Document EqKqb10xaQ3J0b7Yv29pDYEeb

,h NAW: O LOCATION. J. H. Orem - E3ND jpr' ^ r' IS^ A L * ; si SC t TO n COf o H o >~y ic'Otember Ip;, 1972 '-1-. - wCrri03.nv 3l t r Louis Visit September 7&d _1_ y 2 - Dr. Richard K. Heine, Gary Clson r' 'Cook - 1180 To * cc D. H. Beentold cJ A. Cannon nro w. It. Coaker v s. Clark J. H. Darby - 1' D. J. Derby p. E. *RrJ . Graham Kaiser R. E. Lamkin ii * y. Morgan - ; w. Touchette 1C-J >0 Ty- rodeo Fro:. 3 0 . Low r.enperature is not important. Hardness is. a Snore "A" 30 -.-.ax. Oil and grease (axle grease and light weight oil) resistance are needed. Thickness is 10-60 mils ana for the oily environment product it is ca 20 mils. Current plasticize: system is DID? and DIDA. . - Plasticizer system presented and discussed: 40 mil sheer bp ??:R-rO.p?HR DS-2Q7 DIDP/DIDA (p6/S) s-711 S-51p S-711/S-146 (3:1) S-711/S-429 (1:1) 2 --111 (67 PHR) s-T-9 S-711/S-S7A (1:1) S-ml2 (67 PHR) 3-2^8 (67 PHR; S-lcO '/0-LS. L' (j-L 9_ O-V T^C 24 hr/b day -42 -49 -39 -R5 -30 -9 -18 -61 -29.5 -0.9 -24 2.5/9.0 1.7/7.8 3.9/18/7 1.8/3.5 - /6.2 - /1.8 - /2.0 6.0/24.6 - /5-9 1.0/3.4 6.0/ - Shore Hardness ' 72 73 70 73 71 83 76 67 71 79 70 Extraction Kerosene 8p 75 12 46 15 0.6* 1.0* 76 - 4.2* 0.6* 7.9 ~0 C CX -- J ' barer T it 17.0 20. C 7V -9 .,, O t -J _' _ 1C. a- - 21 -hexane, 4 hours/R T volatility = 87C/24 hours in activated carbon Shore Hardness = 10 second hold down Kerosene = 24 hours/R? Soapy Water = 50C/4 days Discussed styrene and A3S mar in relation to their question on laminating PVC film to other polymers. Polymeries are okay with styrene, marginal with some ABS types, and not good on nitrocellulose migration resistance. Melt flow properties of polymeries are higher than monomerics. DSW 587358 STLCOPCB4092694 51: Company 2 >60 --o '-- tr } 1572 On y.-ostherablllty, in general poljnoerics are rood, 077 7.- C. 7. _l. G. w C Z yuoa . <....* ac-ioa ...es are not as good. Filled system 1GC-GC c7T7 opacifying agent - such as TiOp rutile - when used ouOG07o Many of cur Florida and Arizona weathering results v;ei'*e Ghov:n discussed. 3'! Co. has ;ome films being expo: ec in Florida. e Fungicides - Vanelae 89, R.T. Vanderbilt, is the most commonl'* used in ?V0. 5-1 feel it may be deactivated by sunlig Vinasene 3-2-5 (arsenic containing) is deactivated by sunlighv according to 3-M Ve have recently prepared films usi:ng some 20 commercially available fungicides and sent them to ?1 orida for ourdoor exposure evaluation. _ Plastisois Their plasticizer system is not D_lD?/DiDA as we had assumed; it is BBP. Requirements are: Viscosity, Brookfield, 50 rpm Viscosity stability, A8 hours Fusion temperature Tear strength Elongation Tensile strength Oil & C-rease resistance 2000 cps 2500 cos ca 31CbF. 170 lbs. u i/OC/jf, 1500 DSi Formulations discussed: ;1 2 3 7 b Opal on 400 (raed. MW homopolymer) Opalon R-76H (low MV homopolymer) Ooalon 400 (low MW cooolymer) BID? ` DIDA S-711 S-l60 G-62 (ESO) Mark 462 (Ba/Cd/Zn) 100 56 9 3 2 ICO 65 3 2 ICO 100 * 53.5 6.5 3 2 85 3 2 100 Oy b 2 After fusion 310F/5 minutes Tear strength, lbs. Elongation Tensile strength, psi Fusion C : 90 150 1170 172 115 188 1280 165 140 230 1490 - 150 230 1400 160 188 4io 2050 143 To achieve low viscosity and viscosity stability blending resins (MO 85 from Goodyear ana VC 260S from Borden should be considered. We are to develop an organisol or plastisol recipe, using their requirements, that will have good oil and grease resistance. WR has been written. 1 SW 587359 h .. ! STLCOPCB4092695 3H Company Pa September ipj 1972 Plan-mat Hit;/ 3K wants to achieve a 25 flame spread rating in the Stiner tunnel, smoke generation is not a concern at this time. We discussed our Alumina Trihydrate evaluations and explained it works best wish phosphate plasticizers. KH-3o, formerly KH-45 (Kaiser) is 4.pd/lb; Hydral 710 (Alcoa) is 96/lb. The latter is a fine particle size and twice as efficient as KH-36. Flame retardance is more of a concern in the extruded product than it is In the plastisol. In theory, S-148 is only 65/ as efficient as S-140; in practice in PVC, S-148 is 85-90$ as efficient* S-148 is' lower in smoke. <2iW~? / ; - 'fa bs-ji- cC . o When phosphates are used. Drapex 10.4 (epoxidized linseed oil) should be used rather than ESO. The 10.4 has a higher oxirane oxygen content than ESO. Formulations presented and discussed and approximate f'larme spread and smoke ratings: Opalon 650 S-711 S -429 S-148 S-14R S-140 Q QuI Stabilizer Ba/Cd Drapex 10.4 Atomite Hvdral 710 EH-45 100 19 25 21 1. 3 30 OJ 1 i--i m 100 35 30 3 20 30 100 35 .5^ 30 1-2 < 20 30 20 100 35 30 1-2 3 20 30 20 100 65 1-2 3 20 30 * 20 - ca Flame Spread ca Smoke Rating _ 20 20 20 10 - 30 50-60 50-60 20 In the tunnel test. where the specimen "is at tached to the roof. the 3M Company Green Refractory Cement should be used to insure good adhesion and prevent the specimen's separation from the roof and hanging vertically inuo the flame. Smarting point guide line ratios for varying degrees of PR severity are: . STLCOPCB4092696 3M Company Page 4 September 15, 1972 Phosphate:A1. Trlhydrate Maximum FR Steiner = 25 FS or Cal. Fire Marshall CCC 5903-l8l8 (Army vertical burn) 1:1 3:2 Moderate FR Steiner = 75 FS .1:3 DOT (MVSS - 302) MVSS 1:4 1:5 Stabilizer systems Normally 3 PHR of ESO or Drapex 10.4 is used for processing heat stability. When the PVC is used outdoors Epi Rez 8lO or Epon 828 2 PHR should be considered to replace the 3 PHR of ESO. 10$ replacement of the primary with S-l4l improves outdoor stability. Mark LL (liquid Ba/Cd) @ 2 PHR & Mark PL (Zn/phosphite) @ 0.1 PHR with stearic and as needed provides a good stabilizer system. Mark WS (solid Ba/Cd) @ 2 PHR & Mark C (Cjelator) @ 0.5 PHR gives good heat stability but is not good on outdoor exposure. ^. Filler Up to 25-50 PHR does not have too much affect upon extraction resistance or T^. Above 50 PHR there is a decline in properties. Low temperature brittleness is adversely affected by any filler addition. Outdoors, even low levels (5-10 PHR) of calcium carbonate can be detrimental - produces a translucent effect. Oil absorption number of fillers can affect yield in plastisols. Clay is used in electrical compounds for its good electricals. Comment With all this discussion they would not indicate the applications. Believe they have test marketed some products. 1973 potential may be 200 M pounds of plasticizer. /cs I A M ^ohn Orem DSW 587361 STLCOPCB4092697