Document GzV2d34wOV41BR1vgMNXR7e0Y
GEORGIA-PACIFIC CORPORATION GYPSUM DIVISION TIGARD, OREGON
January 19, 1977
TO:
-Mr-r-M-r-Ar:--Pg-lranugVi - rhir-3-g^Hr~G.~~P. FCU/let - Hariot-t-a -Mr. Ei L. Aauut'i - Portland Ms. R7 L,. uixon - Portland Uir. J . Van -~~Portl-aad -Mr--Ar,--J. Petra line------W44fltngton~ ~Mrs--J-.--B. -Moss-----Wilmington --Mr-;;----fcehaax Tigard Lab
Please find enclosed the following Chicago, Illinois Plant Formula revisions:
C-903 C-923 C-933 C-953 C-970 C-973 C-974 C-976 C-978 C-979
TRIPLE DUTY JOINT COMPOUND BEDDING COMPOUND TOPPING COMPOUND ALL PURPOSE JOINT COMPOUND READY MIX FILLER READY MIX FILLER READY MIX TOPPING COMPOUND (HAND TOOLS) READY MIX JOINT COMPOUND (HAND TOOLS) READY MIX FILLER READY MIX JOINT COMPOUND (HAND TOOLS)
REVISED REVISED REVISED REVISED REVISED REVISED REVISED REVISED REVISED REVISED
Please sign and return the attached tear sheet.
TO: TIGARD GYPSUM TAB
C-903 C-923 C-933 C-953 C-970 C-973 C-974 C-976 C-978 C-979
TRIPLE DUTY JOINT COMPOUND
BEDDING COMPOUND
TOPPING COMPOUND ALL PURPOSE JOINT COMPOUND READY MIX FILLER READY MIX FILLER READY. MIX TOPPING COMPOUND (HAND TOOLS) READY MIX JOINT COMPOUND (HAND TOOLS) READY MIX FILLER READY MIX JOINT COMPOUND (HAND TOOLS)
SIGNED WNG
h\-H,__
PLANT
REVISED REVISED REVISED REVISED REVISED REVISED REVISED REVISED REVISED REVISED
DATE
SGP 0018289
GEORGIA
CIFIC CORPOR AT I INI
ROUND TRIP LETTER
TO
Jiiu-
-\ v - 'i
DATE ________duly 79. 1'T__________________________ > SUBJECT
FROM -
,, r. Vi A, . r_<a,x...'.o'.:s, n.i - ^hx.c..a.go .......................................J*
MESSAGE
; In checking the files we find that we have not yet received the
-t ear- shortr-frcr' yb'tr for^the-'followin'** riant-; Formula-- Revision :
C-972 & C--979 dated 'arch 10, 1975.
If you hare recalved aha above, please sign and return the tvir
sheet or sign and return this note. . Than!-: you.
.. ,f
meo//L^,,
MAT NO. 00306
THIS PAGE MUST BE RETURNED TO SENDER
SGP 0018290
GEORGIA PACIFIC CORPORATION GYPSUM DIVISION TIGARD, OREGON
January 16, 1975
r1p'O:
..Mrr--Mt A. PadmowsM----GMeago Mr. G. F. Fowler - Marietta Mr---E---trr~fta3'en - Pcri-t-PandMsv-R-. ^r~D"ixbrr-=HPertiatU-
Mr-.--AJ. -Pet-rapine - "Wilnrmgten Mr---J-, B-.--Mqrs - Wi 1 mi n.gfcoo-- Mr-v--C t--irJ-r-iehnert^^Tigard Tigari Lab'-:'-'-'; ^
Enclosed please find the following Chicago, Illinois, plant formulas:
C-970 C-971 C-973
READY MIX FILLER READY MIX JOINT COMPOUND (HAND TOOLS) READY MIX-FILLER (FILLER "X")
NEW NEW REVISED
Please cancel the following Chicago, Illinois, plant formulas by removing them from your formula books:
C-977 C-979
READY MIX JOINT COMPOUND (MACHINE TOOLS) READY MIX JOINT COMPOUND (HAND TOOLS)
CANCELLED CANCELLED
Please sign and return the attached tear sheet.
TO: 7IGARD GYPSUM LAB
C-970
C-971 C-978 C-977 C-979
READY MIX FILLER READY MIX JOINT COMPOUND (HAND TOOLS) READY MIX FILLER (FILLER "X") READY MIX JOINT COMPOUND (MACHINE TOOLS) READY MIX JOINT COMPOUND (HAND TOOLS)
NEW NEW REVISED CANCELLED CANCELLED
SIGNED ' / ' V j H *PLANTDATE ! ~ ^ ~? WNG
SGP 0018291
GEORGIA-PACIFIC CORPORATION GYPSUM DIVISION TIGARD, OREGON
TO:
.Mr. M. A.'~Pa-fanow3ki---Xh-icago Tlrr-flt-FT-r owler - Marierta-
. L. Aasen - rorcTan'd -Ms---R. Li &raorr=-XP -Mr---5~. Van - Foreland -Mr. k~.----Pe traline--- Wilmington -Mr-:--3-.--B-r- Moss - Wi,' ning-fe-on Hr. C. W. Lohnort -Tfcar-fl -- Tigard
March 23, 1976
Enclosed please find the following new Chicago, Illinois Plant Formula:
C-973
READY MIX FILLER
NEW
Please cancel the following Chicago, Illinois Plant Formulas by removing them from your formula book:
C-972 C-975 C-979
READY MIX FILLER READY MIX TOPPING COMPOUND (MACHINE TOOLS) READY MIX JOINT COMPOUND (HAND TOOLS)
CANCEL CANCEL CANCEL
Please sign and return the attached tear sheet:
TO: TIGARD GYPSUM LAB
C-973 C-972 C-975 C-979
READY MIX FILLER
NEW
READY MIX FILLER
CANCEL
READY MIX TOPPING COMPOUND (MACHINE TOOLS) CANCEL
| READY MIX JOINT COMPOUND (HAND TOOLS)
CANCEL
s IGNED_ (jjr y{,
PLANT
DATE
WNG
SGP 0018292
GEORGIA PACIFIC CORPORATION GYPSUM DIVISION TIGARD, OREGON
February 16, 1978
TO: Mr. M. A. Palmowski - Chicago Mr r TT 1?m,T^r - Maripft~a
--Mr. Di C. Cork!--!""Portland E-r-L~.~ Aascn------Portland
Mr-i--J. Van - Pui Lland Mu. It: L. DIxoti----Pc-rfelrendMr. (J. W. Lehnert - Tigard Tigard Lab
Enclosed please find the following Chicago, Illinois, Plant Formula revisions
C-970 C-971 C-978 C-979
READY MIX FILLER READY MIX TOPPING COMPOUND (HAND TOOLS) READY MIX FILLER READY MIX JOINT COMPOUND (HAND TOOLS)
REVISED REVISED REVISED REVISED
Please sign and return the attached tear sheet.
TO: TIGARD GYPSUM LAB
C-970 C-971 C-978 C-979
READY MIX FILLER READY MIX TOPPING COMPOUND (HAND TOOLS) READY MIX FILLER READY MIX JOINT COMPOUND (HAND TOOLS)
SIGNED_
HCF 2/16/78
7A*>
PLANT
REVISED REVISED REVISED REVISED
DATE
SGP 0018293
GEORGIA PACIFIC CORPORATION GYPSUM DIVISION TIGARD, OREGON
May 21, 1976
TO:
--A-^--Paluiowski - Chira-go
Mr-. E. L-7 Aaoen----Pe-cfl and-
F. Fuwler - MdiTeLL-a
Mg, R --X.-----jTTvnn - PnrManri
Mr. .T_Va-fr-~"Ptyrtiand^
vMrr--AT J. retralxne-^--WriTirtngeon
--f--M- " " Vi 1 min^rnr
<=.Mr. C. Tigard
W. Lehncn Lab-
ItHISCG
Enclosed please find the following NEW Chicago, Illinois Plant Formulas:
C-979 C-979, Page 2
C-978
READY MIX JOINT COMPOUND (HAND TOOLS) READY MIX JOINT COMPOUND (HAND TOOLS) READY MIX FILLER
NEW NEW NEW
Please sign and return the attached tear sheet:
TO: TIGARD GYPSUM LAB
C-979 C-979, Page 2
C-978
READY MIX JOINT COMPOUND (HAND TOOLS) READY MIX JOINT COMPOUND (HAND TOOLS) READY MIX FILLER
SIGNED WNG
/ KJ A -
PLANT
NEW NEW NEW
DATE
/ ?/?>
SGp 0018294
--
GEORGIA-PACIFIC CORPORATION GYPSUM DIVISION TIGARD, OREGON
March 10, 1975
-Mr." E ;-L-.--Aasen - Portland MsR. L--Dixon - Portland Mr.-Jv-Van-- Portland Mrr~A'."J.- Petraline - Wilmington Mr_J.-B.-Moss - Wilmington MrLehnert - Tigard Tigard
Enclosed please find the following Chicago plant formulas:
C-972 C-979
READY MIX FILLER READY MIX JOINT COMPOUND
NEW NEW
Please sign and return the attached tear sheet.
TO: TIGARD GYPSUM LAB
C-972 C-979
READY MIX FILLER READY MIX JOINT COMPOUND
NEW NEW
SIGNED y ' i| 'i , WNG
PLANT
DATE J5 ~ C. -/ ~7 y'
SGP 0018295
GEORGIA-PACIFIC CORPORATION GYPSUM DIVISION TIGARD, OREGON
August 2, 1977
TO:
-Mr-r-M r-A-r--Pa-lniuwski - Chicago 'Mr~;_E': ET~Aarserr-=--PoTtiand -Mr:--dt--Van "- POiri'3'iid-Mst-^Rtt- L^Dixorr^-^^biTlaTrd --Me-^A;~3:- Pefcralirte---- WiiaiHgtro
Tigard Mi. D .~CT~Cork1rt----Peg-tl-and -Mrr~GT~FT~FowIer - Maiietta Tigard Lab
Enclosed please find the following Chicago, Illinois, Plant Formula Revisions:
C-978 READY MIX FILLER C-979 READY MIX JOINT COMPOUND (HAND TOOLS)
REVISION REVISION
Please sign and return the attached tear sheet.
TO: TIGARD GYPSUM LAB
C-978 C-979
READY MIX FILLER READY MIX JOINT COMPOUND (HAND TOOLS)
SIGNED^
HCF 8/2/77
--/
______ PLANT
REVISION REVISION DATE -S' T7
SGP 0018296
GEORGIA PACIFIC CORPORATION GYPSUM DIVISION TIGARD, OREGON
February 23, 1978
TO:
-Mr i G F Fowler' - Marietta
Ml JCj L Adsdii roiLland
--ettn
van ~ rurtxairo
rib X\ . U JJJLAUU---- furinmg
Mr. U. W. LelnteiL --Tig*rd_
Tigard Lab
Enclosed please find the following Chicago, Illinois,'Plant Formula revisions:
C-970 C-971 C-977 C-978 C-979 /
READY MIX FILLER
READY MIX TOPPING COMPOUND (HAND TOOLS)
READY MIX JOINT COMPOUND (HAND TOOLS)
READY MIX FILLER
PJT.
READY MIX JOINT COMPOUND (HAND TOOLS)
REVISED REVISED NEW REVISED REVISED
Please sign and return the attached tear sheet.
TO TIGARD GYPSUM LAB
C-970 C-971 C-977 C-978 C-979
READY MIX FILLER READY MIX TOPPINGCOMPOUND (HAND TOOLS) READY MIX JOINT COMPOUND(HAND TOOLS) READY MIX FILLER READY MIX JOINT COMPOUND (HAND TOOLS
SIGNED
HGF 2/23/78
PLANT
REVISED REVISED NEW REVISED REVISED
DATE
SGP 0018297
February 15, 1978 Supersedes Formula C-979 Dated: 8/2/77
CHICAGO, ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-979 (HAND TOOLS)
DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, topping and texturing.
FORMULA Raw Material / Proxcel-CRL
/ Filler C 978 Elvace E.-200 Nalco 71^-5 Acrysol SE-60
*Water
Function
RM Spec '
Preservative
Filler
--
Adhesive
185
Defoamer
125
Thickener
147
Solvent
--
Percent
.05 93.15
6.5 .1 .2 --
100.0
Lbs/Batch
1.0 1950.0
136.0 (15.25 gals 2.0 4.0
1104.0 (133 gals.) 3197-0**
*Approximately 56.5 lbs/100 lbs. of active ingredients (this may vary + 8 gallons per batch.
,,
** One batch yields f + 1 five gallon pail Ready Mix joint compound at 62 lbs/pail.
SPECIAL MIXING INSTRUCTIONS
Blend ingredients in following order:
1) Water 2) Elvace EP-200 3) Nalco 4) Filler C-978 5) Mix until filler is dispersed 6) Add Acrysol ASE-60 7) Mix until Ready Mix is smooth - pumping viscosity should
be 480 + 20 to allow for 24 hour viscosity build of 100 pts.
WORKING CONSISTENCY Specifications for Paste
- Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5 cc water per 150 grams of paste may be added to adjust.
Brabender: (580 + 20) For Machine tools add 7 gallons ^0 (400 + 20)
PH
Minimum - 9.0
Maximum - 9.5
WORKING PROPERTIES
Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working and free of any coarse, gritty or undispersed particles. Material shall be free from lumps due to incomplete mixing.
HCF:j r
Continued on Page 2...
SGP 018298
GEORGIA PACIFIC CORPORATION GYPSUM DIVISION TIGARD, OREGON
May 2, 1978
TO:
Mr. M. A. Paimowski - Chicago -Mr. E. L. Mr. Ji Vtm----- Portland
--MrT G. r. towler-- Marietta -Mrr-D. C. Curkill - Port-land
Tigard Lab
Enclosed please find the following Chicago, and revision:
C-970
READY MIX FILLER
C-971
READY MIX TOPPING COMPOUND
C-977
READY MIX JOINT COMPOUND
C-978
READY MIX FILLER
C-979 /
READY MIX JOINT COMPOUND
C-973'
READY MIX FILLER
Illinois,
Plant Formula cancellations
CANCELLED CANCELLED CANCELLED CANCELLED CANCELLED REVISED
Please sign and return the attached tear sheet.
TO: TIGARD GYPSUM LAB
C-970 C-971 C-977 C-978 C-979 C-973
SIGNED HCF 5/2/78
READY MIX FILLER READY MIX TOPPING COMPOUND READY MIX JOINT COMPOUND READY MIX FILLER READY MIX JOINT COMPOUND READY MIX FILLER
PLANT
CANCELLED CANCELLED CANCELLED CANCELLED CANCELLED REVISED
DATE if-3
SGP 0018299
March 30, 1978 Supersedes Formula C-979 Dated: 2/22/78
CHICAGO, ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-979 (HAND TOOLS)
DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, topping and texturing.
FORMULA Raw Material _/Proxcel-CRL
-/Filler C-978 -/Elvace EP-200 -/Nalco 71D-5 -/Acrysol ASE-60 /*Water
Function Preservative Filler Adhesive Defoamer Thickener Solvent
RM Spec
--
185 125 147
--
Percent
.048 93.885
5.778 .096 .193
__
100.0
Lbs/Batch
1.0 1950.0
120-0 (13.48 gals.) 2.0 4.0
1120-0 (134.9 gals.) 3197-0**
*Approximately 56.5 lbs/100 lbs. of ac tive ingredients (this may vary + 8 gallons per batch.
** One batch yields 50+1 five gallon pail Ready Mix joint compound at 62 lbs/pail.
SPECIAL MIXING INSTRUCTIONS
--
- Blend ingredients in following order:
1) Water 2) Elvace EP-200 3) Nalco 4) Filler C-978 5) Mix until filler is dispersed 6) Add Acrysol ASE-60 7) Mix until Ready Mix is smooth - pumping viscosity should
be 480 + 20 to allow for 24 hour viscosity build of 100 pts
WORKING CONSISTENCY Specifications for Pas te
- Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5 cc water per 150 grams of paste may be added to adjust.
Brabender: (580 + 20) For Machine tools add 7 gallons H2O (400 + 20)
pH
Minimum - 9.0
Maximum - 9.5
WORKING PROPERTIES
- Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working and free of any coarse, gritty or undispersed particles. Material shall be free from lumps due to incomplete mixing.
HCF:jr
Continued on Page 2...
SGP 0018300
May 21, 1976 Formula C-979 Page 2 NEW
BONDING PROPERTIES Specifications
CRACK RESISTANCE Specifications
COLOR Specifications
- Refer to Plant Testing Procedure No. 35. After compound has dried, tape shall show at least 90% fiber tear when delaminated.
- Refer to Plant Testing Procedure No. 37. Rating shall be 4 or better.
- White Dried compound shall match color of standard sample.
WNG/gvp
SGP 0018301
1
GEORGIA PACIFIC CORPORATION GYPSUM DIVISION TIGARD, OREGON
March 31 , 1978
TO:
Mr. M. A. Palmowski - Chicago Mr~r~U."T. Fuwlci - Marietta --Mi - n -r. . r.mfeill - Pm-t-1 Mr E.--L. Aaseu PuiLland Mr.-J. Van-- Portland-- ^ls. R'." 8. Dixon------Portland Mr. C. W. Lehnert - Tigard Tigard Lab
Enclosed please find the following Chicago, Illinois, Plant Formula revisions:
C-971 C-979
READY MIX TOPPING COMPOUND (HAND TOOLS) READY MIX JOINT COMPOUND (HAND TOOLS)
REVISED REVISED /
Please sign and return the attached tear sheet.
TO: TIGARD GYPSUM LAB
C-971 C-979
READY MIX TOPPING COMPOUND (HAND TOOLS) READY MIX JOINT COMPOUND (HAND TOOLS)
SIGNED
HCF 3/31/78
PLANT
REVISED REVISED
_________ DATE
SGP 0018302
February 22, 1978 Supersedes Formula 0979 Dated: 2/15/78
CHICAGO, ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-979 (HAND TOOLS)
DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, topping and texturing..
FORMULA Raw Material Proxcel-CRL
Filler C-978 Elvace EP-200 Nalco 71D-5 Acrysol ASE-60 *Water
Function ^ RM Spec
Preservative
Filler
Adhesive
185
Defoamer
125
Thickener
147
Solvent
Percent
Lbs/Batch
93.15'-^
1.0 1950.0 /3.ui
-776 /zx> L-36-. 0 (i5r25 gals .)
JZ 2.0
JZ-til
4.0
//7uo HG4.0 (443 gals.)
100.0
3197.0**
*Approximately 56.5 lbs/100 lbs.-of active ingredients (this may vary + 8 gallons per batch.
** One batch yields 50+1 five gallon pail Ready Mix joint compound at 62 Ibs/pail.
SPECIAL MIXING INSTRUCTIONS
Blend ingredients in following order:
1) Water 2) Elvace EP-200 3) Nalco 4) Filler C-978 5) Mix until filler is dispersed 6) Add Acrysol ASE-60 7) Mix until Ready Mix is smooth - pumping viscosity should
be 480 + 20 to allow for 24 hour viscosity build of 100 pts
WORKING CONSISTENCY Specifications for Paste
Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5 cc water per 150 grams of paste may be added to adjust.
Brabender: (580 + 20) For Machine tools add 7 gallons ^0 (400 + 20)
pH
Minimum - 9.0
Maximum - 9.5
WORKING PROPERTIES
- Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working and free of any coarse, gritty or undispersed particles. Material shall be free from lumps due to incomplete mixing.
HCF:jr
Continued on Page 2...
SGP 0018303
February 15, 1978 Supersedes Formula C-979 Dated: 8/2/77
CHICAGO, ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-979 (HAND TOOLS)
DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, topping and texturing.
FORMULA Raw Material Proxcel-CRL
' Filler C-978 Elvace EP-200 Nalco 71D-5 Acrysol ASE-60
*Water
Function
RM Spec
Preservative
Filler
--
Adhesive
185
Defoamer
125
Thickener
147
Solvent
--
Percent
.05 93.15
6.5 .1 .2 --
100.0
Lbs/Batch
1.0 1950.0
136.0 (15.25 gals 2.0 4.0
1104.0 (133 gals.) 3197.0**
^Approximately 56.5 lbs/100 lbs. of active ingredients (this may vary + 8 gallons per batch.
` ** One batch yields 51+1 five gallon pail Ready Mix joint compound at 62 lbs/pail.
SPECIAL MIXING INSTRUCTIONS
Blend ingredients in following order: 1) Water 2) Elvace EP-200 3) Nalco 4) Filler C-978 5) Mix until filler is dispersed 6) Add Acrysol ASE-60 7) Mix until Ready Mix is smooth - pumping viscosity should
be 480 + 20 to allow for 24 hour viscosity build of 100 pts.
WORKING CONSISTENCY Specifications for Paste
Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5 cc water per 150 grams of paste may be added to adjust.
Brabender: (580 + 20) For Machine tools add 7 gallons ^0 (400 + 20)
pH
Minimum - 9.0
Maximum - 9.5
WORKING PROPERTIES
- Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working and free of any coarse, gritty or undispersed particles. Material shall be free from lumps due to incomplete mixing.
HCF:jr
Continued on Page 2...
SGP 0018304
February 22, 1978 Supersedes Formula C-979 Dated: 2/15/78
CHICAGO, ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-979 (HAND TOOLS)
DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, topping and texturing.
FORMULA Raw Material Proxcel-CRL
Filler C-978 Elvace EP-200 Nalco 71D-5 Acrysol ASE-60 *Water
Function
RM Spec
Preservative
Filler
--
Adhesive
185
Defoamer
125
Thickener
147
Solvent
--
Percent
.05 93.15
6.5 .1 .2 --
100.0
Lbs/Batch
1.0 1950.0
136.0 (15.25 gals 2.0 4.0
1104.0 (133 gals.) 3197-0**
*Approximately 56.5 lbs/100 lbs. of active ingredients (this may vary + 8 gallons per batch.
** One batch yields 50+1 five gallon pail Ready Mix joint compound at 62 lbs/pail.
SPECIAL MIXING INSTRUCTIONS
Blend ingredients in following order: 1) Water 2) Elvace EP-200 3) Nalco 4) Filler C-978 5) Mix until filler is dispersed 6) Add Acrysol ASE-60 7) Mix until Ready Mix is smooth - pumping viscosity should
be 480 + 20 to allow for 24 hour viscosity build of 100 pts
WORKING CONSISTENCY Specifications for Paste
Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5 cc water per 150 grams of paste may be added to adjust.
Brabender: (580 + 20) For Machine tools add 7 gallons ^0 (400 + 20)
pH
Minimum - 9.0
Maximum - 9.5
WORKING PROPERTIES
- Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working and free of any coarse, gritty or undispersed particles. Material shall be free from lumps due to incomplete mixing.
HCF:j r
Continued on Page 2.
SGP 0018305
March 30, 1978 Supersedes Formula C-979 Dated: 2/22/78
CHICAGO, ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-979 (HAND TOOLS)
DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, topping and texturing.
FORMULA Raw Material _/Proxce1-CRL
-/Filler C 978 -/Elvace Ef-200 -/Nalco 71"-5 -/Acrysol c 3E-60 /*Water
Function
RM Spec
Preservative
Filler
Adhesive
185
Defoamer
125
Thickener
147
Solvent
--
Percent .048
93.885 5.778 .096 .193
--
100.0
Lbs/Batch
1.0 1950.0
120-0 (13.48 gals.) 2.0 4.0
1120-0 (134.9 gals.) 3197-0**
*Approximately 56.5 lbs/100 lbs. of active ingredients (this may vary + 8 gallons per batch.
** One batch yields 50+1 five gallon pail Ready Mix joint compound at 62 lbs/pail.
SPECIAL MIXING INSTRUCTIONS
Blend ingredients in following order: 1) Water 2) Elvace EP-200 3) Nalco 4) Filler C-978 5) Mix until filler is dispersed 6) Add Acrysol ASE-60 7) Mix until Ready Mix is smooth - pumping viscosity should
be 480 + 20 to allow for 24 hour viscosity build of 100 pts.
WORKING CONSISTENCY Specifications for Paste
Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5 cc water per 150 grams of paste may be added to adjust.
Brabender: (580 + 20) For Machine tools add 7 gallons H2O (400 + 20)
pH
Minimum - 9.0
Maximum - 9.5
WORKING PROPERTIES
- Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working and free of any coarse, gritty or undispersed particles. Material shall be free from lumps due to incomplete mixing.
HCF:jr
Continued on Page 2...
SGP 0018306
October 21, 1970 NEW FORMULA
-'n-c -o----- v n? ~'~C'
CHICAGO, ILLINOIS PLANT FORMULA JOINT COMPOUND C- -v7 9fHANDTCO
r.:.;:e Meacy Mix juir.; topping and texturing recuesc only.)
U wt>C US cC --. *. 0. -y _ . (Supplied on special
unction
yercant
Water
Solvent
A 3 1C O
Polyvinyl Acetate Emulsion Adhesive
Eer.no flex
Plasticizer
Filler C -97S
Filler
0.1 7.0 0.4 92.5 100.0
i-O'J'J.U- ., ** ^ U-T \J
- ^ . s*\J
GuO U \j u4
'"Aoproxir.ately 54.4 lbs/ICO lbs. of active ingredients (this may vary-- 3 gallons per batch.
**0r.a batch yields 95 1 five gallon pail Ready Mix joint compound at 62 Ibs/peii.
:oeciricr.rior.s tor raste:
JdRT_db wlOtS1
oO'.\_ 1'3 r..0rZ?.T>d5 5ns:
ooact-icatrons.
-1 /~
soscincaeions:
Reter to 31
nesting "rocecure no.
1Z OSS03 s not proper ;oricm_2 cor.sit
rr.axrxum or 5 cc. watar par 100 grsr.s
nay be added to adjust.
to Plant _ as t r' .nd shall be pi f any coa rse,
Material sr.ai onpiete r;ixir.g
Prccecur : .\c. w. _/ O cue
to Plant i.cStl` c or.pounc has d 75% fiber tear
rrocacure no. 1, taps sr.a*_ snov: a . ^ ^4 O C w* . to c
to Plant Testi: 1 n 3 r 3 shall be r.o la: ge erasure croc wedge, and no cracks in the thinner the wedge.
:.te
Unite Dried compound shall match :o.or s amo1e.
-/ Denotes change in this reissue. I C 3rl
SGP 0018307
Supersedes Formula lured- 10/21/7C
^ . -r___. / _ u U
/
V
srf W -w
^ V ^ C li ^
?c.c. r ~
SGP 0018308
February 16, 1973 Supersedes Formula C-979 Dated 2/24/71
CHICAGO ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-979 (HAND TOOLS)
DESCRIPTION OF PRODUCT
- White Ready Mix Joint Compound used for taping,
topping and texturing?--
__ ____
FORMULA
Raw Material
Water Nalco Polyvinyl Acetate Emulsion
(preplasticized) Filler C-978
Function
Percent Lbs./Batch
Solvent
- 1200.00* (145
Anti-foaming agent
0.1
2.00
Adhesive Filler
7.4 92.5 100.0
148.00 2050.00 3400.00**
s)
-'Approximately 54.4 lbs/100 lbs. of active ingredients (this may vary + 8 gallons per batch.
**One batch yields 53+1 five gallon pail Ready Mix joint compound at 62 lbs/pail.
WORKING CONSISTENCY
- Refer to Plant Testing Procedure No. 32.
Specifications for Paste: If paste is not proper working consistency, a
maximum of 5 cc water per 150 grams of paste
may be added to adjust.
Brabender: 530 + 20
WORKING PROPERTIES Specifications:
Refer to Plant Testing Procedure No. 33 Compound shall be plastic, buttery working, and free of any coarse, gritty, or undispersed parti cles. Material shall be free from lumps due to incomplete mixing.
BONDING PROPERTIES Specifications:
Refer to Plant Testing Procedure No. 35. After compound has dried, tape shall show at least 757o fiber tear when delaminated.
CRACK RESISTANCE Specifications
Refer to Plant Testing Procedure No. 37. There shall be no large fissure cracks in the wedge, and no cracks in the thinner half of the wedge.
COLOR Specifications
White Dried compound shall match color of standard sample.
ij denotes change
EDO;elz
SGP 0018309
April 26, 1973 Supersedes Formula C-979 Dated 2/16/73
CHICAGO ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-979 (HAND TOOLS)
DESCRIPTION OF PRODUCT
- White Ready Mix Joint Compound used for taping, topping and texturing.
FORMULA
Raw Material
Water Nalco Polyvinyl Acetate Emulsion
(preplasticized) Filler C-978
Function
Percent Lbs. /Batch
Solvent
- 1200.00* (145 gals)
Anti-foaming agent
0.1
2.00
Adhesive Filler
7.4 92.5 100.0
156.00 (17.3 gals. 1950.00 3308.00**
Approximately 54.4 lbs/100 lbs. of active ingredients (this may vary + 8 gallons per batch.
**One batch yields 53+1 five gallon pail Ready Mix joint compound at 62 lbs/pail.
WORKING CONSISTENCY
- Refer to Plant Testing Procedure No. 32.
Specifications for Paste: If paste is not proper working consistency, a
maximum of 5 cc water per 150 grams of paste
may be added to adjust.
Brabender: 530 + 20
WORKING PROPERTIES Specifications:
- Refer to Plant Testing Procedure No. 33 Compound shall be plastic, buttery working, and free of any coarse, gritty, or undispersed parti cles. Material shall be free from lumps due to incomplete mixing.
BONDING PROPERTIES Specifications:
- Refer to Plant Testing Procedure No. 35. After compound has dried, tape shall show at least 7570 fiber tear when delaminated.
CRACK RESISTANCE Specifications:
Refer to Plant Testing Procedure No. 37. There shall be no large fissure cracks in the wedge, and no cracks in the thinner half of the wedge.
COLOR Specifications:
- White Dried compound shall match color of standard sample.
-/ denotes change
WNG:elz
SGP 0018310
January 15, 1974 Supersedes Formula C-979
Dated 4/26/73
CHICAGO ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-979 (HAND TOOLS)
DESCRIPTION OF PRODUCT
- White Ready Mix Joint Compound used for taping, topping and texturing.
FORMULA
Raw Material
Function
Percent Lbs./Batch
Water Nalco Polyvinyl Acetate Emulsion
(preplasticized) Filler C-978
Solvent Anti-foaming agent
0.1
Adhesive Filler
7.4 92.5 100.0
1200.00* (145 gals) 2.00
156.00 (17.3 gals.) 1950..00 3308.00**
'Approximately 54.4 lbs/100 lbs. of active ingredients (this may vary + 8 gallons per batch.
**One batch yields 53+1 five gallon pail Ready Mix joint compound at 62 lbs/pail.
WORKING CONSISTENCY
- Refer to Plant Testing Procedure No. 32.
Specifications for Paste: If paste is not proper working consistency, a
maximum of 5 cc water per 150 grams of paste
may be added to adjust.
Brabender: 580 + 20
WORKING PROPERTIES Specifications:
Refer to Plant Testing Procedure No. 33 Compound shall be plastic, buttery working, and free of any coarse, gritty, or undispersed parti cles. Material shall be free from lumps due to incomplete mixing.
BONDING PROPERTIES Specifications:
Refer to Plant Testing Procedure No. 35. After compound has dried, tape shall show at least 757, fiber tear when delaminated.
CRACK RESISTANCE SDecifications:
Refer to Plant Testing Procedure No. 37. There shall be no large fissure cracks in the wedge, and no cracks in the thinner half of the wedge.
COLOR Specifications:
White Dried compound shall match color of standard sample.
-/ denotes change
WNG:elz
SGP 0018311
March 6, 1974
Supersedes Formula C-979 Dated 1/15/74
CHICAGO ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-979 (HAND, TOOLS)
DESCRIPTION OF PRODUCT
- White Ready Mix Joint Compound used for taping, topping and texturing.
FORMULA
Raw Material
Water Nalco Polyvinyl Acetate Emulsion
(preplasticized) Filler C-978
Function
Percent Lbs./Batch
Solvent Anti-foaming agent
0.1
1024.00* (128 gals) 2.00
Adhesive Filler
7.0 92.9
100.0
147*00 (16.3 gals.)
1950..00 3T737UD +*
*Approximately 54.4 lbs/100 lbs. of active ingredients (this may vary + 8 gallons per batch.
**One batch yields 53+1 five gallon pail Ready Mix joint compound at 62 lbs/pail.
WORKING CONSISTENCY
- Refer to Plant Testing Procedure No. 32.
Specifications for Paste: If paste is not proper working consistency, a
maximum of 5 cc water per 150 grams of paste
may be added to adjust.
Brabender: 580 + 20
WORKING PROPERTIES Specifications:
-
- Refer to Plant Testing Procedure No. 33 Compound shall be plastic, buttery working, and free of any coarse, gritty, or undispersed particles. Material shall be free from lumps due to incomplete mixing.
-/ BONDING PROPERTIES Specifications:
Refer to Plant Testing Procedure No. 35. After compound has dried, tape shall show at least 907o fiber tear when delaminated.
CRACK RESISTANCE Specifications
Refer to Plant Testing Procedure No. 37. There shall be no large fissure cracks in the wedge, and no cracks in the thinner half of the wedge.
COLOR Specifications
Whi.te Dried compound shall match color of standard sample.
-/ denotes change
WNGrelz
SGP 0018312
March 7, 1975 Formula 0979 NEW
CHICAGO, ILLINOIS, PLANT FORMULA READY MIX JOINT COMPOUND C-979 (HAND TOOLS)
DESCRIPTION OF PRODUCT - White Ready Mix Taping Compound used for bedding tape. Special formula. For trial shipments only.
FORMULA
Water Nalco Llvace 1875 Filler C-972
Function
Solvent Anti-foaming agent Adhesive Filler
Percent
_ 2
20 97 8
Lbs/Batch
1024.00 4.00
39.00 1950.00
(128 (4.4
gals.)* gals.)
100 0
3017.00**
^Approximately 56.5 lbs/100 lbs of active ingredients (this may vary + 8 gallons per batch).
**One batch yields 50+1 five-gallon pail Ready Mix joint compound at 62 lbs/pail.
WORKING CONSISTENCY Specifications for Paste
- Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5 cc water per 150 grams of paste may be added to adjust.
Brabender: (540 + 20) For machine tools add 10 gallons water (400 + 20)
WORKING PROPERTIES Specifications
Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working, and free of any coarse, grity or undispersed particles. Material shall be free from lumps due to incomplete mixing.
BONDING PROPERTIES Specifications
Refer to Plant Testing Procedure No. 35. After compound has dried, tape shall show at least 1007o fiber tear when delaminated.
CRACK RESISTANCE Specifications
Refer to Plant Testing Procedure No. 37. Ratings shall be 4 or better.
COLOR WNG:elz
- White Dried compound shall match color of standard sample.
SGP 0018313
March 7, 1975... Formula C-979 NEW
CHICAGO, ILLINOIS, PLANT FORMULA READY MIX JOINT COMPOUND C-979 (HAND TOOLS)
DESCRIPTION OF PRODUCT - White Ready Mix Taping Compound used for bedding tape. Special formula. For trial shipments only.
FORMULA
Function
Percent Lbs/Batch
Water Nalco .lvace 1875 filler C-972
Solvent Anti-foaming agent Adhesive Filler
r.2 2.0 97.8
1024 .00 (128 gals.)*
4 .00
39 .00 (4.4 gals.)
1950 .00-
100.0
3017.00**
*Approximately 56.5 lbs/100 lbs of active ingredients (this may vary + 8 gallons per batch).
**0ne batch yields 50+1 five-gallon pail Ready Mix joint compound at 62 lbs/pail.
WORKING CONSISTENCY Specifications for Paste
- Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5 cc water per 150 grams of paste may be added to adjust.
Brabender: (540 + 20) For machine tools add 10 gallons water (400 + 20)
WORKING PROPERTIES Specifications
Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working, and free of any coarse, gritty or undispersed particles. Material shall be free from lumps due to incomplete mixing.
BONDING PROPERTIES Specifications
Refer to Plant Testing Procedure No. 35. After compound has dried, tape shall show at least 100% fiber tear when delaminated.
CRACK RESISTANCE Specifications
Refer to Plant Testing Procedure No. 37. Ratings shall be 4 or better.
COLOR WNG:elz
- White Dried compound shall match color of standard sample.
Hummrrr
SGP 0018314
May 21, 1976 Formula C-979 NEW
CHICAGO, ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-979 (HAND TOOLS)
DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, topping and texturing. (Special asbestos free formula for all one gallon ready mix and selective five gallon shipment only.)
FORMULA Raw Material
Function 'RM Spec
Percent Lbs/Ba tch
Filler C-978 Elvace 1875 Nalco 71D-5 Acrysol ASE-60 *Water
Filler Adhesive Defoamer Thickener Solvent
--
185 125 147
92.8 6.5 .2 .5
100.0
195C.0 136 0 40 10.0
1120.0
(15. (135
3220.0**
''Approximately 56.5 lbs/100 lbs. of active ingredients (this may vary + 8 gallons per batch.
** One batch yields 51+1 five gallon pail Ready Mix joint compound at 62 lbs/pail.
SPECIAL MIXING INSTRUCTIONS
Blend ingredients in following order: 1) Water 2) Elvace 1875 3) Nalco 4) Filler C-978 5) Mix until filler i, dispersed 6) Add Acrysol ASE-60 7) Mix until Ready Mix is smooth - pumping viscosity should
be 480 + 20 to allow for 24 hour viscosity build of 100 pts.
WORKING CONSISTENCY Specifications for Paste
Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5 cc water per 150 grams of paste may be added to adjust.
Brabender: (580 + 20) For Machine tools add 7 gallons H2O (400 + 20)
pH
Minimum - 9.0
Maximum - 10.0 (24 nrs.)
WORKING PROPERTIES
- Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working and free of any coarse, gritty or undispersed particles. Material shall be free from lumps due to incomplete mixing.
WNG:gvp
Continued on Page 2...
SGP 0018315
May 21, 1976 Formula C-979 Page 2 NEW
BONDING PROPERTIES Specifications
CRACK RESISTANCE Specifications
COLOR Specifications
- Refer to Plant Testing Procedure No. 35. After compound has dried, tape shall show at least 90% fiber tear when delaminated.
- Refer to Plant Testing Procedure No. 37. Rating shall be 4 or better.
- White Dried compound shall match color of standard simple.
WNG/gvp
SGP 0018316
7 a_>. n. a r7 21',-1976--
i Formula C-979
P1-V7/7
CHICAGO, ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-979 (HAND TOOLS)
DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, topping and texturing. (Special asbestos free formula for all one gallon ready mix and selective five gallon shipment only.)
FORMULA Raw Material
Function
RM Spec
Percent Lbs/Batch
Filler C-978 Elvace '1875- Cf. zoo Nalco 71D-5 Acrysol ASE-60 Water
Filler Adhesive Defoamer Thickener Solvent
--
185 125 147
92.8 6.5 .2 .5 --
1950.0
136.0 (15.25 gals.) 4.0
10.0 I3Z MOV i-1-2O-rO (135-gals.)
100.0
3220r0**
Z2 ></
Approximately 56.5 lbs/100 lbs. of active ingredients (this may vary + 8 gallons
per batch.
* ** One batch yields 51+1 five gallon pail Ready Mix joint compound at 62 lbs/pail.
SPECIAL MIXING INSTRUCTIONS
Blend ingredients in following order: 1) Water 2) ElvaceTSW-t?^ too 3) Nalco 4) Filler C-978 5) Mix until filler is dispersed 6) Add Acrysol ASE-60 7) Mix until Ready Mix is smooth - pumping viscosity should
be 480 + 20 to allow for 24 hour viscosity build of 100 pts.
WORKING CONSISTENCY Specifications for Paste
Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5 cc water per 150 grams of paste may be added to adjust.
Brabender: (580 + 20) For Machine tools add 7 gallons H2O (400 + 20)
pH
Minimum - 9.0
Maximum - 10.0 (24 hrs.)
WORKING PROPERTIES
- Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working and free of any coarse, gritty or undispersed particles. Material shall be free from lumps due to incomplete mixing.
WNG:gvp
Continued on Page 2...
SGP 0018317
January 17, 1977 Supersedes Formula C-979 Dated: 5/21/76
CHICAGO, ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-979 (HAND TOOLS)
DESCRIPTION OF PRODUCT r White Ready Mix Joint Compound used for taping, topping' and texturing. (Special asbestos free formula for all one gallon ready mix and selective five gallon shipment only.)
FORMULA Raw Material
Function ' RM Spec
Percent Lbs/Batch
Filler C-978 Elvace EP-200
Nalco 71D-5 Acrysol ASE-60 -/*Water
Filler Adhesive Defoamer Thickener Solvent
--
185 125 147
1950.0 6.5 136.0 (15.
4~0 -t.
4' 0 1104 .0 (133
100.0
"'Approximately 56.5 lbs/100 lbs. of active ingredients (this may vary + 8 gallons per batch.
** One batch yields 51+1 five gallon pail Ready Mix joint compound at 62 lbs/pail.
SPECIAL MIXING INSTRUCTIONS
Blend ingredients in following order: 1) Water 2) Elvace EP-200 3) Nalco 4) Filler C-978 5) Mix until filler is dispersed 6) Add Acrysol ASE-60 7) Mix until Ready Mix is smooth - pumping viscosity should
be 480 + 20 to allow for 24 hour viscosity build of 100 pts.
WORKING CONSISTENCY Specifications for Paste
- Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5 cc water per 150 grams of paste may be added to adjust.
Brabender pH
(580 + 20) For Machine tools add 7 gallons H2O (400 + 20)
_ ?*iT
Minimum - 9.0
Marrrtrcnaf 1-1ID.
^.)
WORKING PROPERTIES
- Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working and free of any coarse, gritty or undispersed particles. Material shall be free from lumps due to incomplete mixing.
WNG:gvp
Continued on Page 2...
auk'll
SGP 0018318
January 17, 1977 Supersedes Formula C-979: Dated: 5/21/76
CHICAGO, ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-979 (HAND TOOLS)
DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, topping and texturing. (Special asbestos free formula for all one gallon ready mix and selective five gallon shipment only.)
FORMULA Raw Material
Filler C-978 Elvace EP-200 Nalco 71D-5 Acrysol ASE-60 Water
Function
RM Spec
Filler Adhesive Defoamer Thickener Solvent
--
185 125 147
Percent
92.8 6.5 .2 .5 --
100.0
Lbs/Batch
1950.0 136.0 4.0 10.0
1104 .0
(15.25 gals.) (133 gals.)
32 04,0**
'"Approximately 56.5 lbs/100 lbs. of active ingredients (this may vary jr 8 gallons per batch.
** One batch yields 51+1 five gallon pail Ready Mix joint compound at 62 Ibs/pail.
SPECIAL MIXING INSTRUCTIONS
- Blend ingredients in following order:
1) Water 2) Elvace EP-200 3) Nalco 4) Filler C-978 5) Mix until filler is dispersed 6) Add Acrysol ASE-60 7) Mix until Ready Mix is smooth - pumping viscosity should
be 480 + 20 to allow for 24 hour viscosity build of 100 pts
WORKING CONSISTENCY Specifications for Paste
- Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5 cc water per 150 grams of paste may be added to adjust.
Brabender: (580 + 20) For Machine tools add 7 gallons H2O (400 + 20)
pH
Minimum - 9.0
Maximum - 10.0 (24 hrs.)
WORKING PROPERTIES
- Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working and free of any coarse, gritty or undispersed particles. Material shall be free from lumps due to incomplete mixing.
WNG:gvp
Continued on Page 2.._.
SGP 0018319
August 1, L'Jj'l Supersedes Formula C-979 Dated: 1/17/77
CHICAGO, ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-979 (HAND TOOLS)
DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, topping and texturing.
FORMULA Raw Material
/ Filler C-978 Elvace EP-200
/ Nalco 71D-5 / Acrysol ASE-60
*Water
Function
Filler Adhesive Defoamer Thickener Solvent
RM Spec
-_ 185 125 147
--
Percent
93.2 6.5 .1 .2 --
100.0
Lbs/Batch
1950.0 136.0 (15.25 gals 2.0 4.0
1104.0 (133 gals.) 3196.0**
*Approximately 56.5 lbs/100 lbs. of active ingredients (this may vary + 8 gallons per batch.
** One batch yields 51 + 1 five gallon pail Ready Mix joint compound at 62- lbs/pail.
SPECIAL MIXING INSTRUCTIONS
- Blend ingredients in following order: 1) Water 2) Elvace EP-200 3) Nalco 4) Filler C-978 5) Mix until filler is dispersed 6) Add Acrysol ASE-60 7) Mix until Ready Mix is smooth - pumping viscosity should be 480 + 20 to allow for 24 hour viscosity build of 100 pts
WORKING CONSISTENCY Specifications for Paste
- Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5 cc water per 150 grams of paste may be added to adjust.
Brabender: (580 + 20) For Machine tools add 7 gallons ^0 (400 + 20)
/ pH
Minimum - 9.0
Maximum - 9.5
WORKING PROPERTIES
- Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working and free of any coarse, gritty or undispersed particles. Material shall be free from lumps due to incomplete mixing.
HCF:jr
Continued on Page 2.
SGP 0018320
August 2, 1977 Supersedes Formula C-979 Dated: 1/17/77
CHICAGO, ILLINOIS PLANT FORMULA READY MIX JOINT COMPOUND C-979 (HAND TOOLS)
DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for taping, topping and texturing.
FORMULA Raw Material
PZsotfcj-L-cjzA. -/ Filler C-978
Elvace EP-200 -/ Nalco 71D-5 -/ Acrysol ASE-60
Water
Function
Filler Adhesive Defoamer Thickener Solvent
RM Spec
185 125 147
--
Percent
93.# 6.5 .1 .2 --
100.0
Lbs/Batch
ho 1950.0
136.0 (15.25 gals.) 2.0 4.0
1104.0 (133 sals.) 3156.0** 3^7*
Approximately 56.5 lbs/100 lbs. of active ingredients (this may vary + 8 gallons per batch.
* One batch yields 51+1 five gallon pail Ready Mix joint compound at 62 lbs/pail.
SPECIAL MIXING INSTRUCTIONS
- Blend ingredients in following order:
1) Water 2) Elvace EP-200 3) Nalco
4) Filler C-978 5) Mix until filler is dispersed 6) Add Acrysol ASE-60 7) Mix until Ready Mix is smooth - pumping viscosity should
be 480 + 20 to allow for 24 hour viscosity build of 100 pts.
WORKING CONSISTENCY Specifications for Paste
Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5 cc water per 150 grams of paste may be added to adjust.
Brabender: (580 + 20) For Machine tools add 7 gallons ^0 (400 + 20)
-/ pH
Minimum - 9.0
Maximum - 9.5
WORKING PROPERTIES
- Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working and free of any coarse, gritty or undispersed particles. Material shall be free from lumps due to incomplete mixing.
HCF:jr
Continued on Page 2..
SGP 0018321
JJ^iVULM 7,
Jaauagy-'TrO', 1975 ` Formula C-97i CL-"IT? NEW
CHICAGO, ILLINOIS, PLANT FORMULA
READY MIX JOINT COMPOUND C-?l (HAND TOOLS)
TV> P i 4*4.
IL~- -- T-
DESCRIPTION OF PRODUCT - White Ready Mix Joint Compound used for ta-ping,
fro-pping, and featuring-. Special low-coat formula
For trial shipments only.
FORMULA Raw Material
Function
Percent Lbs/Batch
Water Nalco Elvace 1875 Fill >r C-9?e 972- '
Solvent Anti-foaming agent Adhesive Filler
-- .2
2.0 97.5
100.0
1024.00 4.00
39.00
1950.00
(128 (4.4
gals.)* gals.)
3017.00**
*Appi,oximately 56.5 lbs/100 lbs. of active ingredients (this may vary 8 gallons per batch.
**0ne batch yields 50 1 five gallon pail Ready Mix joint compound at 62 lbs/pail.
WORKING CONSISTENCY Specifications for Paste
- Refer to Plant Testing Procedure No. 32. If paste is not proper working consistency, a maximum of 5 cc water per 150 grams of paste may be added to adjust.
Brabender: (540 20) For machine tools add 10 gallons H2O. (400 t 20)
WORKING PROPERTIES Specifications
- Refer to Plant Testing Procedure No. 33. Compound shall be plastic, buttery working, and free of any coarse, gritty, or undispersed particles. Material shall be free from lumps due to incomplete mixing.
BONDING PROPERTIES Specifications
CRACK RESISTANCE Specifications
- Refer to Plant Testing Procedure No. 35.
Aftercompound has dried, tape shall show
at least 90^ fiber tear when delaminated.
/ oc)
- Refer to Plant Testing Procedure No. 37.
There shall be no Large fissure cracks,in
tlfe wedgej 'and no^cr^cks.-intKe thinner
haiof-th.Hd-ge.
^
^44.
COLOR
- White Dried compound shall match color of standard sample.
WNG:jg
SGP 0018322
BRUNSWICK FORMULA #979 ASBESTOS CONTAINING PRODUCTS
SGP 0018287
SGP 0018288