Document EqRYQQJMqpqxnxOz6K6Z5mJwb
uv; ocoi
STATUS REPORT MECHANICAL PROPERTIES OF ESTANE-CHLOROBENZENE-
ASBESTOS SYSTEMS
tuthors: J. A. Faucher J. V. Koleske
Oat*:
November 10, 1965
Project No.:
399A50
Fil* No.:
4858
SUMMARY Mechanical properties have been determined for blends of Estane polyurethane, chlorobenzene, and asbestos.
?he tensile properties of these systems are equivalent to or tetter than Estane at asbestos contents of up to 30%.
About 30-35% asbestos can be added to the Estanehlorobenzene system and still obtain transparent molded >laques. Without the chlorobenzene, even 10% asbestos is eadily visible in Estane. Since the additives are considerably < heaper than the elastomer, these systems or similar ones may e of commercial importance.
NTRODUCTION In a recent report (1) we commented on the fact that the addition of chlorobenzene to Estane
S701-F1 (a B. F. Goodrich Chemical Company polyurethane) had a arked effect on the tensile properties of the polymer. This improvement of tensile properties prompted an investigation of the effect of asbestos filler on the tensile properties of the
Rstane-chlorobenzene system.
EXPERIMENTAL Various amounts of chyrsotile asbestos (high purity, Coalinga) were milled into Estane
containing 12-15% chlorobenzene at 120-150C. for 5 minutes. (Ml percentages listed in this report are based on the Estane). ILaques of the milled material were molded at 150C. and 1)00-2000 psi (10 seconds). Room temperature tensile properties vi ire obtained with an Instrom tester at a strain rate of 20 p ircent per minute. The real component of the complex shear m>dulus, G', and the mechanical loss were obtained as a function o ! temperature with the recording torsion pendulum.
Research and Development Department Chemicals Division
Union Carbide Corporation
UC-416*
2
DISCUSSION The first point of interest was that the molded plaques were clear when up to 33% asbestos was
ided, i.e., no small particles of asbestos were visible. H iwever, in the absence of chlorobenzene even 10% asbestos ( ;he lowest asbestos composition investigated) was clearly v sible in the molded plaques. It seemed that milling at 150C. p -oduced clearer plaques than those obtained by milling at a >out 120eC. Orientation of the clear plaques resulted in an o >aque, white material.
In Figure 1 .the mechanical loss spectra of Estane a id of certain chlorobenzene-asbestos-Estane systems are shown. A ; might be expected, chlorobenzene causes a decrease in the g .ass transition temperature, Tg, of Estane. Addition of 23% a ibestos resulted in an increase in Tg. If the asbestos were a :ting as an inert filler one would not expect a change in Tg, a .though the magnitude of the mechanical loss should decrease at t ie transition. Therefore, the increase we see in Tg probably r fleets an interaction of the asbestos with the Estanec ilorobenzene system. The clarity of the molded plaques is a other indication that an interaction exists. Figure 2 shows t e real portion of the complex shear modulus as a function o temperature. It is interesting to note that even though t e glass transition occurs at a lower temperature with the E tane-chlorobenzene system, above 0C. the shear modulus is s gnificantly higher (in keeping with the tensile data). Also, t is. system will be more flexible from -20 to 0C. than Estane. A dition of asbestos caused the shear modulus to be markedly
gher over the temperature range investigated.
The tensile properties of the systems studied a|fe shown in Figure 3, 4, 5 and 6 as a function of the percent a bestos-added. As a reference point, the tensile property of Eitane containing no additives is shown on each plot. Young's m<dulus, Figure 3, increases as the amount of asbestos added is increased. The percent elongation. Figure 4, decreases as tie asbestos content is increased, however,, even with 30-40% as bestos the Estane-chlorobenzene-asbestos system has the same elongation as Estane without these additives. Thus, for an eid use that requires a higher initial modulus along with the iiberent elongation of the polyurethane, these blends may show sc ne promise. In addition, it should be noted that two low cc st materials can be added in fairly high amounts and still msintain the same properties in a rather expensive polymer.
The rapture energy. Figure 5, and the ultimate si rength, Figure 6, of the asbestos systems decrease as the
3
a sbestos content is increased* However, here again up to a jout 30% asbestos can be added to the Estane-chlorobenzene s rstem and still achieve property values equal to that of Estane.
F jferences 1. Faucher, J. A. and J. V. Koleske, Informal Report, Tensile
Properties of Estane with Various Additives, Project No. 399A50, 15 Sept., 1965.
a ic A ;tachments: 6 Figures
Figure 1. Mechanical loss of Estane and Estane plus additives
M e ch a n ica l Loss
lo g G ', G' in dynes/cm
Y o u n g 's M o d u lu s, dynes/cm
'igure 4. ..
Percent Elongation of Estane-ChlorobenzeneAsbestos Systems. Samples contained 12-15% chlorobenzene and indicated amounts of asbestos based on only Estane. Open circles are average values and the vertical lines indicate the maximum and minimum test values.
P ercent E lo n g a tio n ,
.60
igure 6.
Ultimate Stress of Estane-Chlorobenzene-Asbestos Systems. Samples contained 12-15% chlorobenzene and indicated amounts of asbestos based on only Estane. Open circles are average values and the vertical lines indicate the maximum and minimum test values.
n i o
iH
x
a(0
tinn o u
CO
0)
eg E
60
. '399A 0
DIST1 IBUTION
Mr. : H. Anderson Dr. ' . K. Asbeck Dr. '. E. Bailey Dr. i . M. Bryant Dr. . E. Critchfield Mr. >. L. Engle Mr. : M. Harmon Dr. : . Hostettler Mr. ! S. Kincaid Mr. : . G. Lombardi Mr. . . S. Lovell Dr. i . Magnus Mr. i . S. Maxwell Mr. < . E. Montagna Dr. i . H. Potter Mr. j . F. Rogers Mr. : . T. Simon Dr. 1 . N. Stoops Dr. J. W. Tinsley Mr. I . Van Cleve Mr. ]. R. Walter Mr. 1 . D. Whitman Mr. (. J. Whitworth Infoination Retrieval Authqrs (10)
Dr. il. Brown, BB Mr. J. Dagon, BB Dr. I. G. Imhof, BB Dr. C. N. Merriam, BB Mr. V . A. Miller, BB Dr. E. White, BB
Dr. K| L. Brown, TNY Dr. q E. Petersen, TNY
Mr. D. Jenkinson, Orangeburg, NY
Dr. H L. Reichard, Mining and Metals Division Mr. R G. Woolery, Mining and Metals Division