Document GmOKbmYbx70gp8VgN9L8d1w3q
APPENDIX III ASTM METHOD D -- FOR INVESTIGATING THE COMPATIBILITY OF TRANSFORMER INSULATION AND CONSTRUCTION MATERIALS IN ASKARELS
1. Scope 1.1 This method uses the change of electrical and/or chemical characteristics of transformer askarel resulting from controlled exposure to Insulation and construction materials, to evaluate their Immediate major contamination effect on the askarel fluid. Delayed or long time contamination effects may not he detected. 1.2 This method also utilizes various physical tests on the Insulation and construction materials after controlled exposure to the askarel to determine the compatibility of these materials with transformer askarel.
2. Summary of Method 2.1 Properly proportioned specimens of the insulation or structural materials are Immersed In refined askarel for 168 hours at 1001C. In a forced draft oven. Changes in electrical and chemical properties of the transformer askarel are compared against a control sample of the askarel treated in the same manner, in absence of the test specimens. 2.2 Color change or Intensification beyond that of the control indicates that the askarel has extracted color materials from the insulation or structural components.
0079919
TOWOLDMON0057002
-2-
.. > ' r~
2.3 Physical properties of the materials-of ins\fl.ation-and construction are determined before and after exposure to the askarel fluid.
3. Significance 3.1 The changes in the electrical and chemical properties are due to contamination from the test specimens. The magnitude of change is basis for judging the compati bility of the materials for use with askarel fluid. 3.2 Color change or intensification indicates solubility of some components from the test specimen, which may adversely affect the fluid. 3.3 The magnitude of change in physical properties of the specimens after exposure in askarel fluid are basis for Judging the short term compatibility of these insulation and structural components for use in askarel. 3.4 Conformance with the requirements of this method does not recommend a material for application, unless all other required performance criteria are met.
4. Interferences
4.1 If the askarel fluid has not been refined to a proper
level, required for standardization, then the results
may be obscured. Contaminated or improperly handled
test specimens, improperly cleaned sample containers,
handling devices, and electrical testing apparatus, can
also obscure results.
0079920
TOWOLDMON0057003
-3-
4.2 Solvents should not be used to clean the specimens unless It is part of the normal manufacturing handling process.
5. Apparatus
5.1 Sample Handling Apparatus
5.1.1 A forced draft oven, adjustable to 1001C.
5.1.2 Clean glass quart or 800 ml. containers fitted
with glass or aluminum foil covers, without
gaskets.
5.1.3 Clean metal tongs, thermometers.
5.2 Electrical Apparatus
Method
Dissipation Factor Bridge
- ASTM D-150
Resistivity Bridge
- ASTM D-II69
Cell
- ASTM D-924
Dielectric Break Down Voltage -
ASTM D-877
5.3 Chemical Apparatus
'
Neutralization Apparatus
- ASTM D-664
Karl Fischer Apparatus
- ASTM D-1533
5.4 Physical Testing Apparatus
Tensile Strength - Appropriate ASTM Method
Hardness
- Appropriate ASTM Method
Dimensional Change
-
Micrometer or Caliper
Weight Change
- Analytical Balance
Color
- ASTM D-2129
0079921
TOWOLDMONOQ57004
-4 -
6. Procedure
6.1 Refinement of the Askarel Fluid
The transformer askarel should be refined by adsorptive
treatment to the following specifications:
a) Color ASTM D-2129
150
maximum
h) Appearance
clear
c) Neutralization Number
0.014 mg
maximum
ASTM D-664
KOH/g.
d) Moisture, ASTM D-1533
30 ppm.
maximum
e) Dielectric breakdown
voltage, ASTM D-877
35 KV
minimum
t) Dissipation Factor,
ASTM D-924 60 Hertz 100c.
5,0
maximum
e) Specific volume re sistivity 100C.j
500 x 109
VDC, ASTM D-II69
ohm-cm
minimum
6.2 Preparation and Size of the Test Specimens
The specimens are prepared for testing in the same way
that they would be treated in the manufacturing process,
except that they should be transported with tongs.
[Suggested drying time for specimens is 105C. overnight]
The test specimens shall represent the "as used" condition
in the manufacturing process. For solid materials the
ratio of the surface area of the materials to the askarel
fluid will vary and should be estimated to be greater than
the ratio employed in the transformer.
0079VZ2
TOWOLDMON0057005
Some suggested ratios are: a) If the specimen can be measured, no less than 4
square inches (25.8 sq. cm.) are used with each 400 ml. of askarel. b) If the specimen is insoluble in askarel and the surface area cannot be measured, the specimen is used in the amount of one percent by the weight of the askarel. c) If the material is soluble in the askarel, the specimen is used in the amount of 0.5 percent by the weight of the askarel. d) Varnishes, wire enamels and materials used as dip coatings are cured on approved paper or aluminum foil and are tested at a ratio of 7 grams or approximately 100 square inches (645 sq. cm.) of surface area per 400 ml. of askarel fluid. e) Core steel and core 'steel coatings are tested at a ratio of 450 square inches (2903 sq. cm.) for each 375 ml. of askarel, for transformer applications. A realistic core steel ratio for regulators is 900 square inches (58o4 sq. cm.) of surface area per each 350 ml. of askarel. f) Gasket materials are tested at a ratio of 0.5 square inch per gallon (3.23 sq. cm. per 3.8 liters) or 0.053 square inches per 400 ml (0.34 6q. cm. per 400 ml) of askarel.
0079923
-6 -
6.3 Test Details
.
6.3.1 Depending on the volume requirement of the
dielectric cell add 400 ml. to 600 ml. of the
refined askarel fluid into a clean glass Jar
or beaker. Add the test specimen and leave
an air space for expansion.
6.3.2 Cover the beaker or glass Jar with a watch
glass or Jar top made of glass. Prepare a
similar glass container filled with an
equivalent volume of the same source askarel
fluid, as a control.
6.3.3 Place the Jars into a forced air circulation
oven adjusted to 1001C. and heat for 168
hours. Then remove the Jars from the oven.
Remove the specimens. Make the dissipation
factor and resistivity tests. Then pour the
askarel back Into the containers. Cover them
and cool to room temperature.
6.3.4 Observe the Jars containing the cooled fluid
' for cloudiness, discoloration, settling out
of fillers, etc. as compared against the
cooled control askarel fluid.
6.3.5 Determine dielectric breakdown voltage
ASTM D-877.
6.3.6 Wash the specimens with a clean suitable
solvent and dry. Then determine the physical
properties indicated in 5^ and compare against
the unexposed materials.
007<)2>
TOWOLDMONOQ57007
-7 -
7. Interpretation of the Tests Made on the Askarel Fluid
7.1 The test results obtained on the askarel containing the
samples must be compared with those of the control
aBkarel to determine the effect of the samples on the
askarel.
7.2 A significant change in any of the characteristics would
Indicate lack of compatibility and should be further
studied.
7.3 The properties of the control askarel after heating for
168 hours in absence of a test specimen should be:
Charact eristics
Values
Color ASTM D-2129
150, maximum
Moisture ASTM D-1533
30 ppm, maximum
Neutralization Number ASTM D-664
.014 mg KOH/g. max
Dielectric Breakdown Voltage ASTM D-877
35 KV, Minimum
Dissipation Factor ASTM D-924 (60
Hertz, lOO'C.)
7.5$, maximum
Specific volume resistivity 100C. 500 VDC,
ASTM D-II69
'q
~sf^r x l(r ohm-cm min.v
7.4 The properties of the askarel heated for 168 hours in
the presence of a test specimen should be:
Characteristics
Values
Color ASTM D-2129
200 maximum
Moisture ASTM D-1533
35 ppm, maximum
Dielectric Strength, ASTM D-877
28 KV, minimum
Dissipation Factor ASTM D-924,
(60 Hertz, 100C.)
20$, maximum
0079925
TOWOLDMONOQ57008
-8-
Characteristics Neutralization Number, ASTM D-664 Specific volume resistivity 100C., 500 VDC, ASTM D-II69
Values .03 mg KOH/g. max
50 x 10^ ohm-cm min
8. Interpretation of the Tests Made on Solid Insulating Materials 8.1 Obvious changes in the physical properties or dimensions of the insulation or structural materials must be considered on the basis of the specific needs of the application. 8.2 Wire enamel, tests are made to assure the physical integrity of the enamel following exposure to the askarel. Commonly used evaluation tests are bendability, scrape abrasion and dielectric breakdown. 8.3 Gasket materials are evaluated by determining the degree of swelling or embrittlement, using dimensional changes and durometer hardness. 8.4 Organic coatings and adhesive materials shall maintain their integrity after exposure to the askarel. 8.5 Laminated materials shall not delaminate after exposure to the askarel
0079926
TOWOLDMON0057009