem. 20, 68? (1928). 24 0221'*^ TOWOLDMONOQ26616 For romltinaliima wlirrr ihe train ii* of lit** philmlir anliyririilr-plyrrro! ly|*r am! wlirrr the Aroclor it Aroclor 1251. 25 02 2l'*gb TOWOLDMONOQ26617 Practical Composition of Lacquers using Aroclors 1254 and 1262 -- (cn>l>4d) Pt*ce*r''9Q \q AeOCLO/? 00 For combinations where the Arorlor resin is Aroclor 1262* ami where the plasticizer is Dibulyl l'hthalutc. For combinations where the Aroclor resin is Aroclor 1262* am) where the plasticizer is Tricrcayl Phosphate. 26 0221997 l TOWOLDMONOQ26618 Other Literature on Arodor Applications Monsanto Technical Bulletin P-115 THE AROCLORS Monsanto Technical Bulletin P-12'1 AROCI.ORS AS USED IN CHLORINATED RUBBER Monsanto Technical Bulletin P-126 AROCLORS AS USED IN PL10LITE S-5 Monsanto Technical Bulletin P-128 AROCLOR -- INCOMBUSTIBLE LUBRICANTS USED IN HIGHPRESSURE COMPRESSORS Monsanto Technical Bulletin P-130 AN INDIRECT AROCLOR HEATER FOR UNIT CHEMICAL OPERATIONS Monsanto Technical Bulletin P-131 AROCLORS AS CO-PLASTICIZERS FOR POLYVINYLCHLORIDE Monsanto Technical Bulletin P-132 AROCLORS AS USED TO EXTEND OR SUBSTITUTE CARNAUBA WAX Monsanto Technical Bulletin P-134 AROCLOR 1254 CO-PLASTICIZER WITH DOP FOR VINYL ORGANOSOLS AND PASTES Monsanto Technical Bulletin P-137 AROCLOR--A NONFLAMMABLE . HYDRAULIC FLUID FOR DIE-CASTING SYSTEMS 1- IS&-OS-S3-S2M 71 27 rrinli'ti in I'.S A. 0221998 TOWOLDMONOQ26619 The information contained in this booklet has been obtained from sources which we believe to be reliable and dependable, but we cannot guarantee the correctness of the same or be responsible for any loss or damage that results from the use of such information. MONSANTO CHEMICAL COMPANY ST. LOUIS, MO. 0231999 TOWOLDMONOQ26620