Document GKyEXOMewgX4Bab18QxYxd99Y

Monsanto Chemical Company Organic Chemicals Divisio CHEMICAL SPECIALTIES DATA REPORT The informiilion in IliiH ro|H>rl wns compiled to modal you in your cviiIur(ion nnrl development of opecml ubcr for Monsanto product**. ftvery efforl has Iwen made lo include |>crtinent material boarinfl on Ihn nuhjoM. Thin information is intended to guide your development work, hi it Mun*nnlo cannot lake part in the ivjiee/lic formulation or evaluation of any fin/whed product . . since knowledge of such fdmuld be reserved lo youreclf and 19 often your moat valuable trade uccret. No. Date cs-14 November, i960 AROCLOR* FIRE-RETARDINO PLASTICIZERS AND MODIFIERS FOR EPOXY RESINS Beoause of their outstanding ohemlcal resistance and adhesive char acteristics, epoxy resins are widely used for the production of surface ooatings, adhesives, laminations and plastic parts. To impart flame resistance -- with attendant lowering of cost -Aroolor compounds oan be added to the resins in various proportions. The flame retardant resins so produced have many Important uses. In laminations and plastic parts, for example, It is often necessary or even mandatory that flame resistance be built into the finished product. By selecting the proper Aroclor, formulators. can meet requirements for fire resistance while, at the same time, adjusting such other Important properties as flexibility, hardness and viscosity. Chemically, the Aroclor compounds are dl- and poly-phenyls chlorinated to a definite per-cent-by weight of inert, bound chlorine. Physically, they range in form and appearance from Aroolor 1221, mobile oily liquids, to Aroclor 5460, hard transparent resins. Chemically, the Aroclor compounds are impervious to moisture, acids and alkalis; they are extremely heat stable and will not support combustion. When added to resinB, the Aroclor compounds function as low-cost plasticizers imparting fire-retardant properties to the resin formulation as well 63 other desirable end-product oharaoteristlos. This report oovers the application of Aroclor plasticizers in epoxy resin formulations. 0212809 * Aroolor is a trademark of Monsanto Chemical Company for its chlorinated aromatic hydrocarbons and their derivatives, Including chlorinated diphenyl. Reg,. JJ. S. Pat. Ofo. I I I The Irrformulinn in Itiin bulletin Is. ( our l**i ku.<*..<!*.., Irw *.! accural*, Iml alI wommr>n<ialihK <>r n*ijztf****(ar>- inuilw williuui K,,Hr,.inn, (he (vuibiiionH of om* an lw,vn.ul mu cnirol. The J Mniuio Cbamlwl L'miiinoiv diackima uny liability intii'wl ..in ` ...^ ..Jit cunneclion w|ih thn u*' of Him- dl or MumfeitinnH. I'urlltarmore, rwlhin* onuimnc.l herein ihull le ismslrueil t> a rennu nynirtadop to u<m ny iifpduol in oenllul toilh xlsllng p*l*nU covering afljfMwawlal yiy ' *0,10 J TOWOLDMON0043538 WATER_PCB-00028007 TI1K NEED FOR AUOCLOH M 2.KIC; When incorporated Into epoxy rosin formulations, Aroclor compounds can be uaed to impart fire resistance; to increase flexibility; to improve processing; to maintain chemical resistance; to maintain adhesive characteristics and to lower finished product costs. The quality advantage of Belf-extlnguishing epoxy compositions is of great interest in electrical, structural and coatings applications. Aroclor compounds are outstanding for providing fire retardancy since they offer the additional advantages of high chemical resist ance (inertness), resistance to water, acid and alkali extraction and very low per pound co3t. Frequently, the addition.of Aroclor results in lower over-all finished product costs by their replacing a percentage of the higher coat ingredients. SELECTED PROPERTIES OF AROCIOR COMPOUNDS The Aroclor compounds, from Aroclor 1221 to Aroclor 5*160, span a wide range of physical properties. Over the series, the properties vary in a regular gradient; giving a choice for optimum usefulness in any particular application. Adjustment of formulation properties can further be made by "blending" two or more Aroclor compounds to give a mixture for the specific use. The five* (of twelve) Aroclor comppunds listed illustrate the variety of properties available. * For a complete summary describing the properties of the entire series of twelve Aroclor compounds, request a copy of "The Aroclor Compounds." Address request to: Monsanto Chemical Company Organic Chemicals Division Dept. CS-14 800 N. Lindbergh Blvd. St. Louis 66, Missouri . Monsanto Chemical Specialties Data Report CS-14 Page 2 0212810 TOWOLDMON0043539 WATER_PCB-00028008 TABLE I THET PROPERTIES OF AROCLOR COMPOUNDS Aroclor 1221 Colorless mobile oil Aroclor 12^2 Practically colorless mobile oil Aroclor 1260 Light yellow soft sticky resin Aroclor 1268 White opaque resin Aroclor 5^*60 Yellow Trans parent re sir. - Acidity - Maximum (Kgm.KOH per Gm.)................. Typical Density Specific Gravity 250/z5c (tt0/770p)............. Lbs./Gallon-25C (77F).. Distillation Range ASM D-20 (Mod.) Corr. C....................................... Evaporation Loss - ASTH D-6 Mod. 0.015 0.015 1.182 9.85 1.330 11.50 275-320 325-360 1.0 to 1.5 3.0 to 3.6 0.0 to 0.1 0.015 1.620 13.50 385-120 0.5 to 0.8 0.0 to 0.1 Plash Point Cleveland Open Cup-C... F... iii-i5o0 286-302 176-180 318-356 None n Fire Point - Cleveland Open Cup - C......................... P......................... Pour Point-ASTM D-97-C. Softening Point -- ASM E-28 - C....................... F............................ Refractive Index D-llne - 20C............... Visccsity-Saybolt U.- ?10F (98.9C)............... :3of (5i).uc ............... ICO";- (37.8Cl............... 176 349 Crystals at 1C Crystals at 31 F N, S 1.617-1.618 30-31 35-37 10-42 None* -19 2 -- 1.627-1.629 31-35 19-56 80-93 None 31 88 '- 1.617-1.619 72-78 3200-1500 * None indicates "No firs eoint uo to boilinz temperature. 0.05 0.07 1.810 15.09 1.670 13.91 135-150 28o-335 at 5 mm- Kg. 0.1 to 0.2 0.03 0.0 to 0.6 1.5 to 1.7 (at 260-5 hrs.) None None None None -- 135 to 160 100to 105.5 (hold pt.) _ rt 275 to 320 212to 222 (hold pt.) . -- 1.660-1.665 " -- TOWOLDMON0043540 WATER_PCB-00028009 PROPERTY IMPROVEMENTS OF EPOXY FORMULATIONS The Aroclor compounds represent one of the few plasticizer type materials that possess a high degree of compatibility with epoxy resins. The lower chlorinated members, 1S21 and 1232, Impart a high degree of flexibility to epoxies while the more resinous and solid Aroclor compounds, e.g., ;5460, have little flexibilizlng effect, in fact, tend to act as reinforcing resins. Aroclor compounds, in general, have negligible influence on the hardness, tensile or compressive yield strength of epoxy resins. In phthallc anhydride cured systems, the ultimate compressive strongtn can even be Improved by addition of solid Aroclor compounds to the formulation. When used in the range of 15 to 20 parts per hundred of reoln, all of the Aroclor compounds greatly retard the burning rate of epoxy compositions. A small amount of antimony oxide added to the Aroclor formulations further Increases the fire-retardance greatly and the epoxy formulations become non-burning. Aroclor creates self extinguishing characteristic; the antimony oxide functions to reduce afterglow. In addition, the antimony oxide can replace a portion of any fillers that may be employed. Aroclor compounds are especially useful whenever finished product cost plus other specific qualities, such as good resistance to chemicals (especially acid and alkali), are Important factors. In surface coatings, for example, Aroclor 125**, 1260 and 1262 provide both formulating economy and excellent chemical resistance. However, Aroclor should not be used where maximum organic solvent resistance is desired since It Is a true plasticizer and not chemically bound to the resin. In potting compounds, Aroclor compounds can provide added flexi bility to improve the shock resistance of the encapsulated device. In addition, by proper selection of the Aroclor compound, the coating viscosity can be greatly reduced. Better tacklne33 can be developed in epoxy adhesives by the "stickiness" property of Aroclor. In epoxy sealants, besides fire resistance, easier workability develops in the formulations. Wherever fire-resistance. Inertness, better flow and improved handling characteristics are needed, Aroclor compounds should be evaluated. Their unique properties and the effect on the epoxy resin as well as their low cost per pound recommend their evaluatlon for a variety of epoxy resin end uses. LABORATORY DATA -- AROCLOR COMPOUNDS IN LIQUID EPOXY RESINS The following data have been assembled as a guide for formulators of epoxy resins. Careful study of these data disclose several generalizations. 021281* Monsanto Chemical Specialties Data Report CS-14..................... Page 4 TOWOLDMON0043541 WATER_PCB-00028010 The uae of liquid Aroclor In an aliphatic amine-cured system -- 20 parts per 100 parts of resin basl3 -- results In a self-extinguishing formulation. Replacement of five parts of Aroclor with five parts of antimony oxide produces materials with still better flame retardancy. Flexural strength and compressive yield strength Is Improved while tensile strength remains unaffected. There is a slight lowering of heat distortion temperature and ultimate compressive strength. In phthalic anhydride cured systems, solid Aroclor compounds greatly Improve ultimate compressive strength, flexural strength and tensile properties. Compressive yield strength Is comparable to the unplas ticized control while heat distortion temperature Is lowered slightly The liquid epoxy resins used in the experiments recorded In Table II are representative of commercial types such a3 Clba's Araldlte 6010, Jones and Dabney's EPI-Rez 510, Shell's Epon 828, Bakelite's ERL 2774 or Dow's DER 332. 0212B13 Monsanto Chemical Specialties Data Report CS-14.................................... Page 5 ^ TOWOLDMON0043542 WATER_PCB-00028011 TABLE II AROCLOR IN LIQUID EPOXY RESIN Formulation Cure: 16 Hr. R. T. + 2 hrs.g TOOC. Control Modified 12 345 i0 20 Hrs. @ 150C. 769 Control 10 Liquid Eooxy Resin 100 100 100 100 100 ICO 100 100 100 100 Dlethylene Triamine " 13 13 13 13 13 - * - " Aroolor 12o0 0 - 20 15 - - - - - - - Aroolor 1242 s - - - 20 15 - - - - Antimony Oxide > - - 5- 5- 5- 5 Aroolor 1263 - - - - " 20 15 - - - Aroolor 5460 2 - - - - - - - 20 15 - Fh.tha.lic Anhydride ^ - -. - - - 75 75 75 75 75 DM? 30 (Rohm & Haas) a. " " " .1 .1 .1 .1 .1 Flammability astm 635-56T ' .82 in/' min. l-5l-/E8. r1 N.B. S.E. N.B. . 38 in/ N.B. .38 in/ N.B. .6 in/ 2-1/8" min. min. min. Heat Distortion Temp. C. 117-5 87 92 79-5 81.0 128 134 135-5 135 143 Roclewell "M" 104 103 106 108 1C7 112 112 113 111 111 Flex Strength PSI 20,000 23,800 22,100 21,500 22,200 25 ,900 20,0C0 26,300 19,000 16,900 Tensile PSI 11,400 13,000 9,8co 10,700 12,800 13 ,500 11,100 11,500 10,200 11,000 Compressive Yield Strength PSI 15,700 17,250 16,950 17,900 16,700 22,300 20,500 21,000 21,200 20,900 Compressive Ultimate . Strength PSI 43,000 32,900 38,150 32,500 32,400 36 ,500 36,700 41,700 40,700 23,400 S.E. = Self extinguishing N.B. = Mo burning TOWOLDMON0043543 WATER_PCB-00028012 Table III Illustrates some other typical physical property modifi cations Imparted by Aroclor 1221 and 1248. In each case, the formulation consisted of 100 parts epoxy resin (as in Table II), 25 parto of Aroclor and 8 parts of tetraethylenepentamlne. Compatibility Liquid Room Temp. Cure 30 Min. Cure 100C. TABLE III Control Compatible Compatible Compatible Aroclor 1221 Compatible Compatible Compatible Aroclor 1248 Compatible Compatible Compatible VISCOSITY* Before adding curing agent After adding curing agent 12,800 7,900 . 1,650 1,200 7,700 4,300 PHYSICAL PROPERTIES** Izod Impact Resistance 0.2 0.6 Clarity: ^ light reflected 3-0 3.0 3.0 Shore D Hardness (10 sec.) 78 8 40 PHYSICAL PROPERTIES AFTER HEAT AOINO*** Shore D Hardness (10 sec.) % Weight Change 86 -0.012 81 -2,118 88 -0.682 * Brookfield LVF /AI spindle at 60 r.p.m. ** Samples cured 30 min. at 10GC. with 8 p.hr. tetraethylenepentamine *** Aged 24 hours at 86C. In activated carbon EFFECT OF CONCENTRATION OF ANTIMONY OXIDE AND AROCLOR ON FLAMMIBII..ITY To determine the effective concentration of Antimony oxide and Aroclor (equal parts by weight), several test resin mixtures were prepared. Liquid epoxy resin (Shell Epikote 834) was mixed with Aroclor and antimony oxide and cured with 8j! dlethylenetrlamine. Specimens were prepared In wax molds 9"x "x f" . The flammibility tests were based upon the British Ministry of Supply Aircraft Specifications DTD 5537 Appendix 10. This procedure consisted of clamping the test specimen In a support with its longitudinal axis horizontal and Its transverse axle Inclined at 45. A bunsen burner was applied with the tip of the flame 1/2" to 3/4" Just in contact with the end of the specimen. At the end 30 seconds, the flame was removed and the specimen allowed to burn. If burning did not continue, the flame was replaced for 30 seconds and If the specimen again failed to continue burning, the material was classed as Belf-extinguishing. These results are listed In Table IV. 0212815 Monsanto Chemical Specialties Data Report CS-14.....................................Page 7 | TOWOLDMON0043544 WATER_PCB-00028013 TABLE XV AROCLOR AND ANTIMONY OXIDE (50-50 Mix) Weight $ in Resin 5 7.5 10 15 Aroclor 1242 Inflammab]e Inflammable S.E. (30 sec.) Aroclor 1260 Inflammable S.I. S.E. (30 sec.) S, E. immediate Aroclor 4465 Inflammable S.I. S. E. (20 sec.) S.E. immediate Aroclor 546c Inflammable S.E. (40 Bee.) S.E. (20 sec.) S.E. immediate S.E. Self-extinguishing S. I. - Semi-inflammable ************ For samples of the Aroclor products mentioned in this report, contact the nearest.branch office (see attached list) or write to: MONSANTO CHEMICAL COMPANY Organic Chemicals Division Plasticizers Department 800 North Lindbergh St. Louis 66, Missouri Monsanto Chemical Specialties Data Report CS-14.......................................Page 8 TOWOLDMON0043545 WATER_PCB-00028014 . MONSANTO CHEMICAL COMPANY Organic Chemicals Division District Sales Offices ATLANTA: 1401 Peachtree St. N.E., Atlanta 5, Georgia BOSTON: Everett Station, Boston 49, Massachusetts , CH1CAQO: MeOraw-Hill Building, 520 N. Michigan Ave., Chicago 11, 111. CINCINNATI: 2330 Victory Parkway, Cincinnati 6, Ohio CLEVELAND: 427 Hanna Building, Cleveland 15, Ohio DETROIT: 10230 Grand River Avenue, Detroit 23, Michigan HOUSTON: 2472 Bolsover St., P. 0. Box 6863, Houston, Texas LOS ANGELES: 6670 E. Flotilla St., Los Angeles 22, California MINNEAPOLIS: Foshay Tower, Room 515, Minneapolis 2, Minnesota NEW YORK: 445 Park Avenue, New York 22, New York PITTSBURGH: 20 Cedar Boulevard, Pittsburgh 28, Pennsylvania SAN FRANCISCO: 111 Sutter Street, San Francisco 4, California SEATTLE: 911 Western Avenue, Seattle 4, Washington SYRACUSE: 731 James Street, Syracuse 3, New York WILMINGTON: 2005 Concord Pike, Fairfax, Wilmington 3, Delaware ****** LONDON: Monsanto House, 10-18 Victoria St., London S.W, 1, England MELBOURNE: 256 Flinders Street, Adelaide, Australia MONTREAL: P. 0. Box 900, Montreal 3, Canada TORONTO: I83 Front St. East, Toronto 2, Ont., Canada VANCOUVER: 1550 Rand Avenue, Vancouver 14, B. C., Canada 02l*8v7 Monsanto Chemical Specialties Data Report CS-14............................... Page 9 TOWOLDMON0043546 WATER_PCB-00028015