Document ExoXnv7jo5EeE5R35jO9pnXrb
d at e 2-4-66
c har g e
WRITTEN b y
F Klenke, Jr,
OBJECT; tpn prepare a bronze colored flake product using glass flakes as the
_________substrate.
______ .
_____________ __________ ,
.
STEP-VAT
PROCEDURE '
.
#
USE OZ.
ANALYSIS
100%
1 Into 170 lbs. of water at 800. dump 39#
of glass flakes (equivalent of 0U-2351-H)
V
2 Stir 10 minutes, then, over 2 hrs. period.
2.04 lbs, TlOo (using "L" liquor)
'
... 3
Heat to boil, at 1*0./min. and hold at
temp. 1 hr. _________ ~
___________
,4
Eliterf wash SOa2 free (I 1500-^ )
.........5.... Realurry In 25 gal, water at 20t>-250.
6. Pour in 42 lbs. of Copperas (N-262V and
stir 15 mins. at temp.
'
7 Add over 5 min. period a solution of
/water -300#
1 355$ Ho 02 -42# `
_8
Heat to 8oC. at 2C./min, rate and hold
1/2 hr. at 78-82C.
Q Press and wash SOa2 free(ca 1500-*- }
10 Dry, then heat treat 1/2 hr l
at 65o- 66oC.
f
lot ^ 10896
\
V ...... v.,,'
> .
iJ;
mu.
K-14097 '
l u mp ,
4fi . g# naiMO
` PULV.; ..... .
. . SPEED! Mad k By .
N39898
'
NOTES This product is a bronze flake, considerably wore intense and brighter than NF~103-I>. Xt has the gen eral properties of NF'103-D except a lower melting point of about 7500. The final product contains 4.7$ TiOg and has the fol lowing size distribution:
trace + 40 mesh
74$ - 40+200 mesh
11.95?' - 325 mesh
E. KLENKE