Document JN8x3YaOgqeOnMYy0oJ7DwXYO

PLAINTIFF'S EXHIBIT UNITED STATES GYPSUM COMPANY 300 West Adams Street, Chicago 6, Illinois --------- J GP027 0013 TABLE OF CONTENTS Plaster Bases Bosecoat Plotters Finishing Plasters Rocklath Lathing Systems Metal Lathing Systems Plaster Problems and Remedies How to Inspect a Plaster Job i PAGE 9 31 43 57 75 87 101 Gypsum...the basic material for lathing and plastering What U Gypsum? Gypsum is one of the most common minerals of the earth. Xonmetallic. it is usually in the form of grey or white rock, found in veins varying from a few feet to 20 and 30 feet in thickness. Chemically. g> psurn is a mineral composed of calcium sulphate combined with water of crystallization. This "dry" water makes up approximately 20 percent of the weight of raw gypsum rock, and it is this feature which gives g\ psum its Are-protective qualities and makes it so adaptable lor the manutacture of building materials. 5 J GP027 0020 1 How Gypsum is Processed Auer gypsum is mined or quarried, it is crushed and ground and then calcined (or cooked) to remove the greater part of the chemically combined water. This calcined product, or Plaster of Paris, is the basic ingredient of all gypsum materials. Com bined with other materials and water, it is used for the manu facture of gypsum lath, partition tile and gypsum plasters. When it is mixed with water to make gypsum lath or to make a plaster mix on the job, it re-absorbs the water removed in proc essing and reverts to gypsum rock. This recombination with water is why gypsum materials give such excellent fire protec tion to buildings. 6 J GP027 0021 How Gypsum Protects Against Fire When fire heats a gypsum wall or ceiling to about 212 F.. the water of crystallization is gradually converted into steam. The water of crystallization effectively retards the spread of flame. For instance, in an average room 10 feet square finished with gypsum lath and plaster, the heat of a fire could convert the water of crystallization in the gypsum into sufficient steam to fill the room three times. The back of the gypsum wall will not be much hotter than 212 F. until all the water is gone-- a slow process. This protects the wood framing, which doesn't start to burn until about 400 F. Setting Action of Gypsum Water is added to gypsum plaster on the job until the material is sufficiently plastic to spread easily under the trowel. After it is applied, the gypsum particles re-absorb part of the water from the mix and the plaster reverts through crystallization to the chemical form it originally had uhen taken from the ground. Giant rotary calmer in which crushed gypsum is cooked. GP027 0022 The balance of the mixing water is dried out of the plaster slab through ventilation and evaporation. When crystals begin to form in gypsum plaster, it starts to harden; this is known as the '`setting action" of gypsum. Gypsum which has been calcined begins to set soon after water is added. RED TOP-Stabilized Set Mill addition of special ingredients developed by USG Research has resulted in the famous '`Stabilized Set" of all Red Top plasters. Red Top minimizes variability in sets often caused by sand and water impurities which would accelerate or retard the set of ordinary plaster. Whether machine or hand mixed-- applied over metal, wood, gypsum, insulating lath, cement block, brick, clay or gypsum tile--a scratch or brown coat of Red Top mixed with sand or lightweight aggregates (vermiculite, perlite) sets more uniformly. It also sets to more uniform hardness, providing a better surface for application of white coat. The set progresses evenly from the base out to the surface. Why gypsum is better for building In addition to its outstanding fire-protective qualities, the mineral gypsum will not rot nor decay and combines light weight with strength. It builds durable walls that last a lifetime, and may be economically adapted to any architectural design. GP027 0023 Plaster Bases ROCKIATH plaster base PYROBAR and otfiar Masonry Plaster Basas USG COLOR-RITE Metal Lath and Accessaries PAGE 10 17 21 Proper use and application of USG plaster bases is important in the construction of strong durable finished walls and ceilings. A secure bond between the plaster and plaster base is essen tial to develop strength and resistance to abuse and cracking. Gypsum plaster adheres to a plaster base because a bond is developed which virtually makes the two materials a solid unit. A "mechanical" bond is formed when plaster is pressed through the mesh or holes of the lath, forming keys on the other side. The keys actually "rivet" the plaster and lath together. This mechanical bond results when plastering over metal lath or perforated gypsum lath. A "suction" bond is formed when gypsum plaster is applied over gypsum lath, and masonry bases. In this case the tiny needle-like plaster crystals penetrate into the surface pores of the base by suction. When the piaster sets, the base becomes "welded" to the plaster. When perforated gypsum lath is used, both suction and mechanical bonds are developed. 9 GP027 002A ROCKLATH Plaster Bases Plain ROCKLATH Plaster Base is a gypsum lath made in sheet form in thicknesses of } g in. and L> in. It consists or a core of gypsum pressed and rolled between two layers of special absorptive paper, and is the standard of excel lence for receiving gypsum base coat plaster. ADVANTAGES Fireproof--Rocklath has an incom bustible gypsum core and will not transmit temperatures much over 212 degrees F. until completely cal cined. Resistant to Sound Transmission-- Wood stud partitions with Rocklath and gypsum piaster on both sides have a high resistance to sound transmission. (See Rocklath Resili ent System 60 for higher sound transmission resistance.) Strong Bond--Gypsum plaster bonds to Rocklath with a safety factor of 144--far higher than required to meet usual construction standards. Structurally Strong--Large units add resistance to racking of framing members. Durable--Not harmfully affected by decay, dry rot or normal moisture. Will not attract vermin. Economical--The low cost of Rock lath, its ease and speed of erection and savings in plastering are out standing. LIMITATIONS OF USE 1. Gypsum lath, T9 in. thick, is de signed for supports not to exceed 16 in. o.c. For framing spaced more than 16 in. o.c. but not more than 24 in. o.c., } :> in. thick Rocklath should be used. 2. L'se with gypsum plaster only. Bond between lime or portland cement plaster and Rocklath is inadequate. 3. Gypsum lath and plaster, painted with 3 coats ot lead and oil, has a vapor permeability of about Perms (grains of water per square foot per hour per inch of mercury vapor pressure difference). For higher resistance to vapor transmission, use Insulating Rocklath plaster base. 4. Do not use in areas exposed to excessive moisture for long periods of time. Use galvanized metal lath and portland cement-lime plaster. 5. Where one hour fire resistive rat ings are required, Perforated Rock lath plaster base should be used. Perforated ROCKLATH is identical to plain Rocklath ex cept that in. round holes are punched through the lath 4 in. o.c. These perforations allow the applied plaster to "mushroom" through the GP027 0025 10 holes and form "rivets" to mechani cally key the plaster to the Rocklath, providing both mechanical and suction bonds. ADVANTAGES Same as plain Rocklath but with higher fire rating. Gives one hour fire rating on partitions with 1 <> in. gyp sum plaster sanded 1:2-1:2 by weight, or gypsum-perlite plaster 100 lbs. to 2H cu- ft. and a one hour rating on ceilings, with >-$' gypsum-perlite plaster proportioned 100:2 LIMITATIONS OF USE Same as for plain Rocklath plaster base, except perforated Rocklath should not be used on ceilings with Resilient Rocklath clips or other side suspended clip systems. Insulating ROCKLATH is manufactured with a sheet of bright aluminum foil laminated to the back of plain Rocklath. It pro vides insulation against heat and cold and is an effective vapor barrier. ADVANTAGES All those of plain Rocklath plus: 1. Insulating value equal to in. fiber insulation board when installed with at least % inch air space next to foil. 2. Aluminum foil is one of the best vapor barriers known and used com mercially. 3. Economical--one material, one application provides plaster base, insulation, vapor barrier. LIMITATIONS OF USE Same as plain Rocklath plaster base. Use only on the interior of exterior walls and top door ceilings. IMPORTANT When Insulating Rocklath is in stalled with at least a in. air space next to the foil, it has the same insulating value as a half inch of fiber insulating board. An efficient vapor barrier should be installed in all exterior walls and ceilings where freezing weather oc curs for extended periods of time. The vapor barrier should be located on the warm side of the exterior wall or top floor ceiling. GP027 0026 11 PARTITIONS CP027 0027 TECHNICAL DATA Wood Frame Construction Construction Plain ROCKLATH nail-on 2' x 4' studs. Total Weight Lbs. per $q. Ft. lath and Plaster Only 12.0 Gypsum-Sand 1(2 --1:2 Thickness Fire Rating Reference Sound Transmission Loss ft 'h' 45 min. (1) 41 (1) tt* Plain ROCKLATH noil-on, 2* x 4* studs. 11.0 Wood fiber plaster Vi' 1 hr. (1) 41 (2) tt' Perforated ROCKLATH nail-on, 2* x 4" studs. 12.0 Gypsum-Sand 1:2--1:2 Vi' 1 hr. (1) 41 (2) %' Perforated ROCKLATH nail-on, 2* x 4' studs. 8.0 Gypsum-Perlite 100:2'/* >/,' 1 hr. Ill ft' Perforated ROCKLATH nail-on, 2' x 4* studs. 8.0 Gypsum-Vermiculite 100:2 V* 56* 1 hr. (1) *"T - I CEILINGS :i-- $" Perforated ROCKLATH nailed to 2* % 10* wood joists with J/W* headed nail*. V*' sub floor--diophragm of asbestos paper--T&G finished floor 6.0 Gypsum-Sand 1:2--1:2 '/i' 30 min. (1) Same as obove except noils had head. 6.0 Gypsum-Sand 1:2--1.-2 Vi' 4 5 mtn. (1) %* Perforated ROCKLATH nailed to 2* it 10' wood joists with %' headed noils (S per lath per joist). Striploth applied to joists with nails having '/]* head. 6.0 Gypsum-Sand 1:2-- 1:2 'h" 1 hr. (I| W Perforated ROCKLATH nailed to 2* x 10' wood joists with >'4/ head nails-- 4 per loth per joist. 4.0 Gypsum-Perlite 100:2'/] Gypsum.Vermiculite 100-2`/a Viw <A' 1 hr. (I) 1 hr. Ill V%* Plain ROCKLATH nailed to 2' x 10" wood joists with 'Us* head nails-- 4 per lath per joist-- 20 go. 1* hex. wire mesh nailed to joists through loth. 4.0 Gypsum-Perlite 100:2'/] ( fj National Bureau of Standard* BMS 92. (2) Estimated to be tame at plain ROCKLATH Plaster Bose with sanded plaster. Vi' I'/l hr. (1) 8200 IZOdO I ROCKLAIH Plaster Base Typf-- R*commndd Stud Spacing--Special Uiat Stud Spacing far thtckna** indicofad 1 TYPES sizes % 'A" COMMENTS | Plain H', 'A' thick 16'x48' 16' o.c 24' o.c V\* ROCKLATH is particularly adaptable to nailable steel framing spaced 24* o.c Perforated* H', 'A" thick 16' x 48' 16' o.c 16' o.c Required for higher tire rating Insulating H', 'A` thick 16' x 48' 16'o.c 24' o.c Recommended for side walls and top floor ceilings for inswlotion and os a vapor barrier. Ploin Long length V-edgo Vi* thick 24* wide by ceiling height up to \ 2' For constructing 2* Solid ROCKLATH and ploster partitions. (See page 65.) Insulating long length Squore Edge %' thick 24* wide by ceiling heights up to 1 2'. For application to exterior masonry walls using USG Wall Furring (rackets and %* channels. (See page 68.) `Perforated ROCKLATH if not recommended for cerling applications whan sido-tutponsion clip ottochmonts ore used. O -o Q IN* o o fs 14 >0 FIG. 1 (Ashlar pattern) Sidewall and Ceiling Application Apply 16x48 in. ROCKLATH with stag gered end joints on studs or joists, spaced 16 in. o.c Appiy 4 nails par board par support---space approximately 5 in. apart, H in, from edges and ends. FIG. 2. Alternate Ceiling Application (Canadian system) GP027 0030 Long Length ROCKLATH plaster base }A in. thick, 24 in. wide with V edges is used to construct 2 in. Solid Rocklath and plaster partitions. (See page 65.) Long Length Insulating Rocklath, 3 $ in. thick, is used as an economical fur ring application tor exterior masonry walls, providing ease of erection, insulation and an excellent vapor barrier (5ee page 68). ADVANTAGES The same fire protection as other Rocklath plaster bases of corre sponding thickness, as well as econ omy and ease of application. APPLICATION of ROCKLATH Proper Noils--For 2 $ in. ROCKLATH. nails should be l'-j in.. 13 gauge blued, `?i in. flat head, smooth dia mond point. For 11 in. lath, use l14 in. length. For nailable steel fram ing (spaced not more than 24 in. o.c.) use nails of proper gauge with not less than 3/j in. heads and long enough to develop the proper nail holding of the framing. Nailing (Sidewalls and ceilings) -- Space nails approximately ? $ in. from the edges and ends, approx imately 5 in. apart, using four nails per lath per support. For ) > in. Rocklath with supports more than 16 in. o.c., nails must be spaced ap proximately 4 in. apart using 5 nails per lath per support. For a one hour ceiling fire rating when using sand as the aggregate, 5 nails per lath per support plus striplath on joints must be used. 16 Sidewall and Ceiling Application-- Rocklath plaster base should al ways be applied face out with the long dimensions at right angles to the framing members. On walls, end joints should fall on different sup ports in adjacent courses. On ceil ings, end joints are staggered as for side walls (See Fig. 1) or Rocklath should be erected so that end joints are made continuous on a support, in which case end joints must be covered with 3 in. striplath and the long or edge joint offset or staggered (See Fig. 2). In all cases, Rocklath joints should be butted together. Cornerite and Corner Bead Appli cation-- Inside corners should be re inforced over Rocklath plaster base with cornerite. Staple cornerite to the lath to retain position until plastered. Corner bead should be stapled to exterior corners. -5 0 ^ C n J p ^ 7r <7> ^^ and Other Masonry Plaster Bases PYROBAR Gypsum Portition Til*--A precast gypsum tile tor building non-load bearing fireproof partitions, either in new construction or alteration work. Because it is made of gypsum, it has a strong natural bond with gypsum basecoat plaster. Pyrobar is avail able in several types and thicknesses (See chart, pa%e 19), ADVANTAGES Fireproof--3 in. hollow Pyrobar plastered two sides has 3 hour fire rating. 4 in. hollow Pyrobar plas tered two sides has 4 hour fire rating. Lightweight--30 to 50^ lighter than other commonly used masonry units. Platter Bond--safety factor of 173. Saves Platter--large size, machine moulded units lay accurately to form a level surface, requiring less plaster as compared with other masonry units. Sound Resistant--3 inch hollow Pyrobar plastered two sides has a sound transmission loss rating of 39.2 decibels. 4 inch hollow Pyrobar plastered two sides has a rating of 42.8 decibels. Ratings in excess of 50 decibels are obtainable with resilient lath and plaster facings on one side of Pyrobar tile, normal plastering on the opposite side. Economical--low material cost . . . goes up fast . . . fewer joints, saves up to 20*^ of plaster and up to 40^ of mortar. .. easy to cut, less waste. LIMITATIONS OF USE 1. Do not use Pyrobar for load bearing construction. 2. Portland cement and lime mor tars do not bond adequately with Pyrobar. Cse Red Top Partition Tile Cement. 3. Do not use portland cement or lime plasters over Pyrobar. Cse Red Top Cement Plaster. Before applying portland cement bedding for ceramic tile, nail or staple metal lath to Pyrobar. Other types o masonry, such as structural clay tilt also may be used as backing fot ceramic tile. 4. Where concrete floor fill, grano lithic finish, terrazzo or other wet types of riooring or base materials are to be applied to the rough floor construction subsequent to installa tion of Pyrobar tile, a continuous coating of asphaltic material shall be applied from rough floor up to height of wet application on tile. 17 GPOZ7 0 0 3 2 LINTEL SCHEDULE: 1INOU TIU imm IINTOCIS STMUM TIU lINTtl ANOll Ol CMANNH imm DIRECTIONS FOR ERECTING Mortar Requirement*: use Red Top Partition Tile Cement. Mix 1 part cement with 3 parts sand by weight. Mortar must not be retempered. Erection: after door bucks are erected and rough plumbing and wiring are in place, lay the first course, with core holes horizontally, by bedding in mortar to a true and straight line. Lay succeeding courses in approxi mately 12 in. thick mortar beds, uni formly level in each course, and with vertical joints staggered. Cut all joints flush. Anchor partitions to intersecting masonry walls 12J. 2 in. 0. c. vertically, with corrugated wall ties or 16d or 20d cut nails in mortar joints. Wedge tightly at ceiling and slush all chinks and crevices full u ith mortar. 18 Anchor wood door bucks to the Pyrobar with 16d cut nails or three buck ties each side (approximately 12 in. from top and bottom and at center) laid in the mortar joints. Lin tel construction (See above) should be held about J s in. above head of wood buck and not slushed with mortar. Anchor steel door frames with proper ties, minimum of three each side (approximately 12 in. from top and bottom and at center), in mortar joints and slush space between tile and hollow frame with mortar. APPLICATION OF BASECOAT PLASTER Apply Red Top Cement Plaster mixed with 3 parts of sand by weight or 3 cu. ft. lightweight aggregate per 100 lbs. plaster to j s'' grounds. (See Page jj.) ^ C ^ g * u <? <? . / ) /7 Other Masonry Bases Clay Tile and Brick--materials pro duced by exposing a clay putty to extreme heat until hardening has taken place. Clay tile is produced in 12.\- 12 in. size in thicknesses usually 2 to 6 in. with scored faces. Concrete Block--precast in molds using a slurry composed of cemen titious materials and an aggregate. It is generally produced in 8 x 16 in. size in thicknesses usually 3 to 12 in. and must have rough, porous faces. Such units must be properly cured to minimize volume changes during and subsequent to plastering. These masonry plaster bases are available in units for constructing interior bearing and non-loadbear ing partitions and should be used as a backup for ceramic tile, terrazzo and cement bases. Portland cementlime sand mortar is generally used for laying up, although Red Top Partition Tile Cement can be used where construction will not be ex posed to undue wetting. They are 60-80^ heavier in weight than Pyrobar Partition Tile, and thickness for thickness, have a lower tire resistance rating. Gypsum plaster may be applied di rect to these units providing the surface is porous to develop proper suction or scored to develop ade quate mechanical bond with plaster. Monolithic Concrete--many multi ple story fireproof buildings are constructed of poured reinforced concrete. Frequently, specifications require application of plaster basecoats direct to the concrete. It is important, in order to secure proper bond between the concrete and gypsum plaster, that specifica tions for this particular application he strictly adhered to. (Jcc puge jg). PYROBAR Partition Tile Data Six* of PYROBAR Portition Tile Limiting Partition Height Approximate Weight per *q. ft. Tile Partition Tile Cement Required per M sq. ft. Tile 2x 12x30 in. solid 3x12x30 in. hollow 4x 12x30 in. hollow 6x 12x30 in. hollow 10 ft. 13 ft. 17 ft. 30 ft. 10 lbs. 10 lbs. 13 lbs. 20 lbs. 500 lbs. 700 lbs. 900 lbs. 1300 lbs. GP027 0034 19 J c,tOO i.Z d0 USG COLOR-RITE METAL LATH USG Color-Rjte Metal Lath is rustresisting copper alloy sheet steel, slit and expanded to form a multitude of small mesh openings. It is further protected by dipping the expanded sheet into black asphaltum paint. (Exception: 3.4 lb. diamond mesh when made from galvanized sheets.) ADVANTAGES OF USG COLOR-RITE METAL LATH 1. Strength and Reinforcing -- Metal lath embedded within the plas ter provides strength in a manner similar to steel reinforcement in con crete slabs, thus providing high resistance to transverse impact. It decreases the hazards of serious cracks and failures due to structural movement of the frame. 2. Flaxibl*--Readily shaped to or namental contours to a degree not possible with other plaster bases. 3. Quality Plastaring--It makes the use of over-aggregated plaster in the scratch coat impractical. 4. Economy--Intended for highest quality, fire resistant, durable plas tering with low maintenance costs. 5. Fire Resilience--Metal lath and gypsum plaster provide high fire ratings. USG COLOR MARKING SYSTEM USG Color-Rite Metal Lath is the newest development in the metal lath industry. Ends of bundles are spray painted red for all 3.4 lb. lath, white for 2.5 lb. diamond mesh and 2.75 lb. }/$ riblath, yellow for 4.0 lb. Y" riblath. This makes warehousing, inventory and job distribution easier and positive. An architect may quickly and visually inspect a job to make sure the weight lath he speci fied is used. When the lather erects the colored end to the right as we recommend, the plasterer saves up to oercent of the scratch coat; saves time and effort because of the uniform "drag" on his trowel since all sheets lay in the same direction. 21 USG COLOR-RITE 3/8 in. Riblath Size: 27 in. x 96 in. A herringbone potter* mesh with in. deep V-shopod ribs running lengthwise of the sheet of Ay/\ in. intervols, with invert* ed infermediofe in. ribs. The heavy ribs provide exceptional rigid ity. Used when supports ore spaced more than 16 in. o.c. and not more than 24 in. o.c. and for 2 inch solid (sfudless) partitions. Desirable as a plaster base for heavy duty plastering. Used os centering and reinforcement for concrete floor and roof slabs. Weights: 3.4 lbs. (End Painted Red) and 4.0 lbs. (End Painted Yellow) per yard. Limitations of Use--Its extreme rigidity makes Vt in. Rib-lath un suitable for contour lathing. Use Diamond Mesh Lath. GP027 0037 USG COLOR-RITE 4-Mesh Z-Riblath Size: 27 in. x 96 in. A "flat rib" fyp. of loth with imoll.r m.*h op.nings. An ..c.ll.flt nail-on lath, or for tit-on work on flat coiling.. Weights: 2.75 lbs. (End Painted White) and 3.4 lbs. (End Painted Red) per square yard. Limitations of Use--Use Dia mond Mesh lath for contour plas tering. 23 US6 COLOR-RITE Diamond Mesh Lath Six*: 27 in. x 96 in. A small moih (approximately 11,000 mtihit per yard) diamond pattern metal plastering base. A general all purpose lath. Best tor orna mental, contour plastering. The small meshes conserve plaster and reduce drop pings. Weights: 2.5 lbs. (End Painted White) and 3.4 lbs. (End Painted Red) per square yard. Galvanized available in 3.4 lb. weight only. Limitations of Use--Specify "self-furring" for use as stucco base and 3.4 lb. galvanized where additional corrosion resistance is required. Also an ideal plaster base for lathing over old plaster surfaces. USG COLOR-RITE 1/8 in. Riblath (Flat Riblath) Siio: 24 in. x 96 in. A horringbono mosh pattern, with Vs in. doop Z-shopod ribs running longthwiso o# ths shoot of I Vi in. intorvois. Stiffening ribs and herringbone pattern increase rigidity, thus per mitting a wider spacing of sup ports or a saving in the weight of lath required. Particularly suitable for attachment by nailing. Small meshes conserve plaster materials. Weights: 2.75 lbs. (End Painted White) and 3.4 lbs. (End Painted Red) per square yard. Limitations of Use--Its rigidity makes it unsuitable for contour lathing. Use Diamond Mesh. { 22 n <n r f t n .j -o^ STRUCTURAL AND TRIM ACCESSORIES 24 1 USG offers a complete line of cessories. All beads, base screeds arv picture mould made from 26 gavig, galvanized steel. 1 -A Expanded Corner Bead--1[ wide expanded flanges are easil, flexed. Preferred for irregular coi ners. Provides increased reinforct ment close to nose of bead. 4- A Flexible Corner Bead--Tht general purpose corner bead. Eco. nomical and most generally used. By snipping flanges, this bead may b, bent to any curved design (for arch, ways, telephone niches, etc.). 5- A Bull Nose Corner Bead--4 % in. radius bull nose bead with short flange. Used for rounded cor. ners. Can be secured to corners with N'o. 9-A Corner Bead Clips attached to flanges, where wide nailing flanges are required. 10-A Expanded Bull Note Corner Bead--A bull nose bead similar to above, but with 2Yi in. wide expanded flanges. Especially suitable on corners where plaster base is uneven. 3-A Expanded Flange Bate Screed-- A flush type Y in. ground (job shimmed to % inch grounds) with wide flexible expanded flanges for added reinforcement or for attach ment to uneven surfaces. Used as a dividing point between plastered sur faces and Portland cement base. 6- A Plain Bate Screed--A flush type Yi in. ground (job shimmed for % in. grounds), used at the juncture of different finishes. 7- A Curved Point Bate Screed-- For use where base or wainscot is to project beyond the plastered surface. Made for in. plaster ground (job shimmed for % in. grounds) with Vi in. projection for base or wainscot. " t C f ( * ' 'S V /) 8-A Picture Mould--A concealed mould. Attached to lath and plas tered flush to the slotted opening. Grounds 12 in. Cjob shimmed for \ in. grounds). USG 1 in. Partition Terminal--For use as a vertical partition terminal for 2 inch solid metal lath or Rockiath partitions, or as a runner where 2 inch partitions abut an unplastered surface. Cap is of 18 gauge steel welded toa 24 gauge punched runner. Standard length 8'-2". Prime coated. Lathing Chonneli--Strong, light weight cold rolled channel sections used tor furring, suspended ceilings, partitions,etc. Sizes: % in.or IA2 in., 16 ft. or 20 ft. lengths. Weights: in. 300 lbs. per M Lin. Ft., 1*5 in., 514 lbs. per M Lin. Ft. Made of 16 gauge steel, black asphaltum painted. USG Solv-Edge Cornorito and Striplath--Cornerite is a 4 in. or 6 in. wide strip of 2.5 lb. copper alloy painted diamond mesh lath, bent to form a 100 angle, length 96 in, Striplath is a 4 in. or 6 in. wide strip of 2.5 !b diamond mesh lath, copper alloy, painted, 96 in. long. Motol Door and Window Cosing Beads--Used as a plaster stop and ground at window and door open ings, eliminating wood trim. No. Type Flange 4 quarter round expanded 138 quarter round short 60 semi square short or exp. 66 square short or exp. iiO d 'J All expanded flange casings avail able in }'n" and ^4' grounds; short flange in and ?'$* grounds. Ail casings manufactured from 24 gauge galvanized steel and furnished 0 in 8' and 10' lengths. 3 a a GP027 0039 _ of METAL LATH IMPORTANT Observe the minimum weights oi lath for spacing oi supports listed in table below. Lse only clean sand, perlite or vermiculite tor plastering. Do not use unwashed salt water sand. When humidity is higher than nor mal and moisture or acid fumes are anticipated, contact your nearest I'SG Sales Ottice tor proper recom mendations. How to Erect COLOR-RITE METAL LATH 1. Lath ceilings first with sheets carried down six inches on to the walls and partitions. If metal lath is not used on the ceiling, then carry out metal lath six inches from the walls onto the ceiling plaster base. 2. Apply metal lath with long di mension of the sheet running across the studs, joists or furring channels. Secure sheets by nailing along studs or joists or tieing to channels at not more than six inch intervals. 3. On sidewalls, begin lathing at top and continue downward. Place sheets so that the lower sheet laps over the upper sheet. Diamond mesh USG METAL LATH TECHNICAL DATA TYPES AND WEIGHTS OF METAL LATH AND SPACING OF SUPPORTS Typo lath Diamond Math Diamond Math Diamond Math Vi' Z-Rib Z-Rib y.' Rib Vt' Rib . VMgh ter Sywt Yard 2.5 lb. 3.4 lb. 3.4 lb. ' 2.75 lb. 3.4 lb. 3.4 lb. 4.0 lb. Typa of Sfaal Coppor Alloy (1) Coppor Alloy Galvonizod (2) Coppor Alloy Coppor Alloy Coppor Alloy Coppor Alloy STUCCOMESH (3) STUCCOMESH 1.8 lb. 3.6 lb. Notts ( ?) Coppor oltay loth contains from 0.2% to 0.25% pur* coppor. (2) Galvanized lath is cut from galvanized sheets. (3) STUCCOMESH gontroMy applied over exterior sheathing. 26 Coppor Alloy Coppor Alloy Cl TJ O INI O a d* o T lath is carried around corners at least one stud spacing. .4 Riblath on both sidewalls and ceilings is applied with ribs against the supports. 5. Lap diamond mesh at sides not less than 1 > in. and at ends not less than 1 in. Riblath is lapped at sides bv nesting outside ribs, and at ends by lapping not less than l in. 6. Tie all side laps with 18 gauge tic wire at least midway between joist or stud supports, but at not more than 9 in. intervals. 7. Ends of sheets generally should occur over supports; it between, ends of sheets must be securely laced together with IS gauge tie wire. 8. Staggering of sheets is preferred, but not essential. How to Nail COLOR-RITE METAL LATH DIAMOND MESH and FLAT RIBLATH On walls--4d common nails driven in. and bent to engage three strands, or 1 in. '|'6 in. head roofing nails, or 1 in. Xo. 14 wire staples. On catlings--l J 2 in. N`o. 11 gauge, :,is in. head barbed roofing nails. V* IN. RIBLATH On walls--4d common nails driven through the rib or 6d common nails driven in. and bent over the rib. On callings--1'4 in. No. 11 gauge Size Sheets 27'x 94' 27'x 94' 27'x 94' 27'x 94' 27'x 94' 27'x 94' 27' x 94' 48' x 99* 48'x 99# Wood 14' 14' 14' 14' 19' 24' 24' 1 6' (3) 16'(31 Maximum Allowable Spacing* Vertical Support* Horizontal Support* , Metal Solid Partitions 14' 14' 14' 14' 24' 24' 24' Other* (5) 12' 14' 14' 14' 19' 24' 24' Wood or Concrete 14) 14' 14' 14' 19' 24' 24' Motol (4) 13V>' 13ft' 12' 19' 24' 24' GP027 00*1 All motol lath (excopt galvanized) i* painted with o rust-inhibitiv* block asphaltym point. (4) Not recommended, except for fireproofing of iteel shapes. (5) Including vertical furring. 27 'li in. head barbed roofing nail driven through the rib. Lathing nails--for 16 in. stud spacing, nailing 6 in. o.c. requires approximately 17 nails per sq. yd. Tie-Up Work For tying metal lath to channels use 18 gauge galvanized annealed tie wire. For tying channels to channels (horizontal or vertical construction) use 4 strands of 18 gauge or 2 strands of 16 gauge galvanized an nealed tie wire. Estimating Quantities For Suspended Ceilings--The fol lowing ``rule of thumb" method will be found helpful in making a quick approximate quantity estimate. 1. Determine surface area in square feet. Example: ceiling area 30 x 100 feet = 3,000 square feet. Divide by 9 to determine square yards of metal lath required. Assume standard suspended ceiling construction of 1 x/i in. runner chan nels 3 feet apart, and % in. furring channels either 12 in. or 16 in. apart, depending on type and weight of metal lath used. 2. Quantity of \x/% in. channels 3 feet apart--divide square foot area by V/2 (3,000 divided by 2>^= 1200 lineal feet). 3. Quantity of % in. channels 12 in. apart--multiply square foot area by 1.1. (3,000 x 1.1 = 3,300 lineal feet.) 4. Quantity of % in. channels 16 in. apart--multiply square foot area by 0.8. (3,000x0.8 = 2,400 lineal feet.) 5. Figure tie wire at approximately 10 pounds per 100 square yards of lathing. Nail Data Barbed Roofing Nails {% in. hood) Common Nails Length 1 in. 1 in. 4d 6d Gauge No. 11 No. 11 No. 1 2 Vi No. 11 Vi Na. per 275 188 316 181 GP027 0 0 *2 28 1 J SIZE AND SPACING OF HANGERS FOR SUSPENDED CEILINGS Maximum Ceiling Area Maximum Center to Center Supported par Hangar Spacing of Hangars No.9GougeGolvonixed Wire No.8GougeGofvanixed Wire VU* Mild Stool Rod (I) (2) ) 'A* Mild Stool Rod |1) (2) \ 12'/i sq. ft. 16 sq. ft. 25 iq. ft. W x 1m Mild Stool Flat (1) (2H 4 ft. x 3 ft.; 3'A ft. x 3'/i ft. 4 ft. x 4 ft.; 5 ft. x 3 ft. 6ft.x4 ft.;7ft.x3'/j ft.;8ft.x3 ft. (1) Galvanized rods and rust inhibitivo paintod or galvanized strops recommended whore severe moisture conditions may occur. (2) Not manufactured or supplied by United States Gypsum Compony. SIZE AND SPACING OF MAIN RUNNERS Size A Type Weight par 1000 Lineal Feel Maximum Spacing of Hangers alang Runnsrs Csntsr ta Center Spacing af Runners 1 '/i' Cold Rolled Channel 5U lbs. 1 Vi* Hot Rolled Channel (2) 1120 lbs. 2* Cold Rolled Channel 625 lbs. 2* Hot Rolled Channel (2) 1260 lb<. 2 W Hot Rolled Channel (2} 1 600 Ibi. 2 '/i' Hot Rolled Channel (2) 2270 Ibt. 4 ft. 5 ft. 5 ft. 6 ft. 7 ft. 8 ft. Up to 4 ft. Up to 4 ft. Up to 4 ft. Up to 4 ft. Up to 3 Vi ft. Up to 3 ft. 2} Not manufactured or supplied by United States Gypsum Company. STEEL STUD PARTITIONS (PER 100 SQ. YDS.--ANY CEILING HEIGHT) Lineal Feel of Ceiling or Floor Runner Required With Spacing of Studs Approximate lineal Feet of Studs Required 900 *4* ceiling height 1 2 in. Same 16 in. Same 19 in. Some 24 in. lath one side--100 sq. yds. required, lath two sides--200 sq. yds. required. 9 1 0 tin. ft. 675 lin. ft. 570 lin. ft. 455 lin. ft. GP027 0043 29 Basecoat Plasters RED TOP Gypsum Basecoat Plasters Aggregates Mixing--Application Important Job Precautions RED TOP Cement Plaster RED TOP STRUCTO-LITE Plaster RED TOP BONDCRETE Plaster RED TOP Wood Fiber Plaster Portland Cement Plasters PAGE 32 38 38 39 39 41 GP027 004A Basecoat plasters are applied to bases of masonry or lath and support the finish coat. Their primary functions are to cover the base, receive the finish coat, and tie together all units into a durable continuous slab. Of the three general types of basecoat plasters, gypsum plas ter is by far the most modern and widely used. Portland cement plaster excels for a few specialized uses, %vhile lime plasters-- very limited in use--have been largely replaced by gypsum and Portland cement. 31 RED TOP Gypsum Basecoat Plasters ADVANTAGES Uniform--setting time is stabilized. Hazards due to job conditions and variables in water and aggregates are minimized. Controlled set as sures maximum hardness and high strength. Firoproof--gypsum is incombusti ble, will not transmit high tempera tures until completely calcined. It actually tights fire by retarding spread of flame. Plostic--gypsum base coats are highly workable and easy to apply. Strong--capable of withstanding normal wear and abuse for the life time of the building. Adaptable--gypsum bonds firmly to any approved plaster base and will take most any type of finish coat. Economical--high coverage with minimum effort. Easily worked and mixed. GENERAL LIMITATIONS OF USE ). Aggregate must be added strictly according to specifications. Use of too much aggregate reduces the strength of the plaster slab. 2. Red Top Cement, STRUCTOLITE or Wood Fiber Plasters should never be applied to concrete. Use Bo.vdcrete as required according to directions. 3. Red Top Plasters should not be used on exteriors exposed to the ele ments, or on interiors where exces sive water or moisture is expected. Use Portland cement-lime plaster. 4. Bituminous compounds do not provide a good base for gypsum plaster basecoats. Therefore, do not apply such plasters to masonry walls and concrete that have been treated with these compounds. 5. Because of possible moisture con densation or water seepage, direct plastering to the inside of exterior masonry walls is not recommended. Such walls should be furred prior to plastering. 6. When used in conjunction with Radiant Heating systems, the tem perature at the surface of plaster shall not exceed 115 F, nor shall water in the pipes embedded in the plaster exceed 125 F. Gypsum-sand plaster has approximately three times the conductivity of gypsumlightweight aggregate plasters. Aggregates Aggregates in the form of sand--and more recently, perlite and vermiculite--are added to gypsum cement plasters to extend coverage and re duce cost. They also act as a gauging agent to minimize shrinking of gyp sum in setting. The proper use and proportioning of aggregates with gypsum plaster determine the ultimate strength and 32 hardness of a plastered wall. Typical compressive and tensile strengths that result with use of sand and lightweight aggregates (perlite, vermiculite) in varying plaster mixes are shown in the chart on following page. The Americon Society for Testing Materiols in ASTM Designation C35-54T has established the following specifications os standard for the proper gradation of good plostering aggregate: Parcantoga Ratoinad on loch Siovo Siava Site by volvmi Varmfc- uiita by voiuma Sane . by wai 0fct Max Min Max Min Max Min No. 4 0 0 0 No. 8 . 5 0 10 0 50 No. 16 . 4j 10 75 40 30 5 No- 30 85 45 95 45 45 30 No. 50 95 7S 98 75 95 65 No. 100 100 88 5 00 90 ! 00 90 SAND Sand is the most commonly used plaster aggregate because it is eco nomical and widely available. Proper proportioning and gradation of sand are most important in determining bulk and working qualities of plaster, and the ultimate quality of the fin ished wall. Over-sanding or the use of an excessive amount of fine sand reduces the strength and hardness of gypsum plasters. VERMICUIITE is mined as a mica rock, ground and expanded under heat into lightweight granules for use as a plaster aggre gate. It should weigh between 7]^ lbs. and 10 lbs. per cubic foot and comply in gradation with ASTM designation C35-54T Inorganic Ag gregate for use in Interior Plaster. Walls plastered with gypsum plas- Recommended Proportioning & Coverage Gypsum Cement Platter (weight) Gypsum Cement Plotter (100 Ibt.) Sand (weight) or Perlite or Vermiculite (cu. ft.) Platter Bate Two Coot Work Scratch-Double Bock Gypsum lath l:2'/j Metal lath -- Unit Masonry 1:3 Three Coot Work Scrotch coat Brown Coat 1:2 1:2 1:3 1:3 Coverage Range Sg. Yd. Per Ton 175-220 90-125 175-200 9900 iZ 0d3 33 Relative Strength of Various Plaster Mixes Mi* Compressive Strength lbs. per sq. inch Weed Fiber | Cement Plotter Plotter to Send by Weight Neot 1:1 1:2 1:3 Cement Plotter Vermiculite per 100f Cement Plotter 2 eu. ft. 3 cu. ft. Cement Plotter Perlite per 100# Cement Plotter 2 cu. ft. 3 cu. ft. 2100 1900 1200 750 500 300 1000 650 Tensile Strength lbs. per sq. indt 400 245 170 120 130 90 165 105 When the proper amount of aggregate has been used, eoch grain of aggregate is cemented on ail sides to its neighbors by the gypsum. When the proportion of aggregate to plaster is excessive, the aggregate is not properly cemented. See illustrations below. ter containing vermiculite as an ag gregate have lower strength and re quire a longer period tor drying than walls of sanded plaster, but are lighter in weight and have greater fire resistance. Where hard finish coats ! Keenes cement i are to be used, reduce the proportion oi vermiculite to gypsum plaster in the basecoat. Vermiculite is proportioned with gypsum plaster on a volume of aggregate to weight of plaster basis, and the proportion ing should be in strict compliance with the table on Page 33. PERLITE Perlite is a lightweight plaster ag gregate produced from a volcanic rock. The perlite ore is ground and screened to proper size, then ex panded to produce a light grey or white colored aggregate. Perlite ag- PROPER AMOUNT OP AGGREGATE EXCESSIVE AGGREGATE J l N' K X' arcuate tor plastering should weigh between 71 and 15 lbs. per cubic dot. It should meet ASTM C35-54T Inorganic Aggregate for use in In terior Plaster. It has excellent firere-isting qualities and when mixed with gypsum plaster it provides a higher strength plastered wall than does vermiculite. fSee comparative strengths of various basecoat plas ters, page jy.) Perlite is added to gypsum plaster on a volume of perlite to weight of plaster and should be proportioned in strict accordance with specifica tions. Note: See limitations, pages 32 and 37, if perlite or vermiculite aggregate is to be used with plaster on radiant heating jobs. WATER All gypsum plasters require the addi tion of water on the job. Water pro vides lubrication and workability to permit application to the plaster base. It also induces the proper set ting of gypsum. As a general rule, any water fit to drink is suitable for mixing with plaster. MIXING Gypsum basecoat plasters may be machine or hand mixed. The former is preferred because it disperses the plaster, the aggregate and the water more evenly. Machine Mixing--place the required water in the mixer. Add approxi mately half the required aggregate. Add all the plaster. Add the balance of the aggregate. Ii necessary add more water to obtain the proper con sistency. Mix not less than 1 minute or more than 3, depending on the speed of the mixer. Dump the entire batch at once. Clean the mixer thor oughly when not in use or continuous operation. Box Mixing--dry mix plaster and aggregate together until completely blended. Add water, and hoe plaster into the water until thoroughly mixed to proper consistency. PLASTER GROUNDS AND THICKNESS To attain proper wall strength it is essential that the plaster slab be applied to the proper thickness. This is controlled by the use of grounds. Grounds should be set to provide a minimum plaster thickness of: (a) ! ) inch over gypsum lath; (b) /h% inch over gypsum partition tile, brick, clay tile or other masonry, tc) 34 inch over metal lath when measured from the back of the lath (jj inch from face of the lath). O T3 Q Kl O O -f* S 35 APPLICATION of RED TOP PLASTERS Plastering specifications may require either two-coat or three-coat work. Two-Coat Work consists of one base coat and one finish coat. It is gen erally used over a masonry plaster base and often over gypsum lath. The basecoat plaster is applied in one coat by either the "single-toot' 'or the "scratch-double-back" method to slightly less than the thickness of the grounds. It is rodded and darbied to a true, even surface left rough enough to take the finish coat. THrea-Coat Work consists of a scratch coat, a brown coat and a finish coat. Three coats are required over fiber insulating or metal lath. The first or "scratch" coat properly aggregated is applied to a thickness of approximately ,*4 inch over the face of the lath and then cross-raked before it sets. This provides a me chanical key tor the brown coat. The brown coat is then applied directly to the set scratch coat. The brown coat is used to fill out to just slightly below the grounds and is rodded and darbied to a true, even surface. It is left rough enough to properly receive the finish coat. IMPORTANT JOB PRECAUTIONS 1. Equipment and'Storage of Ma terial!-- All successful plaster jobs require adequate equipment (mortar boxes, mortar boards, scaffolding and tools). Every job should be properly planned to provide ample scaffolding 36 to permit continuous application of both basecoat and finish plasters for a complete panel of either a wall or ceiling. Keep all mixing tools clean. Wash them in clear water only. Keep plaster stored in a dry location. Stack on planks raised on the ground and away from damp walls or floors. 2. Heating--Plaster must not be applied to surfaces that contain frost. A minimum temperature of 55 F. should be maintained in the building for an adequate period prior to, dur ing and after the application of the plaster. In cold, damp or rainy weather, properly regulated heat should be provided, but precautions must be taken against too rapid drying before set has occurred. This avoids "dry outs." 3. Ventilation--As soon as the plas ter has set, tree circulation of air should be provided to avoid "sweat outs." After plaster has set, heating should be continued to insure as rapid drying as possible. In hot, dry weather, protect the plaster from wind, and from drying unevenly or too rapidly before set has taken place. If glazed sash are not in posi tion. exterior openings in the build ing should be screened with cheese cloth or similar material. 4. Finishing Over lightweight Aggregate Basecoats--The use of $ lightweight aggregates tperlite and < vermiculitei with gypsum basecoat J plasters often results in a basecoat ( ( 1 V- V having a high suction (because of higher porosity!. In applying a finish coat over this high suction base, the water in the finish coat is quickly sucked into the thirsty basecoat making application of finish difficult, due to loss of easy working charac teristics of the finish plaster. Further more the finish coat is sometimes susceptible to severe check cracking, because water is sucked out before gauging plaster is set --thereby nulli fying purpose of the gauging plaster (provide initial set to avoid possible shrinkage of the lime-putty finish"!. Xecessarv precautions should be taken to apply finish coat plaster before the basecoat becomes thor oughly dry. When a basecoat has become bone dry, before finishing, spray lightly with water to eliminate the excessive suction of the basecoat, then apply finish coat. 5. Radiant Heating--The Gypsum Association makes the following rec ommendations when radiant heat ing coils are specified for use in a ceiling or are to be embedded in the plaster slab. a. In all radiant panel heating sys tems where gypsum plaster or gyp sum products are concerned, the surface temperature shall not exceed 115 degrees F. In those systems where pipes are embedded in gypsum plaster, this shall be met by requir ing the water temperature in the pipes in contact with the plaster not to exceed 125 degrees F. (Xote: The 12;F maximum water temperature is lSaF below that rec ommended in the ASHACE Guide to avoid possibility of calcination of the gypsum.) b. Radiant heating coils should not be used to heat the building or dry the plaster slab in which they are imbedded. The heating system should only be turned on and brought up to operating temperatures very slowly after the plaster slab is thoroughly dry. c. Where heating elements are em bedded in gypsum plaster, a mini mum cover of shall be maintained over the coils. d. In radiant panel heating systems where the pipes are to be embedded in plaster applied to metal lath or gypsum lath, these pipes shall be supported by the framing and not bv the lath. . Gypsum plaster, when used with radiant panel heating systems, shall be mixed and applied in accordance with the ASA A42.1 "Standard Spec ifications for Gypsum Plastering." The design of a radiant panel heat ing system is the responsibility of a heating engineer, and the lathing and plastering specifications must be established by the designer. There fore, lightweight aggregates (Vermiculite and perlite) or mill mixed plasters incorporating them f.Structolite), should not be used unless the heating engineer, heating contractor or architect have designed the heat ing system for their use, as light weight aggregates offer greater re sistance to the flow of heat than plasters mixed with sand. GP027 0050 37 Ttu FCP Cement Plaster This is a "neat" gypsum plaster ivhich requires the addition of an aggregate (sand, vermiculite, per lite) and water on the job. It is the most common base coat plaster be cause job-addition of aggregate gen erally provides low cost. It is used for both scratch and brown coat work, and for application over all approved plaster bases. The use of fiber in plaster stems from its use with lime base coat plasters years ago. Lime does not set and requires a long period of time to harden. Consequently fiber was ne cessary to add cohesiveness to the mass. ADVANTAGES Red Top Cement Plaster is fireproof, adaptable, plastic, uniform and strong. It is perhaps the most eco nomical base coat plaster in use today. 181 RED TOP 0f pt u * CEMENT PLANTE* I LIMITATIONS see general limitations noted on page 32. Job-addition of aggregates must be in strict accord with gradation and proportioning specifications. RED TOP STRUCT0-LITE Plaster This is a mill-prepared base coat plaster using a properly graded and proportioned perlite aggregate. It is Red Top Cement Plaster is avail able in two types: Regular for sand ready for use with the addition of water only on the job. aggregate and L\V Formula for light weight aggregate--both types avail able for machine application or hand application. For hand application both types are available "fibered" or "unfibered." It is usually desirable to use fibered RED TOP plaster for scratch coat work on metal lath. It helps hold plaster STRWCTOdJTt J | jlGYPSUM . O -ao I mortar to lath until set takes place. PUKTCT (SI Unfibered plaster is suitable for use over all either bases. o o 38 J 1 r ADVANTAGES Controlled proportioning of a prop erly graded and sized perlite aggre gate. Weighs much less than plaster and sand aggregate. Less than half the weight on wall. More fireproof. Offers fire ratings almost double those attained with plaster and sand. Mill formulation reduces suction to that of plaster and sand, assures easy application of the finish coat. Job-mixed lightweight aggregates often create considerable suction for finish coat work. Stabilized set. LIMITATIONS See general limitations page 32. approximately .30'7 greater surface hardness; 50 to 100'f greater fire rating than plasters containing sand. Highly desirable for use where good plastering sand is not available, and lor alteration, patch and repair work. LIMITATIONS see general limitations page 32. RED TOP | WOOD FIBER 1 PLASTER RED TOP Wood Fiber Plaster This is a mill prepared base coat piaster containing a wood fiber ag gregate and requiring the addition of water only on the job. Over masonry surfaces, one part sand by w eight may be added for easier work ing qualities, and to minimize shrink age cracks. ADVANTAGES Red Top Wood Fiber Plaster is rec ommended for use where excessive strength, toughness, or a higher fire rating is required. It has: three times the compressive and tensile strength ui plaster sanded 1:3 Isce page RED TOP BONDCRETE Plaster This is a specially formulated gyp sum base coat plaster requiring only the addition of water on the job. It is the only recommended base coat plaster for application to properly prepared, rough monolithic concrete. ADVANTAGES unlike normal gypsum base coat plas ters. Bondcrete has thermal expan sion equal to concrete, which pro vides continuous bond to this type surface. 39 GP027 0052 BONDCRETF | gtpiu* Ptwra I KAMrim & LIMITATIONS Bondcrete should be used only on rough concrete that is properly pre pared for plastering. It should never be applied to smooth concrete. Maximum thickness of Bondcrete and finish coat should not exceed 5's in. on ceilings, and in. on walls. If additional thickness is required, metal lath must be prop erly secured to the concrete surfaces before applying the plaster. Surfac* Preparation--monolithic concrete surfaces should be brushcleaned of all dust, loose particles and other foreign matter. Any laitance and efflorescence should be re moved by washing with a lO^c solu tion of commercial muriatic acid and water. Grease or form oil should be removed by wiping with naphtha spirits. If surfaces are not rough enough to provide necessary mechanical key, they should be hacked or bushhammered; or a dash-coat of port land cement grout composed of 1 part of cement and lj 2 parts of fine sand (mixed to a mushy consistency) may be applied. Keep this coat damp for at least 2 days immediately fol lowing application and then allow to dry. Before application of BondCrete, the surface should be evenly dampened to provide proper suction. Application to Concroto Callings-- apply coat of Bondcrete Plaster, scratching in thoroughly, doubling back and filling out to true, even sur face left rough by brooming to receive the finish coat. Application to Walli and Columni --apply a scratch coat of BondCrete. Follow with a brown coat of gypsum plaster (1 part Red Top Cement Plaster to not more than 3 parts of sand by weight) troweled into the scratch coat before it has set. Bring out to grounds and level to true, even surface using rod and darby. It is then ready to receive the finish coat. Total thickness of plaster should not exceed J-j in. Portland Cement-Lime Base Coat Plaster Portland cement, with the addition of lime to provide working qualities and water resistance, is frequently mixed with sand and water to form a plaster mortar. It is chiefly used as a base coat for exterior stucco and in places subject to excessive moisture, such as swimming pools, showers, dairies and steam rooms, and as a back up material for ceramic tile. 40 Gp027 0053 LIMITATIONS Portland cement-lime base coat plas ter is comparatively unplastic and hard to apply, thus high in cost. It must be kept damp to properly cure and prevent drying out and cracking. Several days delay between coats is necessary to assure proper curing and hardening. Mixing and Application -- Mix scratch coat in the proportion of one bag of portland cement, two bags of Mortaseal or Red Top Masons Hydrated Lime <2 cu. ft. lime putty) and not more than 7% cu. ft. of sand (approximately 40 No. 2 shovels). For application over stucco mesh or self-furring metal lath, approximately two pounds of hair or fiber should be added to each mix. Mix brown coat in the proportion of one bag of portland cement, two bags Mortaseal or Red Top Masons Hydrated Lime (2 cu. ft. lime putty) and not more than 9 cu. ft. of sand, approximately 50 No. 2 shovels). Scratch coat should be applied in a full in. thickness with sufficient pressure to form a good bond with masonry surface or to force it through and completely embed the stucco mesh or metal lath. Cross scratch, and after set, damp cure for not less than 48 hours. Brown coat should be applied over the dampened scratch coat to a full in. thickness with sufficient pres sure to form good bond. Rod the brown coat level, and broom the sur face to provide key for the finish coat. After set, damp cure at least 48 hours before applying the finish coat. (See Oriental Exterior Stucco for finish coat, page 49). Curing--damp cure each coat by applying water in a fine fog spray. Apply only as much water as is readily absorbed. The frequency of spraying depends on the weather, with more frequent applications re quired during hot, dry or windy weather. O TJ O M -J O oun g* 41 - Finishing Plasters Gypsum-Lime Putty Trowel Finish Keene's Cement-Lime Putty Gypsum Trowel Finish STRUCTO-GAUGE Lime Putty Gypsum Sand-Float Finish ORIENTAL Interior Finish ORIENTAL Exterior Finish SABINITE Acoustical Piaster USG HI-LITE Acoustical Plaster RED TOP AUDICOTE Acoustical Plaster PAGE 44 46 47 47 48 49 49 51 53 54 GP027 0055 Finish-coat plasters applied to basecoats (generally of gypsum plaster) provide the surface for final -wall or ceiling decoration. They are either factory prepared, requiring the addition of water only ; or they may be job-mixed by blending lime putty and gauging plaster, or Keene's Cement or Structo-Gauge. Finish-coat plasters are normally applied to a thickness of 14 inch for trowel finishes, up to }/$ inch for float finishes and } 2 inch for acoustical plaster finishes. Finish-coat plasters are selected according to job requirements for texture, color, hardness, sound absorption and type of base coat. 43 Finishing Plasters Gypsum-Lime Putty Finishes Finish lime putty into which is blended a gypsum gauging plaster is commonly known as "white coat.'' It is the most widely used finish coat because of its good working qualities, whiteness, economy and ability to take any form of decoration. Usually it is troweled to a smooth hard sur face over a gypsum base coat. With the addition of sand, it is adaptable tor sand-fioat finishes. FINISHING LIMES Made from specially selected lime stone rock of high purity, the most popular finishing limes come from the dolomitic fields in northwestern Ohio. They have excellent working qualities. There are three types of finishing limes: (1) double hydrate. (21 normal hydrate and (3) quick lime. Each requires specific handling in slaking or soaking to produce a good finish ing lime putty. drate finish lime immediately devel. ops high plasticity. Thus, overnight soaking is unnecessary. ADVANTAGES Can be mixed with water by hand or with mechanical mixer. Becomes highly plastic right away. Easy working; uniform; white. Eliminates troubles from delayed hydration. USG Brand--Ivory Finishing Lime (Genoa, Ohio). Normal Hydrate Finish Lime generally made from Ohio dolomitic limestone, it is the most widely used today. Although hydrated in manu facture, overnight soaking is sbll necessary to develop workability and plasticity. ADVANTAGES economical, uniform, easy working, white and plastic. LIMITATIONS Requires overnight soak. USG Brandt--Grand Prize and Red Top Finish Hydrate (Genoa, Ohio). Double Hydrate Finish Lime Usually' made from Ohio dolomitic limestone. It is over 92^ hydrated during manufacture which eliminates troubles from delayed hydration, ex pansion and separation in the wall. Upon mixing with water, double hy Finish Quicklime is usually made from high calcium limestone. It is produced and used in areas where it is not economical to ship from the Ohio lime fields. Quicklime or "hot" lime requires slaking and relatively long periods 44 Sp027 0056 i t soaking for complete hydration and to develop the plasticity neces-ary tor easy application. ADVANTAGES economical because of its high putty yield. Easy working. LIMITATIONS Requires long slaking period. Unless handled carefully can cause serious bums in handling. USG Brand--Red Top Finish Quick lime (Texas). GAUGING PLASTERS Lime does not "set'' but hardens slowly. It likewise shrinks on drying. Therefore, gauging ~aster is blended into the lime putt\ . . proper propor tion to provide controlled set and strength, and to avoid shrinkage cracks when used as a hnish coat. Red Top Gauging Plasters are carefully ground and screened to just the right particle sizes to make this plaster quick soaking and easy to blend with lime putty. Gypsum gauging piasters are avail able in "quick set" and "slow set," making it possible for the mechanic to use the material which best suits him. This makes it unnecessary to add retarder or accelerator for regu lating the set of the finish. They are available as white gauging and local gauging which is somewhat darker in color. For brilliant white finishes, white gauging plaster should be used. MIXING A APPLICATION Gauging plaster is added to the lime putty in the proportion of one part of dry gauging to not more than 3 parts of lime putty by volume, or one part of dry gauging to not more than 2 parts of dry hydrated lime by weight. (Mixing on board--use 2 quarts of water in putty ring for each 12 qt. bucket of lime putty. One hod of lime putty equals approximately 36 qts. A 12 qt. bucket of lime putty, 35-40 lbs., contains 18-20 lbs. of hydrated lime on dry weight basis. Silt sufficient gauging plaster into this water to completely soak up the water.) After the gauging plaster is sifted into the lime putty ring and allowed to soak a few minutes, the materials are thoroughly blended to avoid gaug ing ``streaks" and to provide uniform density in the finish coat. The gauged lime putty is applied over a partially dry gypsum base coat. Scratch in a thin coat, well ground into the base coat, and im mediately double back with a second coat, filling imperfections. (A third or thin "sweetening coat" is sometimes applied to fill in any further imper fections that remain after the second coat has "taken up.") After the base coat has sucked most of the excess water from the finish, it is troweled to density the surface and help elim inate check cracks. As final set takes place, it is water-troweled thoroughly to pro vide a dense, smooth surface suitable for decoration. GP027 0057 45 < Keene's Cement-Lime Finish Red Top Keene's Cement is a high strength, white gypsum plaster used with finish lime putty for extremely hard, dense surfaces. Although Keene's Cement is a gypsum material, it differs from other gypsum plasters in several particulars; it is slow-setting; it is the only gypsum plaster that can be re-tempered; and the finish coat re quires more troweling. Red Top Quick-Troweling Keene's sets faster and requires less trowel ing. It must be used with a minimum of 25 lbs. of dry hydrated lime per 100 lbs. of Keene's Cement. Keene's-Lime Finish is similar in RED TOP f KEENE9 CEMENT i % many respects to a lime-gauging fin ish except that Keene's Cement is used in varying proportions, depend ing on hardness required, in place of gauging plaster. Keene's-lime finish should be used where greater resist ance to moisture, and greater surface hardness and resistance to abrasion are desired--as in hospitals, kitch ens, bathrooms and corridors. For medium hard finish, mix in the proportion of 50 lbs. of dry hydrated lime (100 lbs. lime putty) to 100 lbs. of Keene's Cement. For hard finish, limit the quantity of lime to 25 lbs. of dry hydrated lime (50 lbs. lime putty) to 100 lbs. oi Keene's Cement. APPLICATION the finish coat is applied over a set base coat which has been broomed and is partially dry. (If base coat has dried out, spray with water before finishing; do not soak). Scratch in a thin coat well ground into the base coat and immediately double back with a second coat filled out to a true, even surface. Allow to draw up a few minutes, then trowel with water to a smooth glossy finish, tree oi cat faces and other blemishes. Continue troweling until finish has set. AVAILABLE USG BRANDS RED TOR CHAMPION Gauging Plotter (white) RED TOP STAR Gouging Platter (white) RED TOP Gauging Platter (gray) RED TOP Gouging Platter (gray) RED TOP Regular Keene't Cement (white) RED TOP Quick Troweling Keene't Cement (white) USG STRUCTO-GAUOI 46 SET WITH LIME PUTTY Quick P--20*30 min. Slow tet-~45-60 min. Slew tot--45-60 min. Quick tot--20-30 min. 3-6 hourt 1 -2 Hour* 1-1 'A hourt SP027 0058 LIMITATIONS For interior uses only. Where ex posure to water is extreme or con tinuous, use Portland cement-lime plaster. Apply Red Top Keene's Cement only over gypsum base coats of high compressive strength. S7RUCTC-GAUGE Lime Finish I'SG Structo-Gauge is a new high strength gypsum gauging plaster for use with varying proportions of lime putty to produce surfaces of extreme hardness and durability. Wherever Keene's Cement is used, Stri'CTO-Gauce Lime Finish may be used. With a faster set than quick troweling Keene's Cement, easier working characteristics and higher lime proportions, Strvcto-Gal'ce finishes are more economical than any other hard finish. With the same proportions of lime, Structo-Gai'ge finishes achieve much greater hard ness than a comparable Keene's Cement-Lime Finish. For medium hard finish, mix in the proportions of 100 lbs. dry SiructoGauce to 200 lbs. dry hydrated lime. For hard finish, mix in the propor tions of 100 lbs. dry Strecto-Gavge to 100 lbs. dry hydrated lime. to a smooth finish, free of all blem ishes. All troweling must be com pleted before final set. Clean tools and equipment immediately after each mix. LIMITATIONS Same as for Keene's cement-lime fin ishes. Gypsum Trowel finish Red Top Gypsum Trowel Finish is miii-prepared and requires the addi tion of water only. It is recommended for use over gypsum base coats where hardness and immediate decoration are required. Red Top Trowel Fin ish is available in most areas and is recognized for its easy working qual ities and pure white finish. TROWEL FINISH | 5 * APPLICATION Apply over a partially dry gypsum base coat. Scratch in a thin coat, well ground into the base and immediate ly double back with a second coat, filling imperfections. Water trowel ADVANTAGES rated one of the hardest of all finish plasters, it provides protection against the most severe wear. It has approxi GP027 0059 47 mately twice the surface hardness of ordinary lime-gauging finishes. Xonalkaline, it will not injure paint or decoration and may be decorated as soon as it has set and dried. Made of gypsum, it provides a durable and natural bond to gypsum base coat plaster. MIXING AND APPLICATION Red Top Trowel Finish requires the addition of water only. Allow to soak to or 15 minutes and then mix to a smooth, lump-free mortar of the de sired consistency. Apply over a gypsum base coat which has set. but is not bone dry. (If base coat has dried out, spray lightly, before the finish coat is ap plied. Do not soak.) Scratch in thor oughly, double back and fill out to true, even surface. The finish should not exceed x/% in. thickness. Trowel the surface free of cat faces and other blemishes, using water spar ingly. Troweling must be complete before final set occurs. Work from unset edges to avoid joining marks. Gypsum Sand-Float Finish Red Top Sand Float Finish is similar in every respect to gypsum trowel finish, except that it is carefully for mulated with the correct proportion of properly graded sand. This pro vides a uniform, easy-working ma terial which eliminates the uncer tainty of job-mixed sand-float fin ishes. Available in its natural gray color, which requires painting for final decoration. Select lime-proof colors may be added which eliminates further decoration. APPLICATION same as for gypsum trowel finish ex cept that the final coat is finished with a wood, carpet, cork or rubber float depending on texture desired. Colored Finish Plasters Colored gypsum finish plasters are frequently used to produce a pre decorated finish of either a finelyfloated or textured surface. Use of colored gypsum finish plasters elimi nates the need for further surface decoration. This speeds the plaster ing job and results in lower costs. Col ored gypsum finish plasters are avail able in either factory-prepared colors or they can be produced on the job. JOB PREPARED FINISHES require addition of limeproof color pigments on the job to proper pro portions of lime putty, aggregate and Keene's Cement. In mixing this ma terial for a job, the lime-proof color should be thoroughly blended and mixed with the plaster to prevent color streaking and variation. It is also necessary to mix job-prepared colored interior finishes in sufficient quantities to complete a job. This eliminates color variation which would result from trying to mix a second batch to match the first. Keene's Cement-Sand Float Finish shall be mixed in the proportions of 100 lbs. of Keene's Cement to 50 lbs. of dry lime and 400 lbs. of sand, with or without the lime-proof colors. 48 GP027 0060 ORIENTAL Interior 0:!cred Finish A factory prepared colored finish con taining properly graded aggregate and select limeproof colors to insure easy working qualities and uniform ity in results. Available in 6 pastel colors and white, it requires no fur ther decoration and may be applied to produce many types of surfaces ranging from a very fine sand-float finish to a ragged texture. It is highly resistant to abrasion because of its great hardness; avoids variations of color intensity which sometimes occur when colors are mixed on the job; permits early occupancy. tionally dry, it should be sprayed uniformly with clean water the night before finishing. Application is made in a two coat double back operation. Scratch in a thin coat well ground into the base coat and double back with a second coat, filling out to a true even sur face. The surface can be floated with a sponge, sponge rubber float or car pet float. The finish can also be ap plied in any desired texture except a smooth trowel finish. Do not use water while floating. / ORIENTAL Exterior Stucco Factory formulated to insure color uniformity. Applied to exterior sur faces over a base coat of portland cement-lime and sand. Oriental Exterior Colored Finish is available in 11 pastel colors and white. Suitable for application on new work or for remodeling, it is an economical means ior beautifying in two ways -- texture and color. MIXING ANO APPLICATION Add clean water only, hoe stucco into the water. Allow to soak 20 or 30 minutes and mix thoroughly to a smooth, creamy easy-working con sistency. Must be applied to a set. "half-green'1 base coat of gypsum plaster. If the base coat is excep 49 MIXING AND APPLICATION Oriental Exterior Stucco requires only the addition of water on the job. When it is mixed and applied in the following manner, excellent finished results may be obtained: 1. The suction of the base coat must be uniform, therefore, the base coat should be in a "half green" condi tion. If it is too dry, spray lightly. (See detailed instructions for mixing, applying, and curing of Portland cement-lime base coat, page 41.) 2. Remove loose and projecting par ticles from base coat, then apply a thin coat well ground into the base and completely covering it. Double back and fill out to a uniform surface about !-g in. thick, covering area from top to bottom, in one operation to eliminate joinings. Trowel three or four times before starting to texture. 3. For a float finish, use a cork, wood, carpet or sponge rubber float, and float the surface to an even texture. 4. Do not use water in floating. 5. After setting, spray the surface periodically tor several days to cure the finish. .6 Do not apply in freezing weather or before or during a rainstorm. FINISH PLASTER data Mix by weight of dry materials Color Finish Texture Hardness in Kilograms {2) Coveroge Gauging Plotter to llms 1:2 White or Gray (1) Smooth 34 1 ton gauging 2 tons lime cover approx* 1000-1400 yds. STRUCTO-OAUGC It lime 1:2 1:1 White Smooth 56 1 ton STRUCTOGAUGE 2 tons lime cover approx. 1000-1200 yards White Smooth 108 1 ton STRUCTOGAUGE 1 ton of lime cover approx. 600-750 yards. { V Cray with `'local" gauging platter. 12i Kilograms required to force a 10 MM ba/l .0 1" into plaster face. 50 -o o rsi ^ O rw SA8INITE Fire Resistant--incombustible, min Acoustical Plaster eral composition. Adaptable--blends with any archi TROWEL OR FLOAT tectural design. a highly sound absorbent acoustical Easily Applied--any good mechan plaster which can produce a trowel ic, provided ordinary precautions . or float finish. It is applied over a are observed, can apply Sabinite. properly prepared gypsum base coat, Economical--applied in two succes and is available in oyster white and sive coats, 16 to 24 hours apart -- | lour standard colors. eliminates re-scafiolding. ADVANTAGES LIMITATIONS High Sound Absorption--carries a Mixing and application instructions 60 XRC in Trowel and .55 XRC in must be closely followed. Float Finish. Designed for use on ceilings or Readily Maintained--cleans with wall areas not subject to contact brush or wallpaper cleaner; may be or high humidity. sprav-painted with only moderate Sabinite is not recommended loss oi acoustical efficiency. over radiant heating panels. Quick Troweling Keene's to limo Gypsum Trowel Finish Gypsum Float Finish ORIENTAL Finish 2:1 Medium Hard 4:1 Hard Neat Neat Neot White White White Gray 12 colors , Smooth Smooth Smooth Float Floot (See (See 50 70 55 Note 3) Note 3) : 2 tons 4 tons 1 ton 1 ton 1 ton will Keene's Keene's will cover will cover cover 1 ton lime 1 ton lime approx. approx. approx. cover approx. 850-1200 yds. cover approx. 1300-1700 yds. 350-400 yd.. 250-275 yd. 250-300 -o yds. o IS) -4 ' {3} These are hard finishes but the aggregate in the surface does not permit an indication with fhis test. o o O' 51 MIXING AND APPLICATION Machine mixing recommended. Put 22 quarts dean water in mixer for each bag of Sabinite. Mix until Sabinite weighs IS to 17 lbs. net per 12-qt. pail (usually 3 to 5 minutes, depending on speed of mixer). To hand mix. place Sabinite in one end of clean mixing box. For each bag, add 23 qts. of clean water in other end. Hoe Sabinite intoWater. The mix will appear dry, but do not add more water. Hoe until Sabinite weighs 15 to 17 lbs. net per 12-qt. pail. Apply in 2 coats to a uniform total thickness of }-$ in. over a base coat of scratching in and doubling back over a set, semi-green gypsum base coat that is level and thoroughly broomed or cross raked. If base coat is dry, spray lightly to reduce suction. Fol low immediately with a wood or metal darby, leveling Sabinite to provide a true, even surface for finish coat. Allow to set and to partially dry (at least overnight or longer de pending on job drying conditions) before applying finish coat. Apply finish coat to a thickness of }t in. by scratching in and doubling back, over a set. partially dry base coat of Sabinite. Bring total thick ness to }'2 in. Leave surface uniformly level and free of trowel marks, work ing from wet edge. Finish ceiling panels in one continuous operation to avoid joinings. Trowel Finish--After water sheen leaves surface (about 30 minutes) trowel lightly to a uniform texture. Do not use water during troweling. Fioot Finish--float second coat 5 to 10 minutes after water sheen has left surface. Cse a shingle, cork, or rubber float. Do not use water in floating. Red Top gypsum plaster. A full scratch and brown coat of gypsum plaster is required over metal lath, Rocklath plaster base, and mason ry bases (excluding monolithic con crete) to provide proper rigidity, strength, and a solid base tor the acoustical plaster. Apply first coat in. thick by Directions for Applying SABINITE Acoustical Plaster Over Rough Monolithic Concrete: Over properly prepared rough monolithic concrete surfaces apply Bondcrete plaster not to exceed 'T in. thickness on ceil ings and ? s in. on side walls. Apply the Sabinite over the set, semi green Bondcrete base coat, as specified. 52 SP027 0064 DIRECTIONS FOR FAINTING USG ADVANTAGES ACOUSTICAL PIASTERS. Remove Hl-LITE Finish--it's snow white, with all loose dirt or dust by use of a over 759c light reflection. vacuum cleaner. Paint should be water-thinned. Texolite Imperial or Standard is recommended. First coat, mix one part Texolite paste Eoiy o Mix and Apply--mechan ically mixed, it works smoothly and easily under the tools. I to one part water by volume. Second Attractive, Adaptable--can be given coat (if required), mix one part Tex- a stippled or stipple-perforated fin / olite paste to two parts water by ish. Can be used in areas of moder volume. Spray on with any gun with ately high humidity, such as swim a medium fine spray. DeVilbiss spray ming pools. gun, type MBD, with a So. SO noz zle or equivalent, is recommended, l'se 30 to 40 lbs. pressure in the gun and 20 to 30 lbs. on the paint. Hold nozzle 14 to 18 in. away from work. L'se a slow, uniform motion. Cover surface in one pass. Do not pass over same area several times as this builds up paint unnecessarily. Allow at least overnight drying Fir* Resistant-- Hi-Lite will not bum or support combustion ... an important safety advantage. Low Maintenance Costs--can be decorated repeatedly with any good resin --emulsion or casein paint (TEXOLITE--Imperial or. Stand ard) without appreciable loss in sound absorption. between coats. If weather is extremely humid, allow additional drying as necessary. GP0Z7 OOS5 * Hl-LITE -.c:usticai Plaster * STIPPLE OR STIPPLE-PERFORATED Highest light reflective acoustical plaster developed by U.S.G. (.77 .80), must be stippled or stippleperforated to provide its acoustical efficiency (.60). Available in white only. LIMITATIONS Hi-Lite must be machine mixed to develop proper density. Designed for use on ceilings or wall areas not subject to contact. 53 When perforated, a special per forator with rust resistant prongs should be u-ed. Ht-LtTE is not recommended tor use over radiant heating panels. MIXING AND APPLICATION USG Hi-Lite Acoustical Plaster shall be applied in two coats to a uniform thickness of 1 >". A full scratch and brown coat, either gypsum plaster or portland cement-lime plaster, that has been cross-raked is required over metal lath, gypsum lath and mason ry bases (except monolithic con crete). First Coot--Apply first coat of HtLite by scratching f/g" hard, imme diately doubling back to a total of 5 s' over a set and dry, partially dry, or semi-green basecoat. Darby light ly to a level surface. Allow to set and dry fairly well (usually overnight) before finish coat. Finiih Coat--Apply finish coat Ag" thick to a set and fairly dry basecoat, scratching and doubling back leaving surface free of trowel marks. Work from wet edge to avoid joinings. When surface gloss has disap peared and surface is crisp and hard enough to give clean perforations, stipple the surface with a rice root stippling brush to a uniform texture. To obtain a stipple-perforated fin ish, perforate about .10 minutes after stippling (when surface is hard enough to give clean perforations), but before set. Use perforator fur nished by the United States Gypsum Company, Perforations should num. ber approximately 500 per square foot and should be at least ?jj" deep AUDICOTE Acoustical Plaster SPRAY OR HAND APPLIED A plastic, high-coverage material with excellent sound-absorbing prop, erties. It has exceptional bonding characteristics, and is designed for use over gypsum basecoat plaster Portland cement-lime basecoat plas ter or monolithic concrete. Available in Satin White and Special White l E ADVANTAGES High Sound Absorption--carries i .60 XRC in darbied finish and 5: XRC if machine textured finish u desired. Low Maintenance--tests reveal no loss in noise reduction coefficient after two spray coats of TEXOLITE (Standard or Imperial), applied ac cording to U.S.G. specifications tor painting acoustical plasters. Audicote may also be redecorated easily by direct spray application of a thin coat of Audicote Plaster. Fire Reiistant-- incombustible, ba sically mineral in composition. Low Cost--the most economical of our acoustical plasters. Versotilo--because it can either be applied by machine or by hand in a variety of appealing finishes. LIMITATIONS Audicote is designed for use on ceil ing and wall areas not subject to contact. Audicote is not recommended for use over radiant heating panels. While a rust inhibitor is used in Audicote Plaster, it is recommended that use of unprotected steel in the surface of monolithic concrete be minimized to avoid rust spotting of the finish. MIXING AND APPLICATION Machin* Mixing--Machine mixing is recommended. Add Audicote to water, using approximately 55 quarts of clean water per bag tor first coat of acoustical plaster. For machine application of finish coat more water will be required--"0 to 90 quarts, depending upon type of machine used and degree of texture desired. An increase in the amount of water used per bag will give a finer texture. If hand application of finish coat is required, use approximately 55 quarts of water per bag for finish coat. Mix lor minimum of five min utes in mixer to develop proper consistency. Hand Mixing--If required, material must be hoed sufficiently to develop even consistency tree of lumps. Machine Application--First coat of acoustical plaster should be ap plied to thickness of ?s", leveled with a darby and pointed up with a trowel if necessary to provide a smooth and level base for finish coat. Allow to dry before applying finish coat, which should be }-g" thick. Hand Application--First coat of acoustical plaster should be applied to thickness of 3 j". Level with a darby to provide a smooth and level base for finish coat, and allow to dry. Finish coat should be applied to a j 5" thickness. After finish coat has taken up sufficiently, it may be stip pled, stipple-perforated, darbied or floated to produce desired finish. a -o o tv o o O' 55' randum Specialized Lathing and Plastering Systems ROCKLATH Lathing Systems PAGE BRIDJOINT Lathing System ROCKLATH Resilient Lathing System 58 60 BRACE-TITE Lathing System 2-inch Solid ROCKLATH and Plaster Partition 62 65 Exterior Wall Furring System 68 Column Fireproofing TRUSSTEEL STUD-ROCKLATH Partition 70 71 I'SC has developed a complete line of attachment systems employing the use of clips tor attaching Rocklath Plaster Base to wood framing, metal grillage, Tressteel Studs and masonry walls. These systems are designed to provide performance and economy in the construction of plastered walls and ceilings which offer: 1. Greater resistance to cracking 2. Reduced sound transmission 3. High fire resistance 4. Insulation 5. Vapor barrier 6. Economy GP02 7 OOV-3 1 DESCRIPTION The Bridjoint lathing system uses Bridjoint clips to apply Rocklath Plaster base on walls and ceilings in such a manner that the ends 116-inch dimension) of the lath fall between and not on the framing members. The H" B-l field clip and B-2 corner dip are used for Rock- lath. A B-l field clip is used when } / Rocklath is specified. G P O Z 7 O D&* ADVANTAGES Crack Resistant--because ends of gypsum lath do not fall on framing members, resistance to cracking is increased at these vulnerable points. Adaptable--This system facilitates application of Rocklath over nail able steel framing. Use Rock lath with framing up to 16" o.c. and 1 _>' Rocklath for framing spaced up to 24" o.c. Economical--25*2^. less nailing is re quired than conventional nailing of Rocklath plaster base to wood studs. On wood frame construction Cornerite and nailings are eliminated in the internal angles. 58 I J DIRECTIONS FOR LATHING AND PLASTERING lothing-- Rocklath is applied in such a manner that the ends of the lath do not tall on the framing mem bers. End joints are staggered in adjacent courses. A Bridtoint clip is used at corners of each piece of lath to support the lath ends which fali between the framing members. Rocklath is nailed to the wood or steel framing. (See page 16 for nail specifications.) Plastering--plaster in two or three coats to 12-inch thickness. (5ee page 36 for plastering specifications.) Estimating Quantities--B-l clips, .5'2 per square yard; B-2 clips, one for each 16 inches of corner angles for ro'~r of total lineal feet of corner angles). 59 ROCKLATH RESILIENT uu..-n Syst.m DESCRIPTION Rocklath Resilient Lathing System uses steel spring clips lor attaching Rocklath plaster base to wood iraming, steel channels or masonry. These resilient clips float the Rock lath and plaster iree irom framing members. ADVANTAGES Resistant to Sound Transmission-- National Bureau of Standards as signs average sound transmission loss rating of 52 decibels to a wood stud partition with R-t resilient dips, gypsum lath and plaster both sides. Crack Resistant--plaster cracking due to framing movement is greatly reduced. Where framing movement occurs back of lath and plaster, it is absorbed by the spring dips in much the same manner as automobile springs soften road shocks. One Hour Firo Rating--wood stud partitions with R-l Resilient Clips, perforated Rocklath. and 1 Tinch g\ psum-perlite plaster proportioned 100 lbs. ; 2' i cu. ft. Scratch and brown coats) have a one hour tire rating. Economical--For a nominal increase in the lathing cost, the Rocklath. Resilient Lathing System provides outstanding sound and crack resist ance features. DIRECTIONS FOR LATHING AND PLASTERING Lathing--apply Rocklath plaster base face out with the long dimen sions at right angles to the framing members 16 inches o c. Stagger end joints. Rocklath ends must occur over framing members and be secured with dips. Place a dip at every inter section of Rocklath edges and fram ing members. Staple or wire-tie all corner bead to Rocklath. Do not nail Rocklath Plaster Base or ac cessories to framing. Where Resilient Rocklath ceiling joins conventional nail-on walls or partitions, a !s-inch thick furring strip iusually a strip of Rocklath 2 inches wide) should be nailed to joists at ceiling angle to compen-ate for wood stud or joist forming. R-2 for corners ond angles of wood frame construction. OPOZ7 OOT1 e I i FLEXIBILITY replaces rigidity without loss of strength; walls and ceilings are thus able to compensate for normal frame movement, and the plaster surfaces are protected against cracking. for the 1 3-inch furring or R-l Resili ent Clips. Cse a B-2 Bridjoint Cor ner Clip in place ot R-2 Resilient CornerClip. If nails are resilient and ceilings nail on. nail turring strip to the studs at the ceiling line. Do not use nails in corner angles. CAUTION Perforated Rocklath is not recom mended for use on ceilings uhen applied with resilient clips. Plastering -- plaster to W-inch grounds with sand or perlite aggre gates. On ceiling work use only plain for Va inch steel furring channels, in ceiling construction. Rocklath and apply plaster in three coats (do not "scratch-doubleback"). Where one hour fire rated wood stud partition is required, plas ter to J-^-inch grounds with gypsumperlite plaster proportioned 100 pounds gypsum plaster to 2\ > cubic feet perlite (scratch and brown coats). Estimating Quantities--R-l, R-3, R-5 clips--Estimate S\i t0 6 per square yard. R-2 clips -- 1 for each 16 inches of corner angles (or oW of total lineal feet of corner angles). R-l and R-2 combined. 6 per square yard. P.R for masonry or solid concrete con* r BRACE-TITE Lathing Systems DESCRIPTION The Brace-Tite Lathing System attaches Rocklath piaster base to standard metal grillage (3i'-inch cold rolled channels not over 10 inches o.c.). This system is also used as a base tor direct application of acousti cal tile. ADVANTAGES Versatile--may be used lor plastered ceilings or tor acoustical tile base without plaster. Strong--gives support across the full width of Rocklath. Clip provides spring tension to the center. Eo*y to Erect--requires no special tools. Maximum spacing of chan nels 16" o.c. Two-Coot Plastering--permits use of scratch double-back method over plain or perforated Rocklath. Plas ter thickness is J^-inch. Fireproof--fire resistive ratings of one to four hours are obtainable. DIRECTIONS FOR LATHING AND PLASTERING Lathing--1. Place starter clip over ?4-inch channel at juncture of chan nel and side wall. (Xote: If hot rolled channels are used, hand crimp dips tojit snugly over channel legs). 2. Place Rocklath plaster base on top of starter dip loop and at right angles to channel. Engage BraceTite field dip over channel and hook it into starter clip loop. On first course of lath, crimp field GP027 0075 BT-1 STARTER CUP, uie ot beginning of channel run. B-1 BRIDJOINT CUP, use at each ROCKLATH cor ner. 8-1A 8RIDJOINT CUP, use at each ROCKLATH comer. 62 I clip wire to accommodate slack caused by starter clip loop project ing from wall. (See B.) L se B-l ; Bridjoint clip at each end joint of I kith on rirst course only. I End joints should be staggered j and tall between channels. Use a B-l Bridjoint clip on both sides of lath end joints, See tO. Upon completing ''l a course of Rocklath. slip a B-l Bridjoint clip over each end joint so that it is firmly supported. A 3. After first course of Rocklath is FIGURE A completed, no further crimping of wire is necessary. Nucceeding courses are rapidly applied by looping each field clip over channel and inserting hook into eye of preceding field clip. Complete last course by cutting Rocklath to fit remaining space. Hang field clip over channel end, insert hook end under preceding clip, pull back and snip off excess length. BRACE-TITE Acoustical Lathing system. Place the full loop end of Brace-Tite Acoustical clip over end of each 34 inch channel at juncture of channel and wall. Rocklath plas ter base shall be applied at right angles to channels, and the half loop end of the field clip snapped over the inch channel. Succeeding . courses shall be applied in same manner using Bl-A Bridjoint clips 'prongs fiat on tile side) in lieu of the B-l clips used for plastering. Plastering--apply gypsum plaster in two or three coats 1 A-inch thick, using sand or perlite as aggregate. If one hour fire rating is required, apply psum-periite plaster proportioned FIGURE C 63 MOO e l 1 100 lbs. : 2'> cu. it., 2s-inch thick over perforated Rocklaih. Estimating Quantities--ior p^-inch channels, 16 inches o.c.: one BT-1 Starter Clip tor each channel abut ting a vertical plane and at any interruption of channel. 5T2 to 6 BT-1 or BT-A Field Clips per yard. j'..> to 4 B-l or B-1A Bridjoi.vt Field Clips per card. For ?i-mch channels, 12 inches o.c.: BT-1 Starter Clips, same as before. > to 8 BT-I or BT-A Field Clips per yard. B-l or B-1A Brid;oint Field Clips, same as for 16inch spacing. GP027 0075 64 2-IN. SOLID ROCKLATH and Plaster Partition DESCRIPTION A studless non load-bearing partition consisting of } >-inch V-edge, Long Length Rocklath plaster base, held vertically by floor and ceiling run ners, up to 12 feet in height, and plastered on both sides, ADVANTAGES Save Space--Saves 40 to 60 per cent of space occupied by conventional partitions. In every five lineal feet a 2" partition creates one extra square foot of usable space over a 41 i partition, Lightweight--only 16 pounds with gypsum-sand plaster and 9 pounds with gypsum-perlite per square foot of finished partition i25r,' to 40ir7 lighter than commonly used masonry partitions). Strong--official impact test rec ords show that a 60 pound weight traveling through a full arc fall of 4 feet failed to produce a discernible crack on a lull size partition alter three successive blows. One Hour Fire Rating--with gyp sum plaster sanded 1:1 for scratch and 1:2 for brown coat or gypsumperlite proportioned 100 lbs. to 2 cu. ft. on scratch coat and 3 cu. ft. on brown coat. Where one hour fire rat ing is not required, plaster may be sanded 1:2 for scratch and 1:3 for brown coat. DIRECTIONS FOR LATHING AND PLASTERING Floor Runner--USG Metal base or wood runner. Indicate positions of floor runners with chalk lines. When USG Metal base is used, metal floor clips should be nailed approximately 24 inches o.c. Snap metal base side plates over shoulders of the clips. Wood runner should be milled lUs x 2 inches from select stock re sistant to splitting. Ceiling Runner* -- Apply USG L-shape ceiling runner using J-j-inch GP027 007S 65 J *. I concrete stub nails or power driven nails approximately 24 inches apart. Nail to a line plumbed up from center line of door runner. If ceiling is suspended type, wire-tie L-shape runner to lath. Grouting--Fill metal base with gyp sum grout using uniform V-groove. Recommended grout mixtures: 100 lbs. gypsum plaster to 21 > cu. ft. of perlite, or 250 lbs. of sand. All metal door bucks shall be grouted, providing uniform V-groove prior to erection ot lath. Lathing--Cut Long Length Rocklath to allow a minimum of 14-inch and a maximum ot 1*4 inches top clearance. Set in V-grooved base sec tion with top edge against vertical flange of ceiling runner. Edges should be piumb and butting. To hold lath to ceiling runner, snap two L'SG Ceiling Runner Clips through the top or center row of slots. Lath is cut and tit closely around conduits, outlet boxes and steel door buck struts. One side of opening is covered with metal lath strips backed with X'o. JO asphalt felt (usually 5 to 5 inches widej applied with hand stapling machines. Partitions up to 9 feet high) are then horizontally braced in the fol lowing manner, see photo below: 66 _______J GfOZT OOTT (11 Punch hole in center of each lath slightly below mid-point lor bracing clip; 1,-1 insert bracing clip; (.3) spring a partition length !a-inch cold rolled channel into bracing clip with channel legs pointing down; (4) insert remaining bracing clips and spring channel into place; (5) wiretie channel ends at abutting parti tion angles to cornerite; (,6) parti tions 9 to 12 teet high require two horizontal braces at third points in stalled as described above; (71 wedge vertical brace (usually wood l.x4's or 11 -i"xl * 2" angle iron! between floor and ceiling every 6 feet and wire-tie to horizontal channel Plastering--Apply a full i^-inch thick scratch coat of plaster with maximum of 3 hour set, to each side of the lath. In no case should application of scratch coat to second side of lath be delayed longer than the setting time of the scratch coat applied to the first side. Scratch lightly in horizontal direction only. Let scratch coat set a minimum of 16 hours before browning. Apply the brown coat as follows: (1) After the scratch coats have set firmly and have partially dried, the brown coat should be applied to the unbraced side, bringing it out to within !(e-inch of ground dimension tor finish coat. (2) When this brown coat has set firmly, (not less than 3 hours) remove braces carefully from opposite side and apply brown coat to that side in similar manner. GP027 007$ 67 f I EXTERIOR ILL FURRING s,s,em DESCRIPTION A simple practical system for furring exterior masonry walls using L'SG Adjustable Wall Furring Brackets, `4-inch channels and Long Length Insulating Rocklath (? 3-inch thick by 24-inch x ceiling heightl. ADVANTAGES USG Furring Bracket--Heavy gauge galvanized steel with serrated edge which holds channel firmly in place. Permits proper wall alignment. Adjustable--uneven walls can be furred quickly to true, even surface without expensive, time consuming 'shimming." Low Cost--large 2 ft. wide ceiling high sheets of long length Rocklath plaster base go up quickly. Lni- formly even plaster base saves plas tering material and labor. Vapor Barriar--provides inexpensive and efficient safeguard against con densation within the wall. Insulation--offers the equivalent of ! 2-inch of fiber insulation board when erected with the required minimum air space between exterior wall and lath. DIRECTIONS FOR LATHING AND PLASTERING Application of Metal or Wood Floor Runnor--Nail single metal base clips to rough floor not over 24 inches o.c. Snap the sideplate over the clips. Fill the back of the base with grout and form a V-groove as grout stiffens and before it sets providing a ?i-inch t>l OO IZ O dD txriCAl FURRING OF EXTERIOR MASONRY WALL 68 ground for plastering. Alternate. A milled wood runner may be attached to the rough floor by nailing with cut nails or concrete stub nails in the center groove. Application of Coiling Runner-- Attach L-shaped ceiling runner to the construction above as required, locating it by plumbing up from the floor runner. Where furring does not extend to the construction above, install horizontal iurring channel 4" to 6'' below top of lath. Application of Furring -- for furred walls up to 9 feet high, locate furring brackets to the masonry walls not over 4 inches from columns or other abutting construction. Locate brack ets at third points vertically and not over 36 inches o.c. horizontally. For walls from 9 to 12 feet, locate brackets vertically at quarter points. Set brackets in mortar joints or use 2-inch cut nail to attach bracket to mortar joints of brick, clay tile or cement block, or in the held of light weight aggregate blocks. Use one j^-inch concrete stub nail or one power driven nail per bracket on monolithic concrete. Lay 34-inch furring channels horizontally on the furring brackets with the legs down, plumbed in line with the base. Wire tie to the bracket with a double strand of 18 gauge tie wire. Bend down excess bracket length. Lathing--Apply gypsum lath with the long length vertical, butted light ly with the foil facing the furred space. Set bottom of lath in the groove of base grout, clipping top of lath to the ceiling runner and v,ire-tying (over a nail) at the edges to intermediate horizontal channel furring. Cut and fit gypsum lath to allow *4" clearance around window frames. Apply a 3-inch strip of metal lath over each Rocklath Plaster Base joint under window. Plastering--Apply scratch, brown and finish coats to a full ?'4-inch over face of lath. Cut plaster base coats with the edge of the trowel along margin of metal window frames. and PLASIER 1, l/j, 2, 3 AND 4 HOUR FIRE RATINGS DESCRIPTION Rocklath Plaster Base wired in place against structural steel column, and plastered with gypsum cement plaster and sand or perlite aggregate in proportions and thickness required to give tire rating desired. In certain higher ratings, 20 gauge galvanized l-inch hexagonal mesh wire fabric is used in addition to the Rocklath. ADVANTAGES Fireproof--column tire ratings of 1, ll j, 2, 3 or 4 hours are obtained. Lightweight--6 pounds per square foot of completed surface area for l hour protection to 11 pounds for 4 hour protection. Low Cost--Standard materials used. Easily attached, economy of plaster ing over gypsum lath. 1-1 !/2 Hour Rating^/i"--16"x48" Perforated ROCKLATH, cut as required, is opplied vertically against the column and fastened with a double strand of 18 gauge tie wire approximately 2" from the ends and 15" o.c. 1-A bead, set at each corner, establishes Vi" plaster grounds for 1 hour and */" grounds for I/2 hour ratings. Apply gypsum-sand plaster proportioned 1:2/2 and any finish coat. A 2 Hour Rating is obtained by lath ing in the same manner as indicated above except that the I-A bead must be set to establish 1" plaster grounds over the lath and gypsum-perlite plas ter, proportioned 100:2/2 must be used. 3 Hour Rating--Loth the some os for I hour rating except set 1-A bead to provide 1 grounds by snipping ex panded flanges 12" o.c., bending bock and stapling to ROCKLATH. Apply Gypsum-Perlite plaster propor tioned 100 lbs.: 2 cu. ft. for scratch coat and 100 lbs.: 3 cu. ft. for brown coat. Use any standard finish coat. 4 Hour Roting--Apply a double thick ness of Vi" long length ROCKLATH Plaster Base cut as required, vertically against the column and fastened with double strand of 18 gauge tie wire about 4" from top and bottom and 24" o.c. Wrap hexagonal 20 gauge galvanized wire fabric over the lath and set 1-A bead to establish 1 Vi" grounds. Apply gypsum-perlite plaster proportioned 100 lbs.: 2 cu. ft. for first of thickness and 100 lbs.: 3 cu. ft. for second V*n. Use any stan dard finish coat. 70 GP027 0031 ; TRUSSTEEL STUD rocklath Partition Assembly DESCRIPTION A non-load-bearing partition of Trussteel Studs, Rocklath Plas ter Base with Trus-Lok Clip attach ment, and plaster. Over-all thick nesses: 4'A", Sla", 6", and 8", depending on stud width. ADVANTAGES Flexible--The open web design of the Trcssteel Stud allows encase ment of small pipes, conduits, heat controls, and small ducts horizon tally and vertically without weaken ing the partition structurally by chasing. Web members are easily cut for larger pipes or ducts. Versatile--Hi', 3 J^", 4", and 6" Trcssteel Studs provide wall thick nesses to meet job requirements. Strong--Strength of studs is derived from strategic use of metal in a truss design--not from bulk weight. The partition assembly of Trussteel Studs, Rocklath plaster base, and plaster has more than adequate strength for building construction practices and is nationally accepted by building code authorities. GP027 0032 71 lightweight--This partition assem bly weighs approximately 10 lbs. per square foot when plastered with per lite aggregate plaster, and approxi mately 15 lbs. per square foot with sand aggregate plaster, in any Trussteel Stud width. Fir* Resistant--Built of incombus tible materials. One hour fire rating is obtained when perforated Rocklath plaster base is used and plas tered with gypsum-sand plaster 1:1, 1:2, or with Structo-lite plaster or gypsum perlite 100:2]^. Sound Reduction--This partition assembly has good resistance to sound transmission, attaining aver age sound transmission loss ratings of 48 decibels with sand aggregate plaster, and 44 decibels with perlite aggregate plaster, in tests at a na tionally recognized laboratory. Economical--Material costs are low, job erection fast--provides installa tion economies for mechanical trades. DIRECTIONS FOR LATHING AND PLASTERING Lathing--install Trussteel studs not over 16 inches o.c. (See pages So8/ for details.) Studs shall be located approxi mately T from all door buck jambs, abutting partitions, or other con struction. With steel bucks, an additional anchorage stud is required at each jamb. All corners shall be framed with a stud approximately 2" from each side of the internal angle. Securely wire-tie studs adjacent to door bucks to the jamb anchors. Start lath application at the bot tom with long dimension of Rocklath at right angles to the stud. The first course of lath shall be set in 72 GP027 00J3 TL-2 Starter Clips spaced approx imately 16' on center along the run ner track and secured to the studs bv TL-1 Field Clips hooked around the stud and over the top of the lath. The end joints of the Rocklath shall occur between studs, staggered in alternate courses, and joined to gether at the corners with B-l Bridjoi.vt Clips. Where wood grounds are wire-tied to the studs the lath shall be held in place by driving a nail into the ground at each stud, with the nail head held tight against the lath and projecting up from the ground of an inch. Succeeding courses of Rocklath shall be attached by inserting the lath into the top portion of the TL-1 Field Clips of the preceding course and securing the top edge of the lath to the studs with TL-1 Field Clips. The top course of lath shall be cut to the width required, B-l Clips placed on the previous course of lath in each stud space and the lath se cured to the runner track with a TL-3 Finisher Clip driven into the lath, or shall be secured by wiretying tnroueh the lath around the stud or stud shoes with a double strand of tie-wire twisted tight over a nail on the face of the lath. In the case where ceilings are lathed the last course of lath shall be cut to fit as required and held in place with cornerite stapled to the Rocklath and wire-tied or stapled to the ceiling lath. The course of lath immediately over metal frames shall be set in a groove provided in the grout, if grout is used, or shall be set in TL-3 Clips clipped to the runner track, or shall be wire-tied to the studs over a nail on the face of the lath. Where ceilings are lathed, the last course of lath shall be cut to fit as required and held in place with cornerite stapled to Rocklath and wire-tied to metal lath. Cornerite shall be used on all in ternal angles, and corner bead at external corners, by stapling to Rocklath plaster base. Metal lath reinforcement over frame corners shall be 13H" x 19* pieces or 9" x 48* strips of 2.5 lb. self-furring metal lath stapled to the Rocklath. Metal door frames shall be securely anchored to the floor by two power driven anchors or equivalent attach ment through a clip at each jamb. Jamb anchor clips shall be welded in each jamb at top, 12' down from top, 27" from top and 18' from bot tom. Use runner track at head of buck to receive studs over opening, runner to turn up 4" each side at the jambs and wire-tied to studs used as door frame struts, or use a hori zontal channel extending to third stud each side of frame approxi mately 4" above frame to which studs are tied and grout in over frame. Secure studs to jamb anchor clips by engaging in notches and wire- tying securely in place, using double strand of iS-gauge tie wire. If wood door bucks are used call for rough bucks of same width as &P02 7 0034 73 i J studs, and of not less than \Ys' stock with the jambs running to underside of construction above and well anchored top and bottom. For stair rails, lavatories, etc., bolts welded or locked to channels, angles, or plates shall be anchored to studs prior to lathing. For cabinets, 1' wood grounds may be tied to studs prior to lathing or 8-A picture mould may be tied over Rocklaih to studs. Plastering -- plaster to '.-2-inch grounds using gypsum-sand or gyp sum-perlite plaster. Plaster may be applied in two or three coats. Grout ing steel frames with plaster prior to lathing is recommended. Estimating Quantities--for studs spaced 16 inches o.c.: TL-2 Starter clips, two for each Trussteel Stud; TL-1 Field Clip, 5'^ to 6 clips per square yard each side; B-l Bridjois't Field Clip, 3!-2 to 4 per square yard each side. Figure Two TL-3 Finisher Clips per stud if lath goes to underside of concrete slab, otherwise figure wire tieing or cornerite depending on conditions. GPOZT O O f5 74 J Specialized Lathing and Plastering Systems 4 Metal Lathing Systems l PAGE Metal Lath Resilient Lathing System 76 2-Inch Solid USG Metal Lath Partition 78 TRUS5TEEL Stud Metal Lath Partition Metal Base 80 84 GP027 0086 75 METAL LATH RESILIENT Lathing System DESCRIPTION A system composed ot metal lath, steel furring members and spring clips that provides a floating attach ment of plastered surfaces to struc tural members. ADVANTAGES It offers greatly increased protection against plaster cracking due to struc tural movement, and a considerable reduction in the transmission of sound through walls and ceilings. It is adaptable to wood supports, sus pended ceilings, hollow partitions, and masonry or concrete surfaces. ESTIMATING QUANTITIES No. 100 Clip, runner channels o'-O' o.c.. furring channels 12 inches o.c.: 340 clips per 100 sq. yds.; furring channels 16 inches o.c.; 264 clips per 100 sq. yds. No. 200 Clip, walls (clip spacing 16 GPOZ? 0 0 * 7 Suspended Ceiling--Showing opplication of No. 100 Clip for suspended ceiling con* struction. The dip provides resilient attach* ment of furring channel to runner chonnel by repiocmg use of the tie wire. Easy to erect. Wood From* Contraction--Showing ap plication of No. 200 Clip on wood studs and joist* and on wood furring on masonry walls. Clips provide resilient attachment of metal lath and protect plaster finish. 76 inches o.c. along studs spaced 16 in. o.c.), 610 clips per 100 sq. yds. Ceil ings (clip spacing 12 inches o.c. along joist spaced 16' o.c.), 744 clips per 100 sq. yds. No. 400 Clip*, Trvssteel Studs, 16 in. o.c., clips spaced 12 inches o.c., 780 clips per 100 sq. yds. Spacing 16 inches o.c., 600 clips per 100 sq. yds. No. 500 Clip Spacing of furring Channel*, o.c. Spacing of Clips Quantify of Clips per 100 sq. yds. 12 inches 24 inches 496 16 inches 18 inches 504 24 inches 12 inches 496 GP027 0 0 3 * Moaonry Surf oeaa--Showing use of No. 500 Clip on ceiling under concrete joist and on masonry walls. Clip is also used on other masonry surfaces. Provides furring and resilient attachment of metal loth. TRUSSTEEL Stud Partition--Showing use of No. 400 Clips spaced 16 inches along studs. A %* pencil rod is wired into the notch on outside flange of clip to provide resilient furring member for metal lath. CLIP Na 400 TBUSSTIEL STUO PARTITION 77 GPOZ7 0 0 8 9 2-IN. SOLID USG METAL LATH and Plaster Partition DESCRIPTION A non-load bearing partition that finishes to an overall thickness oi 2 in. May be erected using f4 in. chan nel studs with Diamond Mesh metal lath or with jhg in. Riblath without channel studs. ADVANTAGES Saves Space-- saves 40^ to 60^ of the space usually occupied by con ventional partition. One Hour Fire Roting--when plas tered with sanded plaster mixed 1:2, 1:2 for scratch and brown coats. Highly Crock Resistant Good Sound Transmission Rating-- 38 average decibel transmission loss, lightweight--only 18 lbs. per parti tion square loot with gypsum-sand plaster. DIRECTIONS FOR ERECTING Stud Partition --Snap partition lines 78 on floor and ceiling . . . Fasten Z- lath to USG L-type ceiling runner type ceiling runner to ceiling ... At nailed to the bucks ... Provide tem I tach double base clips, 16' o.c., to structural floor with concrete stub porary bracing by placing % in. channel horizontally near mid-height nails. (See page 84) .. . Insert M in. of partition for partitions up to channels into floor clips and fasten 9'-0* height. Partitions 9' to 12'-0' to ceiling . . . Wire-tie Diamond high require two horizontal braces at Mesh lath in conventional manner third points tie to lath 24 in. o.c. . . Snap on metal base side plates Place a vertical \Vi in. angle brace > and grout base. not over 6 ft. o.c. to hold the lath Sh>dla*f Partition--Snap partition in position until brown coat on side lines at floor and ceiling... Fasten opposite bracing has set. phsd 1:2, ts. ting-- n loss, parti3-sand NO 1 lines L-type ceiling runner to structural ceiling or furred-down ceiling... Attach double base clips, 24' o.c., to structural floor with concrete stub nails, snap side plates in place and grout, leaving V-groove to receive 3'g in. Riblath . . . Erect ceiling height l/% in. Riblath vertically by dropping into grouting groove and wire-tying top to L-type ceiling run ner not over 8 in. o.c. . . . Metal door bucks shall be provided with clips along jamb and wire-tie the in. Riblath to these clips . . . Where wood bucks are used, wire-tie the DIRECTIONS FOR PLASTERING 2 In. Solid Motal Lath Partitions-- Apply scratch-coat to side opposite braces or channels, allow to set and partially dry ... metal door frame shall be slushed full with plaster. .. On studless partition apply browncoat to side opposite braces and al low to set before removing braces. Apply brown coat to previously braced side bringing it out to finish grounds. On stud partition, apply back-up coat on channel side to full grounds. Apply brown coat to lath side. Apply finish coats to both sides. 79 r 1 t ____ j TRUSSTEEL STUD UAL LA1H and Plaster Partition DESCRIPTION This truss design stud permits the erection oi hollow, non-ioad bearing partitions in which ducts and pipes can be easily fitted and concealed. ADVANTAGES lightweight--Finished partition weighs 13 to 17 lbs. per square loot. One hour fire rating--when plas tered with gypsum--sand mixed 1 .2, 1.2. Strong--Withstands up to 30^ greater transverse loads than l,1 > in. steel channels. Economical -- Requires no special tools or structural framing, goes up fast. Can be used with metal lath or Rocklath plaster base. This system is available in the following sites: Stud lengths, 7 to 20 it.; stud widths. 2'1, 3>4, 4 and ! 6 in. It contains the following parts I as shown in sketch at right: (A) 22 gauge top and bottom runner tracks; (B) 7 gauge rod studs spot welded. (C) Shoes tor attaching studs to run ners. These shoes allow an adjust ment up to 3 in. .-r' GP027 0071 1 80 s' i a. ! * e I j STEP BY STEP ERECTION Runnor track ii aligned and attached to concrete floor and ceiling with stub nail* at 2 ft. intervals, or wired to suspended ceiling every 24". Studs are secured to runner track by meons of two snap-on attachment shoes at top and bottom by inserting flange between runner track and floor or ceiling, Leg of thee is then snapped over side of stud and wire tied. Metal lath is applied to both sides of studs with I 8 gauge galvanized tie wire. RECOMMENDED STUD SPACING TRUSSTIEL 1 Type of lath Stud Spacing j 2.5 lb. Diamond Mesh Lath 3.4 lb. Diamond Mesh Lath 2.75 lb. '/" Riblath 3.4 lb. Vt" Riblath 3.4 lb. Vt" Riblath 4.0 lb. W Riblath V\ ROCKLATH Plaster Base 12 inches 16 inches 16 inches 19 inches 24 inches 24 inches 16 inches FINISHED PARTITION THICKNESS AND LIMITING HEIGHTS Stud Width Finished Wall Thickness Metal Lath and Piaster--Nermal Grounds Maximum Partition Haight Studs 24" 19* 16- 2'/j" 3 'A" 4" 6" 4" 4 V." 5 Vi" 7Vi~ 9' 14' 15' 1 3' 18' 21' 16' 20' 22' 20' 24' 26' GP027 0092 81 I GENERAL DATA FOR PARTITIONS . Caataartiaa Total Wright lha. par tg. ft. ----------------- y Hollow PVROBaR Tile-------------- plastered two sides 21 4* Hollow PYROBAR plastered one side 20 4" Hollow PYROBAR plastered two sides 25 2' Solid ROCKLATH 16 Same 10 2* SOLID Metal Lath (studs) 18 Same (studless) 18 TRUSSTEEl stud -- metal lath 19 nMr and AggragaN Gypsum sand 1:3, 1:2 Gypsum sand 1:3, 1:2 Gypsum sand 1:3, 1:2 Gypsum sand 1:2, 1:3 Gypsum-perlite 100:2, 100:3 Gypsum sand 1:2, 1:2 Gypsum perlite 1:2, 1:2 Gypsum sand 1:2, 1:3 | TRUSSTEEl .tod--ROCKLATH 15 STRUCTO-UTE or Gypsum Sand 1:2 perforated ROCKLATH GENERAL PLASTER BASE DATA FOR CEILINGS I Ceedmliee Plaster and Agfreyde 1 Steel joists--metal lath Same Same 2,/i" reinforced concrete slab on riblath Steel joist construction with metal lath furred or suspended Same Same H* Perforated ROCKLATH attached by BRACETITE system--channels 16" on centers Same as above plus 14 gauge diagonal wires through dipt Some as above except channels 1 2" on centers and 1 4 gauge diagonal wire through dips Vt' Perforated ROCKLATH attached by BRACETITE system--channels 12" on centers and 20 gauge hex, mesh 82 gypsum sand 1:2, 1:3 y*' gypsum perlite 100:2, 100:3 1* gypsum perlite 100:2, 100:3 " V** gypsum sand 1:2, 1:3 3/>%" gypsum perlite 100:2, 100:3 1' gypsum perlite 100:2, 100:3 Vt" STRUCTO LITE Plaster or gypsum perlite 100:2, 100:3 '/a" STRUCTO LITE or gypsum perlite 100:2'/a Vt" STRUCTO LITE or gypsum perlite 100:2'/i 1" STRUCTO LITE or gypsum perlite 100:2Vi O -o o IN) o o J J I' - TMitatw 4 VS 4 54' 5%' 2' 2' 2' 2' 4% to 7%' 4/1 to 8' Fir* Rating. Rafawiico 3 hours 3 hours 4 hours 34 hour 1 hour I hour 1 hour 1 hour 1 hour lw< In- Mm Lou Mill 39 decibali 43 d.b. 37 d.b. 37 d.b. 38 d.b. 37 (o.t.l 40 44 to 48 lias. Haight 1 3 f*at 17' 17' 12' 12' 14' 8'4' 14 to 20' Dapandlng on width. Fir* Rating I R*fr*ne ! 2 houn 3 hours 4 hours 2 hours 3 hours 4 hours 1 hour ------------------------------------------------------- a----- 2 hours 111 O ------------------- fst -- 3 hours ----------------------------------------------------------------------------------- O ------o 4 hours * 83 I USG METAL BASE DIRECTIONS A "piastered-in'' metal base system for partitions and walls, composed ot door clips or masonry wall clips and steel side plates. May be used with metal lath or Rocklath plaster bases or masonry piaster bases. Side plates: 18 gauge steel, 10 t'eet long by 2} > inches high. ADVANTAGES Eay Application--Snap-on attach ment feature permits faster installa tion with automatic and independent adjustment on any rough or finished floor. Versatile--Internal and external cor ners can readily be formed on the notching tool. Safety--Adds no combustible mate rials to the construction and protects base of the partition. USG METAL LATH For Column Fireproofing This time proven system provides a 1, 2, 3, or -I hour fire rating. It util izes self-furring Diamond Mesh lath and accessories and typical metal lath construction. Grounds: One hour--1 + " gypsum sand 1:2, 13; two hours -- 1" gyp sum-perlite 100:2, 100:3: three hours -- l3 s" gypsum-perlite 100 2, 100 3: four hours --I-**" g> psum-perlite 100:2, 100:3. rC 9 i tfc O O iiJ O d O j USG READY-FORMED METAL ARCHES DESCRIPTION I'SG Metal Arches are the practical and easy way to form symmetrical arched openings in either new con struction or remodeling. Precisionmade for doorways and recesses. Available in three styles, seven sizes for finished openings 20" to 70J^". L'SG Metal Arches are made of gal vanized steel, perforated for proper plaster keying. ADVANTAGES Varsatil*--Choice of size or style. Easy to vary size and shape for any size openings and partitions of any thickness by combining sections in various combinations. Eoty to oroet--ready to put in place as they come from the carton. There are no forms to make; no corner bead to bend or shape by hand. No special preparation of the rough opening is necessary. Economical -- Since these arches combine plaster base, corner bead and plaster grounds, there's a saving in time, labor and materials. DIRECTIONS FOR ERECTING The arch sections fit perfectly over 2x4 studs and any type lath, or over masonry of similar width. For other partition thicknesses merely split arch soffit, overlapping for thin partitions and filling in gap with metal lath for thicker walls. Studs on each side of the arch should be spaced inches wider than the desired finished opening. Assemble the metal arch units on the floor. Join the units, using connector pins. Strike exact center of the opening on header. Then insert the assembled metal arch in the opening over the lath. Xail in place, temporarily. Then level the arch and nail it se curely in place with lath nails through the solid part of the flanges. Vertical corner beads are aligned to the metal arch with connector pins. TRUE CIRCLE ARCH No. 11 -- 10" rodluo No. 22-- I5H" radio* GP027 0096 GOTHIC ARCH No. 33--2' TVi' flnithod opening No. 44--4' 1'/t' flnithod opening 1 ELLIPTICAL ARCH No. 36--3' 1 Vi" flnithod opening No. 55--5' l'/i" flnithod opening No. 66--5' 101/]" flnithod opening 85 Style f Arch Width of Finished Opening Dimension tram Arch Base to Header Spacing between Studs or Sucks (Rough Opening) oK) - No. 11 10' No. 22 31 '/,' 15%' . No. 33 31'/j* 11%' ' No. 36 37'/,' 11' No. 44 49 Vi* 12'/j' - No. 55 61'/,' 13' No. 66 70'/,' 13' 21'/, 33' 33' 39' 51' 62' 72' GP027 0097 86 Plaster Problems RemediesTheir Causes and Basecoat and finish coat plasters are so closely interrelated that the treatment of problems pertaining to their use will be handled simultaneously in the following pages. All Red Top basecoat and finish coat plasters are carefully manufactured and thoroughly tested before shipment, and any troubles or problems experienced in their use are normally found to be caused by job conditions. 87 J GP027 0 0 7 * INTRODUCTION As a general rule, most plaster problems result from the following conditions: 1. Atmospheric conditions. 2. Conditions due to set --fast or slow. 3. Improper heat and ventilation. 4. Improper application or thick ness of basecoat or finish coat. 5. Improper proportioning of aggre gate or improper mixing. .6 Improper workmanship. 7. Improper plaster base applica tion. .8 Improper bond. 9. Poor aggregate (improper grada tion, impurities, etc.). Plaster problems are classified under the specific type of condition which exists. These problems are dis cussed in order under these following types and specialty products: 1. Plaster Cracks. 2. Weak, Soft Walls. 3. Bond Failures. 4. Set and Working Qualities. 5. Color, Surface Stains and Blem ishes. 6. Acoustical Plaster Problems. 7. Cover Coat Finish Plaster Problems. PLASTER CRACKS It should be understood in reviewing this broad subject that a plaster slab is not a delicate material and will take considerable abuse without cracking. It cracks only when some excessive external force is applied, 88 or when some excessive internal strains are induced within it. The stresses, conducive to cracking, are normally caused by movement in the building frame, or other components of the building over which plaster is applied, or by variations in the at mosphere surrounding the plaster slab. Cracking of plaster occurs more readily where the plaster slab is weaker or thinner than standards permit, and if stresses are encount ered before the plaster is dry and has attained full strength. Proper plaster bases are important to prevent plaster cracking. They also must be sound--this is equally important in the foundations and in the structural framing. Structural weaknesses cannot be corrected in lath and plaster work. One of the largest single factors causing plaster cracks is the lack of understanding the need for and use of proper heat and ventilation. Cracking of Partitions installed in lino with tha face of concrete col umns and beams--Reinforced con crete frame buildings and steel frame buildings with columns and beams encased in concrete may induce cracking of plaster in partitions when such partitions are located so that the plaster plane continues from the plaster base over the column and/or beam face, and is bonded to the concrete. This cracking can occur either at the joining of the concrete and the plaster base, or in the field of the partition, whether the plaster O ^ O 4) d J base is masonry, metal lath or gyp sum lath. The cracking is caused by difference in movement between the concrete and the partition mass -- the severity of cracking varying with the age of the concrete and the at mospheric conditions at the time ot plastering. The cracking tendencywill be reduced if the concrete has aged a year or more, or when build ing temperatures are moderate and stable tor a reasonable time prior to plastering. In normal construction, where plastering occurs four to eight months after the pouring of concrete, and is frequently done during colder and changeable temperature conditions, cracking may be minimized or elimi nated by either, (1) relocating the partition to come several inches back from the column and/or beam face, or f2) if plaster base is installed in line with column and beam by ap plying heavy paper (X'o. 30 asphalt felt) over the concrete, lapping onto the plaster base about 1 inch, and then applying diamond mesh metal lath over the paper, scatter-nailing it 12" on center to the concrete, using stub nails, and fastening it to the edge of the plaster base by nailing to masonry, wire-tieing to metal lath, or stapling to gypsum lath. This avoids a bond of the plaster to the concrete, thus reducing stress due to movement of column or beam in relation to the partition mass. ____ 1 89 I PLASTER PROBLEMS AND REMEDIES Becdu> of variation* in market practices, aggregates, plaster bases, weather and workmanship, GP027 013L this chart has been prepared to assist in the understanding, diagnosis and treatment of job problems. CONDITION 1. Connected vertical and horizontal cracks at somewhat regular intervals often in "stepped" pattern. n x 2. Cracks over and from corners of openings. MATERIAL Plaster over ony sheet lath: metal or gypsum. Plaster over unit masonry Plaster over brick, clay tile or cement block. Plaster over lath bases. CAUSE Plaster too thin, insufficient plaster grounds. Weak plaster. Stress from differential structural movement. Lath not properly applied. Structural movement of masonry units. Lintel construction is poor. Improper from# construction. Plaster too thin. Weak piaster. Failure to use metal lath reinforcement. REMEDY OR PREVENTION Reinforce and patch. Apply to proper thickness. j See "Weak Soft Wolls," Page Reinforce and patch. 1. Remove enisling lath and plaster and then relath properly and replaster. 2. Where condition exists on ceilings and joists will support weight of new plastered ceiling, nail wood furring strips across joists on 16* centers with embedment of nails at least 1 V*m into joists, then apply gypsum lath across noil* ing strips and replaster. 3. Nail self-furring 3.4 diamond mesh metal lath into joists, with embedment of nails at least I Vi* into joists, and replaster. Cut out, reinforce ond patch. Correct masonry construction. Patch. Prevent by using proper frame and lintel construction with metal lath reinforcement. Patch. Apply to proper grounds. See "Weak Soft Walls," Page Cut out, reinforce, and repair. M--' ------- - -----------------' " ~ \ 3. fine crocks, random pottem, generally l* to 3' apart. "Shrinkage cracks" "Croijng" "Ailigaloring" "Chip Cracks" fine cracks, irregular pattern, generally 6* to 14* apart. "Map cracking" 4. Crocks in random potfern usually less than 12* apart, Map, Shrinkage or fissure crocking pottcrn. GP027 0 102 Crock. ii.ga,.,uu lime putt) t; nish over gyp*vm bosecoat--any ploster base. Cracks in trowel finishes over gypsum basecoat-- unit mosonry plaster base msurncienl gauging plaster-- shrinkage of lime. Insufficient troweling during set Basecoat too wet or too dry and too little or too much suction finish coat applied loo thick, Improper timing of final troweling, Retempering of gauged lime putty finish coat on board. Stress from differential movement of plaster base. Cracks in trowel finishes--over gypsum basecoat-- lath bases Basecoat over masonry. Plaster too thin, insufficient plaster grounds. Weak plaster. High suction of masonry bose. Under aggregating of basecoat. Slow set. As result of dry-out condition. Trowel with speckling putty and apply USG Sealer. Prevent by using sufficient gauging plaster, water troweling sufficiently, or prop erty conditioning the basecoat before apply ing finish. Excessive thickness is conducive to shrinkage. Apply to thickness of VW* to not more than '/i#. final troweling too soon may result in shrinkage. Water trowel a> final set takes place to provide dense, smooth surface. Gauged lime putty should not be retempered once if has started its initial set on board; il should be discarded and new gauge made up. Apply USG Sealer. Prevent by changing plaster base to a type not subject to inducing such crocking. Potch. Apply to proper thickness. Patch or remove and replace with proper mix. Wet masonry with water to reduce suction or trowel in a scratch coat and double back after a few minutes to fill out to grounds. Use 3 cu.fl. of aggregate per 100 lbs. of gypsum. Discontinue use of job odded retarder and odd accelerator if necessary to obtoin proper job set. Spray walls either with water or alum solution to set basecoat plaster through to base. If bond to base is sound and crocks ore open 'V or more fill by troweling across cracks with properiy aggregated ploster. If fine cracks finish with highly gauged trowel finish or a float finish. If curled at edges and bond unsound remove and re-apply with proper ploster and method. ! j | ; I CRACKS CONDITION 5. Crock at woll or ceiling angles. 6. Wall ond ceiling cracks. long crack at right angles to framing. Cracks at ond poratlel to framing members. Long cracks generally in direction of main runners. Random cracking generoliy 12' to 36* opart. Vertical crack*. Random cracks manoting from GP027 0103 PLASTER PROBLEMS AND REMEDIES MATERIAL Ploster over gypsum lath. Plaster over masonry. Gypsum lath on wood frame con struction. Metal loth on wood frame construction. Suspended metal lath or furred walls. Suspended metal loth or furred metol lath. Masonry blocks Masonry or lath boses aligned with concrete. Ploster over any plaster base. CAUSE Thin plaster. Failure to use cornerite Poilure to wedge tile at ceiling, interlock or tie walls together or use cornerite. Thin plaster. Deflection of joists. Rapid thermal change or extreme thermal differential between face and back of plaster. Thin plaster. Weak plaster. Twisting of framing members. Extreme thermal differential. Weak plaster. Rapid thermal chonge. Shrinkage of units. Differential movement. Stress created at corners of square or rectongular openings. REMEDY OK PREVENTION Cut out ond patch. Correct construction or application details. Prevent by correct construction. Use adequate dimension framing members. Control job temperature in a normal uniform range above 55F. 1 Use a strong plaster mix. Use well dried odequate dimension framing members. Control job temperatures in a normal uniform range above 55F. Control job temperatures In a normal uniform range above 55UF. Use a strong ploster mix. Use cured units. See Page . To minimize prevent bond of plaster to concrete. Realign partition locotion. Patch. Prevent by furnishing adequate support for fixture, ute high itrmngth flatter, grvt __ . * /rrr**. I 1. Woter soluble mildew--like fuzz on tvrfocc, generally while but may be colored. Con be brushed off. 2. Streaky discolora tions. 3. Streaked--joinings show "Slobbers." 4. light and dark spots due to causes other than "dry-out." 5. "Pops"--peak-like projections which foil out making little croters or pits; often with fine radio! crocks .6 Some as (5) above except pit is dlscolored tan or greenish tan. Sasecoot and finish plaster over concrete, brick. cement block or GPQ27 0104 Lime finishes gouged with gauging plaster or with Keenes Cement. Gouged lime putty finish or gypsum trowel finish. Float finish. Lime finish coat. Gypsum base coats and finishes. Efflorescence. As masonry units dry out, water soluble salts from the units or mortar joints leach out and are deposited on the ploster surface. Lime and gauging plaster not thoroughly mixed. Too much wafer used in troweling Efflorescence from masonry. Dirty tools or dirty water. Improper joining technique or excessive troweling at joining. Improper troweling to leave "slobbers" on finish surface. Improper Rooting or too much water used in flooting. Dampening basecoat by throwing water on with brush rother than hose with flne-sproy nozzle. This causes patty correction of suction. Variable suction in basecoat Unslaked lime in mortar which stakes and swells after it is opplied. Contamination by foreign matter. Retorder spots. Lumpy or un dissolved retarder added at job. Retarder lumps swell or "pop" when wet. Contamination by foreign matter such as cinders, etc 1. After plastered surfaces are thoroughly dry, remove efflorescence, then seal with oil base sealer and paint. 2. On interior walls, eliminate source of moisture, then remove efflorescence and decorate. 3. On exterior walls, eliminate source of moisture, furr out, loth ond ploster. Prevent by thorough mixing. Remedy by appli cation of TEXOLITE Primer or TEXOLITE Vinyl Seoier--then point. Remedy same as above. See condition No. 1, above. Wash fools ond use clean water. Remedy by sealing ond painting as above. 1. Previously applied finish should be cut squore for application of bolance of finish. 2. Avoid excessive troweling of joining, 3. Scrape off "slobbers" before decoration. 4. Seal surface when plaster is dry. Point with TEXOLITE paint products to get uniform color. Same os above. ' Dampen basecoat uniformly using hose and fine-spray adjustment to nozzle. Remove core of "pops" and potch. Prevent by proper soaking period with normal hydrated lime or by using double hydrated lime. Cut out spots and patch. Prevented by screening retarder thru 40 mesh screen. Eliminate source. J 1 COLOR. SURFACE STAIN S A N D BLEM CONDITION 7. Blisters {do not confute with (5) above). V. Uneven color (not due to texture shadows). 9. Uneven color-- light, or MAat" spots in light colors {See below). 10. Uneven color -- dark colors. 11. Yellow, brown, or pink surface stains-- "yellowing.*' MATERIAL Gauged lime putty finishes. Gypsum trowel finish Interior colored plaster finishes. Oil paint over gauged lime putty finish. Any colored paint over any piaster finish. Any lime finish over any plaster base, generolly occurs while surface is damp. GP027 0135 PLASTER PROBLEMS AND REMEDIES CAUSE Bose too green, insufficient suction; or too much water used in trowelling. finish lime too plastic Base coot too wet when finish applied. Uneven absorption of base coat, water used in finishing, or dirty box and tools, or varia* tion in woter content of successive batches. Failure to finish single oreas to ongles in one operation. finish not dry. Painted too soon after plostering (alkali in lime soponifles point); or pigment not limeproof Color variation due to non* uniform absorption. Binder strikes in unevenly Contaminated sand. Burning green wood in fire place. Open gos heaters not vented to outside. Tarpaper back of plaster base. Creosote treated framing lumber, tar, or tar derivatives REMEDV OR PREVENTION After finish has "set" trowel with very little water. Do not opply finish over green base coat. Cut putty with small omount fine white sand or increase amount of gauging plaster. After finish begins to "set," trowel with very little water. Prevented by following specifications. Remedied by painting with TEXOUTE paint. Ventilote to dry wall properly Paint with TEXOUTE Primer and TEXOUTE paint. Apply USG Sealer ond repaint. Prevent by using clean sond. Improve draft to stop smoke. Vent heaters to outside. Use asphalt paper. Avoid source of air contamination. $al with USG Sealer. Decorate. 1 I 1. Soft, white, chalky surfaces, occurring during hot, dry weather, usually near opening. 2. Soft, dark, damp surfaces occurring during damp weather. 3. Soft (exactly os 2 above), but occurring in freezing weather. 4. Soft, weak wall. Condition general--not spotty nor due to slow set. S. Weak plaster. 6. Soft, weak wall. 7. Soft, weak wall. 1. Separating from plaster base. 2. Separating from plaster base. 1 3. Separating from plaster base. Gypsum base coat over any plaster base. Gypsum base coat over any plaster base. Gypsum base coat over any plaster base. Gypsum base coat over any piaster base. Gypsum basecoat Gypsum trowel finish over any base coat. Gauged lime putty finish over ony base. Gypsum plaster over gypsum loth. Gypsum plaster over metal loth. Gypsum ploster over masonry. Dry-out. Too much ventilation has removed writer before nlnster 0106could ..1 QPQ27 Sweat-out. \j\j mu* venti lation allowed water to re main in wall after plaster set. Some of plaster has re-dissoved. Frozen plaster. Remedy--Persistent spraying will set-up the dry-out areas. Prevention--Screen openings in hot, dry weother spray during set time if necessary. Remedy--Dry the walls with heot and ventilation. Prevention--Heat and ventilate during plaster ing. If condition exists for too long a period there is no remedy. Remove and replaster. Close building, supply heat. When plaster has set, continue heat and ventilate. Use of too much aggregate, or a One, poorly graded aggregate. Extreme slow set (more than 6 hours). Dry-out or retempered finish. Insufficient gauging with insuf ficient trowelling or retempered. Too much aggregate, freezing, or addition of Nme or Portland cement. Excessive delay in plaster appli cation after mixing or excessive use of retarder resulting in extremely slow set. Too much aggregate. low plaster strength. Freezing. Masonry non-absorbent, has glazed surface. Efflorescence. Insufficient aggregate. No remedy. Prevent by use of aggregate that meets specifications for gradation and pro portions. Spray with alum water to accelerate set. Add accelerator to ploster mix to bring setting time within normal ronge. If dry-out treat as condition (1) obove. Trowel well when set. If retempered, no remedy except tear off and reflnish. No remedy except to remove finish and reploster. No remedy except to replaster. Reploster with correct mix. Thow and allow to set and dry, or replaster. Dampen masonry surfaces No remedy. Prevent by hacking masonry surface. Eliminate source of moisture, reploster. Remedy--Follow directions. .-*****, -------------------------------------------------------- -------------- -- ------------------------------------------ , ------------ , ------_ CONDITION 4. Separating from plotter bate. 5. Brown coot separating from scratch coot. 6. Finish separating from brown coat. 7. Finish separating from brown coat. 1. Finish separating from brown coat. i 1 MATERIAL GP02? 0107 PLASTER PROBLEMS AND REMtDIES CAUSE REMEDY OR PREVENTION 1 Gypsum plaster over concrete. Gypsum bond plaster over concrete. Gypsum bosecoot plasters. Gouged lime putty finish over gypsum brown coat. Gypsum floot and trowel finish over gypsum brown coat. Colored interior finishes over brown coat. Use of ordinary gypsum plaster. Surface oily, too smooth, dirty, or efflorescing. Application of too thick a coat of BONDCRETE Plaster. Weak scrotch coat. Failure to provide mechanical key in scratch coat. Dry-out of scratch coat. Brown coat too smooth, too dry, too wet or loo weak; finish improperly applied; incomplete hydrotion of finish line. Frozen finish coat. Brown coat too smooth. Brown coat too dry. Brown coat too weak. Finish improperly applied. Frozen finish coat. Brown coot not broomed. Thin finish not ground in. Brown coat too weak. Froxen finish coot. Remove and replaster with BONDCRETE, or use plaster bonding medium. Remove plaster. Clean and roughen surface. Replaster. Do not exceed !4# thickness on ceilings and on side walls. Prevent by proper amount of aggregate. Roughen scratch coat and replaster. Remedy--Sproy scratch coat for thorough set before application of brown coot. Where brown coot is cause, strip off finish, correct condition of brown coat ond replaster. Where finish is cause, refinish properly using IVORY double hydrated lime. Remove and re-apply finish. Roughen brown coat. Dampen brown coat until half green. Strip down to lath and replaster. Apply os directed. Remove and re-apply finish. Roughen brown coat and refinish Finish following application directions. Correct condition of base coat and refinish. (See 7 above). Remove and rm-apply finith. \ rit I. Soft walls. GP027 0108 2. Sets in box or sets on wall before it con be darbied or stroighlened. 3- Works hord or "short." Will not spread. Does not carry proper amount of sand. 4. Works hard or "short". Will not spread. S. Tough and short working, rubbery or lumpy lime putty. 6. Lack of* uniformity in set. , 7. finish works hard. Gypsum base coat over any plaster base. Gypsum base coat over any base. Gypsum base coat over any plaster bose. Gypsum bose coat over any plaster base. Gauged lime putty over gypsum base coot. Gauged lime putty over gypsum base coat. Gypsum finishes over base coot. Dry-out, sweat-out, frozen plaster, overloading, sand too fine, or dirty sand. Slow set due to error in manufactureSlow set due to poor sand or poor water. Stow set due lo excessive job use of retarder. Quick set due to dirty water, tools and mixing equipment. Mixing too long. Quick set due to poor sand. Quick set due to error in manufactureQuick set due to machine Aged or badly stored plaster. Over-aggregating. Old material partially carbonoted, warehoused loo long. Improper soaking, oging, or slaking. Low temperatures. Unusual temperatures. Improper gauging. Mined too stiff. Rose too dry. See "Weak, Soft Walls" page Send samples to manufacturers' representative, Obtain good sand ond water or accelerate plaster. Avoid careless job use of retarder, Use dean water, foots, equipment. Reduce mixing time. Use good washed sand or odd retorder. Add retarder. Send samples to manufacturers' representative. Add retarder. Get fresh plaster, use equal parts fresh and aged ploster, or use less sand. Correct conditions by using proper propor tioning. No remedy. Can be used for masons lime. No remedy. Prevented by proper preparation. Do not soak at temperotures below 40F. Properly heat the building in cold weather min. 55P. Use slow set gouging in hot weather. Use proper type ond amount of gauging plaster. Use more water. Apply to half green base. Spray dry base lightly and uniformly before finishing. 1 I GP027 0109 6. ACOUSTICAL PLASTER PROBLEMS Acousticol plasters (SABINITE, USG HI-LITE and RED TOP AUDICOTE) ore special finish coat plasters that require additional job precautions due to the special function which they perform -- that of absorbing sound. By properly following manufacturer's mixing and application directions, an excellent attractive and efficient acovsticol ceiling will result. However, job abuses in mixing and application can destroy the acoustical efficiency as well os the appearance of the job. Indicated below are problems orising from improper use of acoustical plasters, their causes, remedies, and preventive measures. CONDITION SABIN1TE ACOUSTICAL BLASTER CAUSE REMEDY OR PREVENTION USG HI-LITE ACOUSTICAL PLASTER RED TOP AUOICOTE ACOUSTICAL PLASTER CAUSE REMEDY OR PREVENTION CAUSE REMEDY OR PREVENTION Drop-outs and lack of bond. 1. Improper basecoat. 2. Over mixing. 3. Under mixing. 1. Not properly crossraked. lack of suction-- basecoat too green. Base coat too dry--excessive suction--spray lightly. 2. No remedy -- Dump mixed material. 3. Mix to proper mortar weight. Blisters. 1. Basecoat too green. 2. Over mixing. 1. Provide proper heat and ventilation. 2. No remedy -- Dump mixed material. I. Improper bosetoat. 2. Over mixing. 3. Under mixing . 1. Not properly crossraked. lack of suction -- basecoat too wet. Ex cessive suction--spray lightly. 2. No remedy--Dump mixed moterial. 3. Mix to proper mortor weight. 4. Appli cation. 1. Basecoat too green. 2. Over mixing. 4. Failure to scrotch in hard '/#* -- failure to double-up to a full W immediately behind scratching, 1. Provide proper heat and ventilation. 2. No remedy--Dump mixed material. 1. Improper basecoat. I. Not properly cross-raked, lack of of suction--bosecoaf too wet. 2. Mixing 3. Appli cation. 2. Improper woler content. Insufficient mixing. 3. Where applied by hand -- failure to scratch in hard Z%*--failure to double-up to a full H* immediately behind scratching. 1. Basecoat too green. 2. Appli cation. 1. Provide proper heat and ventilation. 2. Where applied by hand -- foilure to scrotch hard Z%m and failure to double-up immediately behind '* ;nr.T*N*.. \ Weak, Soft Ceilings. joinings. Trowel marks. Slick spots in finish surface. loss of sound absorption. 1. Over* mining. 1. No remedy -- scrape down to basecoot and re-apply. 2. Sweat* out. 2. No remedy -- scrape down to basecoot and re-opply with correct heat and ventilation. 1. Improper planning-- plostering to a partially set edge. 1. Provide sufficient scaffolding ond men. Work in a continuous operation. Remedy -- Cover with skim coat of material. 1. Improper 1. Finol trowel in all troweling. directions. 2. Poor lighting. 2. Supply some lighting os for finished job. 1. Final troweling too soon. 1. Cover with thin skim coat--trowel after water sheen has left surface. 1. Over* troweling. 1. No remedy -- trowel lightly on finol troweling. 2. Finol troweling too soon. 2. Cover with skim coot -- re-trowel. 3. Too thin 3. Apply full Vi" application. acoustical plaster. 4. Improper 4. No remedy, pointing. 5. Water floatinq. 5. Apply skim coat-- refloat--use no woter. 3. Application. 1. Overmixing. 3. Failure to scratch hard V%" and failure to double-up immedi ately behind scratching. 1. No remedy--scrape down to basecoot and re-apply. GP027 0110 1. Improper planning-- plastering to a partioily set edge. 1. Provide sufficient scaffolding and men. Work in a continuous operation. Remedy -- Cover with skim coat of material. 1. Too thin 1. Apply full Vi" application. ocoustical plaster. 2. Improper See Painting painting. Directions. 3. Stipple texture too light. 3. Surface allowed to take up loo much prior to stippling. Stipple as specified. 1. Too thin application. 2. Improper painting. 1. Apply full Vi" acousticol plaster. See Painting Directions. \ -* How To Inspect A Plaster lob Approximately 80rf of the visible wall surface in the average building is plaster. It is fundamental that all those involved in the plastering operation cooperate to obtain the best pos sible job. This section attempts to point the way to achieving such an objective--a 'itdlily plaster job. Proper inspection of a lathing and plastering job requires a complete understanding of job details, schedules and specincations. All walls must be judged within the framework, of the drawings and the specifications on which the contract is based. It is most important that these drawings and specifications be complete, accurate and easily interpreted. g -4 g 101 J r i I t SCHEDULE OF INSPECTION Job impoctioni should bo mod* al Iho following stages:-- A. When job is ready tor lathing and plastering. 1. Determine that the brands and types of materials delivered to the job are in accordance with specifica tions and approvals granted. 2. Determine that proper storage facilities are provided tor the mate rials. (See page j6, paragraph J.) B. When lathing has started but be fore plastering has begun. C. When base coat plaster is being applied. D. When finish coat is being applied. E. When job is completed. PLASTER BASES A. A plaster job is only as good as the base over which it is applied. Generally, plaster bases can be clas sified under these headings: 1. Suction Type--Gypsum lath and fiber insulating lath in which the water of the plaster mix carries gypsum into the porous surface, forming tiny keys which hold the plaster to the base. 2. Mechanical Type-Metal lath, in which the lath is embedded in the plaster and, in effect, forms a rein forced plaster slab. 3. Combination Type --Gypsum block, clay tile, other masonry and perforated gypsum lath, in which both suction and mechanical keycombine to hold the plaster to the base. B. The most commonly used bases, along with points that should be checked prior to base coat applica tion are: 1. Cnit Masonry (gypsum block, clay tile, porous brick or rough con" Crete block) a. Has correct mortar been used for laying? (See pages 17-19.) b. Are walls straight and true? c. Are any structural cracks evident? d. Have proper grounds been in stalled? (See page 17.) .2 Gypsum Lath a. Has it been applied according to manufacturer's specifications. (See page 16.) b. Have proper grounds been estab lished, angles and corners reinforced? (See page 16.) 3. Metal Lath a. Have specifications of manufac turer been followed for proper nail ing or tieing? (See pages 26-28.) b. If suspended, furred or contact work, have proper weights of lath and spacing supports been main tained. (See pages 26-27.) c. Have proper grounds been pro vided? 4. Insulation Fiber Board Lath a. Check for correct application. b. Check for proper grounds, angle and corner reinforcement. 5. Monolithic Concrete a. When bond plaster is used, has surface been prepared and material applied according to manufacturer's specifications" fSee page j8.) GP02T OL1Z 102 SUSPENDED GRIllAGE Spacing oi hangers and channels shall be in accordance with spacings recommended for the type of hanger and weight oi metal lath used. Runner or furring channels shall not be let into or be supported by abutting walls. Place runner chan nels within 6" of walls. GROUNDS The thickness of base coat plaster is one of the most important elements of a good plaster job. To insure proper thickness, grounds should be prop erly set and followed. Grounds may be defined as wooden strips, corner beads tplumbed and straight>, metal base screed, or metal casing beads applied at the perimeter of all open ings and other locations. In addition to these, and especially on walls with no openings, and on ceilings, plaster screeds should be installed to insure plumb and level surfaces. Plaster screeds are either dots or continuous strips of plaster applied to required ground thickness to permit proper plumbing and leveling. Grounds should be set to obtain the follow ing minimum plaster thick nesses: 1. Over gypsum lath, and fiber insulating lath................................1 { 2. Over brick, day tile, gypsum block, or other masonry . . j 3" 3. Over metal lath, measured from face of lath........................... ? a" PLASTERING MATERIALS The plastering materials generally in use today are gypsum cement plaster (See page js'), gypsum mill-mixed base coat plasters (See pages jS Sr jp), hydrated finish limes (See page 44), gypsum gauging plaster (See page 45), sand (See page jj 1, vermiculite t See page J4), perlite (See page J4) and water (5te page J5). After determining what materials are specified for use on the job, refer ence to the pages indicated above will describe the nature of each material and point out precautions that should be taken for storing it before it is mixed into plaster. JOB CONDITIONS pages 36-37--This phase of the inspection is most important and. in many cases, will determine the success oi the entire operation. An accurate check of the following points will prove well worthwhile: A. Storage 1. Has material been properly stored on the job for maximum protection from weather and dampness? B. Heating and Ventilation 1. Have proper heating and ventila tion been provided? .If no time should any plastering be performed without proper heating and ventilation. A principal reasor for this is that circulation of air al the right temperature is necessary tc carry off the excess water in the plaster, helping to avoid "sweat out" conditions. GP027 0113 103 7.In enclosed areas uhere adequate normal ventilation through doors and windows is not provided, sup plementary artificial ventilation must be provided. 3. In colder climates during the late fall, winter and early spring, the building should be heated in the nor mal range ot 55 to 70 degrees for some time prior to plastering and maintained at a uniform tempera ture in this range during all plaster ing and after the completion of the plaster work. TWO COAT VERSUS THREE COAT WORK S pagm 36--The architect's spec ifications and the plaster base will determine what plastering method will be used. There are two general ways of applying plaster: 1. Two-coat work. 7. Three-coat work. Except over metal lath, long length gypsum lath, fiber insulation lath, and wood lath, either of these two methods with the plaster properly mixed and applied can be employed. MIXING 5 pag* 35--A mechanical mixer is preierred to box mixing, because it is easier to assure that the plaster aggregate and water are more evenly mixed. Keep the mixer continually clean. which is most important, be cause partially set material is a powerful accelerator. When mixing by hand, plaster and sand first should be mixed dry to a uniform color in a mixing box, and the water added and the plaster hoed into the water immediately and thor oughly mixed to a proper consistency. Remember a number 2 shovel gen erally used to add sand to the mix carries approximately 15 pounds. Therefore, a 1:1 mix would use 6 to 7 number 2 shovels to 100 pounds of gypsum plaster. A 1.2 mix is 12 to 14 shovels, and 1:3 mix is 18 to 21 shovels. When perlite or vermiculite aggre gate is used instead of sand, remem ber the proportioning is weight of gypsum to volume of aggregate. (See page JJ tor proper mixing propor tions.) SCRATCH COAT Section on "Plaster Bases"--(page 9) stated that there are three gen eral types of plaster base: suction type, mechanical type, and a com bination of both. Let's approach the actual application with this in mind and, as a result, know what to look for to help assure a good job. A. Application over Suction Type 1. Is the base properly applied and ready for plaster? <See pages 16.) 7. Is the correct aggregate being used in the proper proportion" (See pages J2-JJ.) 3. Is the building properly heated and/or ventilated, as suggested under Section on "Job Conditions." 4. Is scratch coat being applied to correct thickness and left in proper condition to receive the brown coat? [See page j6 ) 104 GP02T O il* 1 B. Application over Mechanical Type Observance oi the same precautions as indicated above should be checked, and it is recommended that ribered plaster be used, as fiber prevents the passage oi excessive mortar through the keys and holds plaster to lath until set. C. Application over Combination Type The same requirements as apply in (A) above should be followed. BROWN COAT Once the scratch coat has set and is partially dry (usually overnight is sufficient), the brown or second coat is applied. Of course, precaution must be taken by the inspector to assure himself that the plaster is being prepared with the proper ag gregate correctly proportioned. (Sec pastes ye sir jy.) This coat of plaster, together with the scratch coat, forms the backbone of the plastered wall or ceiling, and it is important to see that it is applied to full grounds. All brown coat work ?hould be left rough under the rod or darby to provide "tooth" lor the finish coat. The use oi excessive water in rodding or darb> ing the brown coat, which leaves the surface smooth and slick, is not good practice. SET OF BASE COAT PLASTER The proper setting time fur base coat plasters is generally from 2 to 4 hours after mixing, and this should be checked 'or close conformity on both the scratch coat and the brown coat operation. The danger ot '`quick set" plaster is that there will not be sufficient time to get the plaster from the mixer to the walls without retempering on the mortar board, and such retempering will produce a plaster of lower than normal strength. The correction for "quick set" is to add the proper amount of retarder in solution with water at the mixer. If plaster does not set ior 5 to 6 hours, no harm will be done to the resulting plaster surfaces, but a "slow set" of the plaster (generally one tak ing more than 6 hours) should be avoided by adding accelerator in a dry state at the mixer, as such plas ter may be subject to a "dry out" (See paste 95), particularly in hot, dry weather, and will have a lower than normal strength when finally set. The setting oi base coat plaster is indicated by the hardening of the plaster and by a darkening oi the surface as the set takes place. The portion of the plaster which has set but has not yet thoroughly dried will be darker in color than the unset portion of the plaster This accounts ior the mottled effect in ba=e coat plaster which appears as the set is taking place. FINISH COAT fn addition to gypsum-lime putty trowel finish (See pate 44). the most common types of finishes are Keene's cement lime putty finish (See page 4^ 1. prepared gypsum trowel finish (5a page 44), gypsum-sand float fin- GP027 0115 105 J ish (See p<ige 43), Oriental Interior finish [See page 49). I'SG Acoustical Plasters. (See page j/1. Generally, all finish coats are ap plied to a properly prepared base coat oi gypsum plaster (.See page 43). In the mixing and application of fin ish coats, it is most important that the recommendations of the manu facturer be followed. These recom mendations, along with mixing di rections, are printed on each bag and can also be found in the finish plaster section of this book. (See page 43). The visible success of the job is now at stake, and the required measures should be taken to finish correctly. SUM MAR i m GPOZ7 O il* 106 T UNITED STATES GYPSUM COMPANY DISTRICT SALES OFFICES Further information about item* mentioned in this manual and complete detail* about all other U.S.G. products are available at offices located in the following cities. ALBANY ALBUQUERQUE ATLANTA BALTIMORE BIRMINGHAM BOSTON (Newton Centre, Ma.)* BUFFALO CHARLOTTE CHICAGO CINCINNATI CLEVELAND (Cleveland Heights, Ohio)* DALLAS DENVER DETROIT GRAND RAPIDS `Mailing Addreis HARRISBURG HOUSTON INDIANAPOLIS JACKSONVILLE Kansas city LOS ANGELES LOUISVILLE MILWAUKEE MINNEAPOLIS NEWARK (Clifton, N. J.)* NEW HAVEN (Hamden, Conn.)* NEW YORK OAKLAND OKLAHOMA CITY OMAHA PEORIA PHILADELPHIA PHOENIX PITTSBURGH PORTLAND PROVIDENCE (Warwick, R. I.J* RICHMOND SACRAMENTO ST. LOUIS SALT LAKE CITY SAN ANTONIO SAN DIEGO SEATTLE SAN FRANCISCO SYRACUSE (Oe Witt, N. Y.r WASHINGTON (Arlington, Vq.|* GP0Z7 0117 The Greatest Name In Building GP0Z7 OL18 .. X