Document Ed5g5OB4b24Ye33Jqx97g6r5n
--J )
UNITED STATES PATENT OFFICE
2.6CS.996
HYDROUS CALCIUM SILICATES AND METHOD OF PREPARATION
George L. Kaiouaek, Toledo. Ohio, tiilrior to Owens-nJinois CUn Companj. * corporation of Ohio
No Drawing. Application March 26, 1552. Serial No. 271.745
1C Claims. I CL IOC--1201
1
This Invention relates to a new hydrous eal-
Further dispersion may be employed for the
c:um silicate, and to a method of preparing the purpose of avoiding aggregation between the re
lime:
actants and/or the reaction products--and thus
In the art of making hydrous or hydrated lime to assure a product of small particle size.
iriicate*. it has heretofore bees the controlling * The preparation of the new compound may be
aim to obtain a product havint a desired com effected with anhydrous silica la the form of
bination of physical properties which would en quartz, or with the successive grtdes of hydrated
able it to serve the purpose or purposes for silicas, to and Including silicic add--and like
which the product was Intended. Such products wise with any selective mixture of such silicas
have been a compromise between the available l(* as the silica component.
raw materials, the known processes of manipula
The lime component Is preferably freshly
tion id the requirements of use. In ceneral. slaked lime--and prepared with hot water, to
such products have been made from mixtures of increase the fineness and completeness of sub
raw materials and have presented a mixture of division, dispersion and dissolution, which re
components In their ultimate structure and com- M sults.
position.
The silica component Is ground to a degree of
It is now found that hydrous calcium silicates fineness sufficient at least to pass a 325 mesh
may be prepared of predetermined chemical screen. A finer degree of subdivision may be
composition, physical properties and other char made, as In a colloid mill, thereby to reduce the acteristics. including freedom from unreacted 50 effective period of time required for its dsolu
component* or by-products, or other Impurities. tion and reaction. The lime may also be sim In particular. I have now found that a new ilarly ground to advantage--but this appears to
hydrous calcium silicate, which I have called be leaa necessary, especially when prepared as
Leplsll. may be synthesised from Its compo- above described, on account of Its greater and
rent*--lime, silica and water--as a substantially more rapid solubility la water.
;ure chemical compound of unique characteristic properties.
Quartz
In genera). I have found that preferably pure
In carrying out the synthesis of Leplsil with
lima and lilic* may be caused to react with each quartz, the finely divided lime (99.7% CaO) ob
other and with water. In aqueous medium dl- 30 tained by Igniting pure CaCOi at 1150-1200' C..
rectry to form a hydrous calcium silicate of the for 2 to 4 hours--and finely divided quartz
desired composition, and that this reaction may (99.1% SlOi) may be mixed dry and the mixture
be controlled and carried substantially to com pletion.
dispersed In the required volume of water: or the lime may be first slaked or hydrated and dis
One condition of effecting the desired reaction -** persed in water and added to a separately pre
Is that the lime and silica shall be in finely di pared aqueoui dispersion of the quartz.
vided reactive condition--the silica especially
Tha proportion* used will be accurately
being of a particle size sufficient to pass through weighed out In amounts as indicated by the mo
325 meah screen--L e,, 44 microns In diameter lecular ratios of the equation:
or Oner.
40 <C>0 + JSIOt + SHiO + q. -<C0 JSlOi.JHiO + >q.
Another condition of the reaction la that It
aoo i.oos too*
'hall be effected In an aqueous dispersion of ihe reactive solids, such that free reaction there-
The water component is sufficient to present a water/solIds ratio of at least 7:1 by volume--
bet"**a (and between Intermediate reaction Products) shall be provided and maintained
throughout the required period of the reaction.
Sueh-dlsperalon. for example, should be sufficient jo provide a space between the dispersed par ticles. which la at least equal to the avenge of
their diameters In each direction--or a water
**
or about 3/1 by weight, taking the specific grav ity of lime at 3.4 and of quartz as 2 2-2.66--but
preferably a degree of dispersion several times
greater--for example about 26/1 by volume or
9/1 by weight, or higher, is employed. The dispersion of the solids may be main
tained by agitation or by the addition of a small
jo-solld ratio of about 7:1 by volume, or greater. amount of Inert finely divided fibrous material,
If the particle* are separated by twice their aver such as paper pulp which Is subject to subsequent
age-diameter--as by a water to solids ratio of removal in various ways, as by ignition.
J6/i by-volume (or about 8/1 by weight)--such
The charge, preferably in dispersion and while
d*rree of dispersion Is desinble.
still hot, as above prepared, is then subjected to
im
1,888,BM
an elevated temperature--above the boiling ratios, ultimately to completion at a point corre
point of water (129* C.-200* C.)--and to an In sponding to the proportions of reactive lime acd
creased pressure, accordingly. to prevent ebulli reactive silica present.
tion--as in an autoclave. The container for the
Upon disappearance of solid lime therefore, by
liquid dispersion may be uncovered In the auto- I solution and reaction, the resulting hydrous
clave, or closed as desired. Accordingly, the dis calcium silicates--Phase a. especially, but tbo
persion may be spontaneously preserved, even Phase B and Phase C--if present--undergo fur
though quiescent, as above pointed out, or may ther reaction. Such reaction 1* effective to con be maintained by mechanical agitation or by tinue the general dissolving and reaction effect revolving the container or the autoclave Itself. 10 with respect to the residual silica--whether the The atmosphere of the autoclave la preferably latter Is dissolved or is still present as residual
provided with a slight excess of water and main quarts particles--resulting in a series of inter
tained with a saturated or slightly supersatu mediate reaction compounds, which may be repre-
rated atmosphere--thereby to assure a main aented as follows:
tained or expanding dispersion and avoid a con- II
tractlng degree of dlsperson or segregation. A preferred autoclaving treatment Is effected
by beating up to 125* C. over a period of 1 to 2
VC0 193I0ijR|0
MMt|
hours and then maintaining this temperature tor
a period of S to 8 hours--or overnight for 18 hours, to
C*(0SM-SI04-HK)
fbaw a+C4(0Clt..\fwBi`JOf"r*TAS1O'6C*.1a1* am m
Ii..Sa&DCCaOo.1..i0.Si<OOfu^kn!i,OOwHi.Oa*.bo>-ajitOO*
4C*0.i5i0i
uUUAUltf
ptau rmctio* Upuii>
At tha end of the heating period, the autoclave
Silicic acid
t* cooled to room temperature over a convenient
period--e. g.. of 1 hour or less In the overnight
In carrying out the process of the invention.
runs, or 8 to 10 hours in the shorter runs--and with silicic acid, as the silica component, tbe
then opened to the atmosphere.
ti reaeui. \ end reaction mixture a:: prepared in
The product may then be dried either at 150* substantially the same way, and an equivalent .
C in a properly ventilated oven or by washing decree of dispersion in water Is effected.
it repeatedly in acetone, followed by ether and
The charge of dispersed finely divided reactive
finally drying for an hour at 100* C.
lime and finely divided reactive sillcie acid is sub--
In such procedure. It Is found that the lime * Jected to heating. In an suloelavo or the like. is
first goes into solution, as would be expected, and heating up to 175* C. It la found that la 1 or 3
that It acta and reacts upon the dispersed quarts-- hours, a preliminary reaction is effected which is
first to produce, with the thus dissolved quarts--a somewhat different from that with quartz as t&e-
solubility product probably In tha form of silica tilica component.
chains, each associated with a molecule of lime u The effective lime: silica ratio or free lime po
which serves as an instigator and preserver of tentiality of such a reaction mixture does cot .
Its dissolution. Such silica chains react, in solu appear to be so great as with quartz particles.
tion. with more lime to produce a gelatinous phase This Is due to the hydrated condition of the silicic-
as a precipitate, which I have denominated Phase acid. which..pre. s,ents a greater (solid) surface area. -
A and which has a definite chemical composition 40 one which is more reactive, both to absorb or
represented by the formula:
to adsorb and to combine with the solid and-dis solved lime, more rapidly and in greater propor
2-OCiO.l.OSiCh-iHjO. (tml or more)
tion. Such proportion is probably not limited to
The formation of this preliminary reaction product and its continued presence in the reaction
valence as in the silica chains or in the Phase A.,
compound which is formed in dispersions of lime
and quartz.
- -. r
mixture are predicated upon the provision of an
Thus, after 1 hour's heating up of the mixture-.-
excess of lime over silica. 8uch critical excess It is found to consist of a mixture of a compound
may be and probably Is the dissolved lime--rela having the composition 1.25CaO: I.OSIOvJSjO:.'
tive to the dissolved silica. It apparently re quires the presence of free solid lime--though, of
80
some unreacted silica, and a lime-silica gel. Tht: reaction mixture is characterized by being with- -
course, as long aa there is free solid lime, this out any free solid lime.
assures a saturated solution of lime. As mon as
This lime-silica gel composition, upon being
aO of the solid lime la dissolved as such, though subjected to thermal analysis, n anifests an exo
reaction continues, the concentration of the satu rated solution of free lime will fall.
88
thermic reaction which may occur between 400* and 750* C. It is not sharp at a given tempera
Likewise, under such conditions, two other hy ture but gradual over a considerable temperature
drous dlcalclum silicates have been observed-- range.
though in minor amounts--and been separated.
Continued autoclaving at this temperature
I have deslcnated these compounds as Phase B ,, (175* C.) for 1 or 2 hours, effects the transfor
and Phase C--which have compositions as lndl- mation of most of the original reactants, by re
eated by the formulae:
action of tha lime-silica compounds with the
Phase B.--2CaO.SIOv.KiO. fibrous crystals.
residual silicic add and with one another, to
Phase C.--2CiO.SIOi.l.2HiO. pltty crystals.
the composition 1.0 CaO.l.O-SiOiJnfcO. Alter
The Phase A compound, upon being subject to about about 5 to 7 hours such transformation
thermal analysis, manifests an endothermic re (with reference to the lime component) is sub
action whteh is gradual and takes place between stantially complete. But this Intermedlite com
400* C. and 600* C.. with a maximum at about pound is still associated with residual silicic add
530* C. Phase B exhibits a sharp endothermic In the reaction mixture--and reaction takes
reaction at 570* C. and Phase C exhibits a sharp place between them, though more slowly, so thst
endothermic reaction at 480* C. Phase A erm- in about 24 hours, the transformation w
pound Is also characterized by Its capacity to re Lepisil 4Ca0.5Si0'.5HK> is about SOT. to 75^
act further with silica chains or residual particles complete--and after 4 days, little If any of the
of silica Itself to form lime-silica compounds or original reactants, or Intermediate by-products
uprMeathydrous calcium silicates of lower CaO:S!Oi it
42 014 1077
2,66ft,BOA
56
However. It I* sometimes found that therw tween the reactions end results obtained wlLfr.
mar be a small amount of silicic tad. gyrolite or quartz and silicic aod. per se.
Xonotllte (till pretest. This Is attributable to
While, as indicated above. Leplsil is farmed,
the slower action and subsequent retardlnt ef- most rapidly at ITS* C.. it may be diverted by
feet of the silicic add which tends to stabilize j conducting the reaction very much above 175*
the Intermediate product ICaO: ISIOj-XHtO. C. Thus, it may also be formed at 200* C. more
By Increasing the time content of the ordinal rapidly but with Increased dancers of partial
raw mixture of line and silica by only .25%--or formations of gyrolite or Xonotllte. On the
from a CaOtSIOj ratio of .80:1.00 to .12 to 1.00-- other hand, at lower temperatures, the speed of
the transformation of the charte to Lepisll is jq reaction is slower--being reduced by approxt-
substantially completed.
.'lately one-half at 12* C.. and requiring 15 to
The transformation reactions of lime, silted 70 hours for a comparable degree ofcomple-
acid and water to Lepisll may be represented as tion--and at 125* C --2 to 4 weeks,
follows:
Tha product Is characteristically formed, by
C*O-.flO,H.O+0,O --
*IO-THrO +SIO, HtO
-w-iart-f.i"*sioBrO............................. i iseo sio, XHtO+sio. HiO. uac*o sio, xrr,o*Jio. 'ro....................... tooc>o i on Ot..\riO*siOi.BiO. ILaDCaO.l.OOSiOi.tEKil+SIOiJfl^).............CaO.tfi0i.jai0.+Hi0
+ Uv*t C*0 SSIOviSItO
Lepiril 4CaO SSlOs.5HiO
20 the described procedure. In finely divided form,
As-obtained by either procedure, whether from quartz or silicic add or other Intermediate form of silica--from anhydrous to hydrous--tha com
position of Lepisll Is chemically and physically the same. Upon thermal analysis. It exhibits s small but prolonged endothermic reaction or "break** In the heating curve, at 260*-: 10* C.
But it Is to be observed that this constitutes the only break--upon subletting Lepisll to ther mal analysis--from tha rise of temperature Im posed. whether at lower or higher ranges of tem
perature. This Is a very significant and char acteristic property, therefore, of this compound and is unique In Identifying It or Its presence.
Upon X-ray analysis, it manifests the follow
ing unique and characteristic pattern:
ti io U
as crystals of very thin flaky characteristics, and a surface area, aa determined by the gaa adsorption method, of about 50 square meters per gram.
Lepisll is therefore a new hydrous ealdum silicate of deflrute chemical composition-- 4Ca0.5510r.3H:0--of a thin flaky, crystalline
habit, finely divided and presenting a high specific surface area, substantially free from 1mPurities whether of the Initial reactants from which It Is made or of Intermediate by-products of the reaction. It manifests a novel and unique
X-ray pattern, with new lines therein, not
shown by any other of the known hydrous lime. silicates. It Is stable, at ordinary and normally
elevated temperatures, and exhibits an endo thermic, specific reaction at 260*--10* C.--upon
InutiKy
*mL
thermal analysis. Upon re-heating the same simple again, however, to this temperature--
v ................... ........ ................................
w ...
w....................................................................
V|#w,,................................................................
1.
.......
. ..
so this thermo reaction Is not repeated.
1L 3 14
The product Is. therefore, useful wherever a
m crystalline solid of definite composition Is re
Iff quired. or one which has a high specific surface
in m
area. Identifiable temperature characteristics and X-ray psttenv--freedom from free alkalies, free
V........
....... ............. ....................
ir _...................................._..................... .
r. .... ........................ .............................
141 43 silica, water, or other associated materials--and
19 tts 19
dependable as a bads of reference with respect to Ume-slllea-witer syntheses, generally--their
\.n LSI
degree of progress or completion.
].Ma4 While the procedures above described are In
L*l> 1t..41S9
w
terms of the Urn*
an Initial and silica
reaction mixture containing components In substantially
139 the molecular proportions required to produce
the ultimate product. Lepisll -- by continuous
VS-Vrrynrann M-M-dtu:
l-IVwc VW-vy treatment of the same. It la to be understood
It mar be pointed out that: with quartz az tha source of tha silica component, tha reaction la apparently progressive dissolution of silica into a concentrated alkaline medium and formation of-a high CaO/SiOa ratio compound which forms
a 2CaO.S!OiXHiO gelatinous precipitate, Phase A--which Is. In turn, subject to a subsequent se quence of reactions with tha residual quartz, to equilibrium or completion--with silicic add as the source of silica the reaction mixture first tends to form an Initial gelatinous precipitate,
a portion of which quickly absorbs all of the lime from solution, and this gel then reacts with
the residual silicic add gel and solution (with
43 40 *
that the procedure may be effective stepwise. That Is. the lime tnd silica components may bereacted In appropriate proportions substantially completely to produce, for example, the composltlon of Phase A (with cr without Phase B or C> or othT predetermined Intermediate when using quartz as the silica component, or to produce the
"TJme-slllca gel" or other predetermined inter mediate, when using silicic acid as the silica eompoaent--and thereafter. In a second stage, the Intermediate may be reacted with additional pro portions of silica component end under appropri
ate conditions to effect the required molecular
ratio cf iCaOASlOs. Io form Lepisll
characteristic properties and chemical physical 70 reactions accordingly)--hut much more slowly In reaching an equilibrium or in going to com
4CaO.3StOi.5HsO For example, somewhat different source* of the
pletion. Compounds of intermediate composi lime and silica components may be employed.
tion, degree or hydration and other properties, Instead of or supplemental to free lime and free
or mixtures of them win vary accordingly be- 78 silica, as above-described. The lime and silica
42 014 1075
2,esa,M
78
mar be already combined, but the resulting com* structure are of continuous, homogeneous com
pound must be reactive. la aqueous medium, with position. Conversely, such bodies are free froc
other components of the reaction mixture and the necessity or presence of sny other boodmi
In suitable proportions to form Leplsll Thu*, medium or material. They sre also substantial!-,
hlch Uma silicates, such as beta-2CaO.SiOi. 5 free from unreacted reagent materials or by
gamma 2CaO-SiOi or ICaO-SlOi. In suitably finely products--for all of the reagent materials art
divided condition and la the presence of suffi reacted Into the formation of Leplsll and no by
cient water, are susceptible to reaction with silica products are formed or reagent materials left tc
la the form of quarts or silicic acid, or the like-- If the reaction mixture presents a CaOrSIOi mo
10
constitute a component of the finished product. in making a shaped Integrated product com
lecular ratio of 0J:1.0. Accordingly, certain ap prising a porous body structure, which body con
propriately prepared blast furnace sloes (which may consist In large part of beta 2CaO.SiOi)
sists essentially of pure synthesized crystals hav ing the formula 4CaO.SSlOi.SHjO. or a combi
may be found suitable for the synthesis of Leplsll. nation of said crystals and other known crystals to constitute at least a major phase of the re 15 (which may have been added for dispersion and
sulting product.
suspension of the solids or like purposes, but
It should be understood that the present dis closure Is for the purpose of illustration only and
which are not reactive per se and do not inter fere with the reaction of the reactive lime, sili
that this invention Includes all modifications and ca and water components, such as the fiber com-
equivalents which fall within the scope of the 20 ponent of asbestos crystals, cellulose fibers or thi
appended claims.
like), the previously described process (without
The foregoing constitutes the specification of agitation) can be carried out. The crystals of
my application Serial No. 12,692. filed March 2. the compound thus fot'aed may be and are con
1946, now abandoned, of which this application tinuously Integrated with each other without say
Is a continuation-in-part.
25 other booding medium to thereby form a three-
Supplementary to my sold disclosure. It Is fur dimensional network interspersed with voids and
ther found that Leplsll crystals, as therein syn may have the aggregate volume of voids less than
thesized. may be simultaneously caused to Inte or greatly In excess of that of the crystals. How
grate to a unified body structure, if it Is so de ever, it will be necessary to regulate and eon-
sired. That Is the crystals may be caused to grow *0 trol the basic Ingredients, the water to solids
together to form an Integrated porous product of continuous solid formation, the density of
which is controllable: by the dispersion of finely
ratios and other relationships between the com ponents of the mixture such as a maintained and uniform dispersion and suspension of the react
divided fibers (such is of asbestos or cellulose ants (as by the use of highly spiculated asbestos
fibers) in uniform distribution throughout the i < or cellulose fibers or other means known to the mixture (thereby to effect a substantially static art), during the reaction and integration, ss dispersion and suspension of the solids); by well as the time, the pressures and/or tempera
avoiding agitation of the mixed charge during tures utilized.
the integrating portion of the reaction; and/or
There are several factors that govern In the
further, by regulating the water to solid mix 40 preparation of 4CaO.5SIOi.5HiO. for example:
tures--that Is to say. restricting the volume of
(X) Composition.--The CaO/SlOi ratio of the-
the mixture within which the reaction la caused raw mix must be approximately 0.8 CaO:l.OSlO>.
to take place to on overall volume which the
(2) Form of silica and time.--Finely ground
synthesized reaction product Is competent to oc quartz must be used In order to produce the
cupy In continuous Integrated formation sad of Leplsll hi a pure form or condition, end should
the required strength--which will, ordinarily, be ** be used If the desired product Is to be obtained
downwardly from a water to talida ratio of ap In practicable time. The use of silicic sold
proximately 26:1 by volume or 9:1 by weight. greatly retards the final formation of the de
Such conditions and procedures permit the reac sired product, although the initial rate only of
tion to proceed and the synthetic product to grow the reaction is markedly more rapid with the
by accretion and ultimate contact and union of silicic add. By analogy the dlatomltles may be
tig crystals, so as to constitute a continuous syn assumed to behave similarly os the silicic sold.
thetic integrated crystalline structure of the sub
In addition. It is pointed out that the lime and
stantially purs Leplsll compound, without other silica components may In part be already in
bonding stent, while maintaining such static u combination with each other and yet be capable-
dispersion throughout the volume of the mixture end throughout the time of the Integrating re action of the reactant components of the charge
until substantially complete reaction thereof bos been effected throughout the entire volume of the reactive mesa.
Shaped end Integrated Leplsll or Leplsfi-bonded
to
of entering Into the reaction to produce Lepisll. For example, finely divided Portland cement, typically containing time and silica In combina tion and In a ratio of about 2.5 CaO:10 SlOi. may serve as a source of reactive lime and re active silica, to the emount and In the ratio of
Leplsll products generally may be utltlzed u in sulating and structural materials and particu
Its specific lime and silica contents. In fact, such association of lime and silica, as
larly where volume stability Is desirable at high it appears In Portland cement, seems to render temperatures, i. e., temperatures In excess of 600* * both components especially reactive, and partic
P. However, they may also be used In the lower ularly so when very finely ground.
temperature fields and for other purposes where
Moreover, It Is further found that all of the
the Inert, porous, and like properties of Leplsll reactive lime component of the reaction mixture
sre desired or required.
may be Introduced In the form of finely divided
A novel and characteristic feature of such 0 Portland cement and that other high lime: sili<*
structures of Integrated synthetic Leplsll Is that ratio compounds, In which the lime and silica
not only the crystals of Leplsll but the planes components are similarly suitably reactive with
-- --qf -ontact and union at and through reactive quartz or silicic acid In an aqueous me-
~~ 42 'oiTToTiT'
(3) Temperalvre.--Under optimum conditions, dispersion and suspension of the finely divided
tha temperature of 173* C. la sufficiently high for reactant solids and reaction products thereof in
completion of the reaction In about I hours. In* aqueous media such as rater or aqueous solutions.
creasing the temperature accelerates the reaction
The charge as thus prepared la shaped and
but some uncertainty may exist as to the purity ) mmntainrd In uniform ouirscent or static dis
of the product. It Is preferable that the temper* persion and while still hot at above prepared is
ature not exceed 200* C. and that the desirable then subjected to an elevated temperature--above
range Is downwardly therefrom to approximate the boiling point of rater 1133' C.. 34 p. s. 1. gauge
ly 125* C.
or (9 p. a. i. abs.-200* C.. 211 p. a. i. gauge or
(4) Time o/ induration,--Increasing tha tem 10 223 p. s. I. abs.i--and to an Increased pressure,
perature has the effect of accelerating tha rate accordingly, to prevent ebullition--as in an auto
of the reactions. The relation between these two clave The container for the liquid dispersion
factors may be predetermined, and aueb is the ma7 be uncovered in tha autoclave, or dosed as
case but only if certain of the other factora re desired.
main unaltered. For example, raisin: the tem 13 The atmosphere of the autoclave Is preferably
perature of a quartz mixture to a relatively high provided with a slight exeaaa of water and main-
level (e. g. above 200* C.) does not appear to tamed with a saturated or slightly supersaturated
hare the desired effect of converting the lime atmosphere--thereby substantially avoiding a Iosj
and quartz completely to 4CaOSSIO:.SJfcO--In of water and the resultant shrinkage of the
stead. the formation of some other crystalline 20 charge.
compound Is favored, such as SCaO.5SiOs.JIiO.
A preferred autoclaving treatment Is effected
(5) Proper suspension and mixing.--This fac by heating the shaped or molded charge quickly
tor comes Into plsy st sll densities. It 1a ob and throughout, to the desired reaction tempera
served that the rates of reaction are decreased ture--for example. 173* C. at which it Is held over
st densities of about 30-40 pcf. in the prepara .`5 a period of d to g hour*--or overnight for 18
tion of 4Ca0.5SI0.5H:O. A water to solids ratio hours. At the end of the recctlon period, the
of 3:1 by a-elght is preferable so far as speed of autoclave Is cooled to room temperature over a
reaction la concerned as lower ratio* lead to re convenient period, e. g_ of 1 hour or less tn the
tardation of the speed of reaction.
overnight runs, or 8 to 10 hours in the shorter
In a consideration of the factora discussed. It .-in runs--and then opened to the atmosphere.
'follows that If one is changed (except thcrmtlo
The range of temperature and time for indurat
' of effective reactive lime to effective reactive sill- ing these produets of various densities should
-c* CaO/SlOs for the given product. Leplsll. which preferably be temperatures from ISO* C. to sbout
in terms of Its formation has to be fairly rigidly 2C0* C. and time Intervals ranging and depending
'fixed) another usually has to be altered In order 35 inversely upon the temperature being utilized.
'that the reaction proceeds to the desired state
The Integrated porous product may be dried
and/or composition.
at temperatures In tha rang* from 300*-33o* 7.,
Da carrying out the synthesis of Leplsll In depending upon the density of the product.
-porous structural form with quarm. the finely Owing to the high porosity and strength of the
divided lime and finely divided quartz may be product, by integration of the reaction product.
mixed dry and the mixture dispersed In the re Leplsll. it Is found that as such reactions and tha
quired volume of water; or the lime may be first Integration of the mixture progress--from the
slaked or hydrated and dispersed In water and outside of the mass Inwardly--as soon aa the
added to a separately prepared aqueous disper outer portions attain a aelf-sustainlng consist-
sion of the quartz. The slurry of lime, as pre u eacy. vaporization and evaporation of the water
pared. may be at elevated temperature--or both component therefrom may be permitted and pro
the lime slurry and dispersion of quartz may be moted so long as they do not proceed too rapidly
at substantially elevated temperature. The re nor ahead of or beyond the development of such
sulting mixture, as thus freshly prepared and at high temperature, is then brought to the shape
M
conditions--according to the principles of slraultaneoua Induration and drying of lime-siltca-
and dimensions desired In the finished Integrated .productto be made therefrom.
The proportions used will be accordingly
weighed out In the amounts as indicated by the molecular ratios of the equation:
**
water reaction mixtures as set forth tn V. 8. patent to Nto 8. Serials 2,524.303.
Thus. It will be apparent that by proper control
of the molecular ratio of the lime-silica componente at .1. the conversion.temperature and the
<jCetO
IuSrInOt
+
1S>0 ijos
+
e.-sCaO-SSiOUHfO-t'
.
time intervale of the conversion, that a porous
integrated structure may be produced, the body of
The water component of the lime-silica mixture which may be composed of an integrated struc-
-will usually range from approximately 9/1 by 10 lure of Leplsll without other or residual unre
-weight, downwardly depending upon the density acted Taw materials or reagents or by-products.
-desired in the end product. The dispersion of the nllds may be effected
'-by agitation and also by the addition of Inert finely divided fibrous material. For example, as
bestos fibers which are separated longitudinally -to a sufficient degree--such that the Individual
<8
In the adaptation of the invention to the pro duction of shaped and Integrated Leplsil prod ucts. such as molded heat Insulation. It is found that the compositions employed In terms of CsO and SlOi may advantageously be from 0.800 to
fibrous filaments resulting present cross-sectional 0.823 mol of CaO to 1 mol SiOa. the final results
dimensions of the order of ^ to 1 microns, tn being about the same through this range.
either width or breadth, and which tn length may
For example, the amounts of raw ingredients--
be of different orders--but characteristically 70 Industrial quicklime (containing 94 per cent CsO)
fibrous by being of appreciably greater length quartz flour with sbout 90 to 98 per cent p***1"*
than thickness--and. also cellulose fiber* of simi the No. 325 screen and containing 99.8 per cent
lar characteristic or dimensions, are especially -SlOi or lime and silica In the form of Portland
effective ln.provldlng aad.malntslrUng the static 74 cement and different gta^e^ an^
ol *^- ^
Alter integ.a..,a c( t.-.e c.'.arje Mas aeec
density of 20 pounds Ptr cubic loot:
fected to a degree sufficient to effect a *eii
sustaining consistency throughout the volume c
fl.sc*oaiOi CSClO/SIOi
the charge, the water component may be cause
8 or permitted to evaporate and such evcpora
WVACQQf3uafji1UiiacUm0r3rkfr/1.olaS1la.%tpoiM,oUpiiaped.,eooJ#pdotios0adRusdaae.A.dd.n..a..J.d.._.*(...C,......p_...o0..._..u>...o_....d.._..s..._.....-
U:itr*lun4ol
L11MTT111OO433I
10
tlon may be conducted rapidly and to sub stantlally any degree of residual moisture qe aired--or to complete dryness. If required. Sue evaporation may commence before chemical re action between the reactive components of th
charge is complete aueh as set forth In Sertni:
When a part ol the lime and/or alUea com 17. S. Patent 2.334.303 above mentioned--or com
ponents. which are to be used as raw materials, plete chemical and physical reaction may b-
are already in combination with each other, as In completed and then followed by drying.
Portland cement, lor example, the amounts to be 15 Prom the preceding It will be apparent that th.
used will be apportioned In terms of such com specific compound. Leplsll, 4Ca0.5S10s.3Hj0 ma;
bination and ol the reactive lime and reactive be synthesized in discrete particle form or In pun
silica contained therein. Thus tor example 100 crystalline porous structural form, thereby u
parts ol Portland cement may be used with 62 provide Insulation material for use In connec parts ol quartz to provide a reactive CaO.-SlOi 20 tion with temperatures in excess of 600* F. or ratio ol .80:1.0 or with 60 parts ol quartz to pro below same.
vide a reactive CaOrSlOi ratio ol .823:1.0.
However, of course It will be considered ant
The quicklime Is hydrated in four times Its is contemplated that circumstances alter case: weight of hot water (about 130* to 170* P.) using and that necessity or convenience may suggest a mixer tor agitation. The remainder of the 28 or dictate variations from the preferred pro water, being In the torm ol a 5 to 10 per cent cedures, compositions and resulting products tc slurry with the asbestos. Is then added, which Is be obtained as above described. Pure quartz
followed by the addition ol the quartz flour. Alter while obtainable, may be used for ancillary rea all ol the Ingredients have been added, the mix sons. such as economy of cost. Less pure, tbough ture is agitated tor an addtlonal live minutes. 30 virgin raw materials may be preferred--or in
The resulting slurry Is then poured Into pans, termediate products or by-products as above de
ot the desired size and shape, and autoclaved at scribed may be chosen--and the resulting chemi
a steam pressure (gauge) ot 123 pounds per cal and physical reactions of the process may
square Inch (178.3* C.) tor 8 hours, or at 220 and will be modified accordingly. In such event,
pounds per square Inch (201J* C.) tor 5 hours. 33 the products thereby obtained may contain con
The asbestos fiber, as prepared for use. Is sequent Impurities from the raw materials, inter
treated as a 5 to 10 per cent water suspenson mediate or by-products used--or may presfr.:
In a hydrapulper, to separate and splculate the variations due to the modification of the reac
same to finely divided forms. In respect ot the tion or a less complete reaction to Leplsll and
Individual discrete fibers. By "splculate" Is to conversion to crystal formation or Integrated
meant the separation of the asbestos fibers, or solid bodies. Such products may not be, for ex
reduction of size of the cellulose or other fibers ample, completely free from other and different
used, to a very fine diameter of the order of .1 to substances than pure Leplsll crystals or aggre
3.0 microns, without destroying the character gates. But such variations In materials, pro
istic of the individual fiber being at least several cedures and reactions, and In the product ob
times as long as Its cross-sectional dimensions. tained, are to a considerable degree In the do
Both the degree of splcualtian and the amounts main of optional variation, at the will of the
used axe dependent on a number of factors. The individual operator and to such extent as such
splculated asbestos Is especially effective tor sus variations lead to an equivalent function and/or
pending the solids--while the addition of asbestos result are to be construed as nonetheless em In all forms Imparts hinging strength and pre M bodying applicant's Invention In respect ot the
vents cracking during drying.
main disclosures and recommendations ot raw
To make an Integrated LeplsQ product of tower materials, process steps, reactions and product
density, as for example 10 pounds per cubic foot, or products formed, as herein set forth, disclosed
the above procedure may be followed except that and claimed. the asbestos used would be splculated to a high 65 Likewise, while splculated fibers, as of asbestos
degree of separation of the fibers. Also, a rela tively high percentage, up to 20 per cent of long
and cellulose, described and defined above, are predominantly effective and recommended for
fiber asbestos might be found necessary or ad purposes of dispersion of the finely divided solid
vantageous to afford the desired hinging effect reactants of the charge--whether discrete crys
and strength. The ratio of water to solids used <0 tals of Leplsll or Integrated bodies ot the reac
In the mixture would also be Increased to 6.0 to tion mixture or charge are desired to be pro
8.2 parts of water by weight, to each part by duced--It Is to be understood that ordinary as
weight of solids, for finished products of such lower apparent density--e. g. 10 pounds per cubic
foot. For integrated products of lower apparent
densities, reaction mixtures of the reactive Ume.
reactive siUca and Inert splculated fiber and/or
bestos fibers and cellulose fibers may be added tor their usual and eustomary purpose func
tion of lending strength and toughness, and the o-called "hinging effect" when incipient cracks occur. In solidified products, to prevent develop
ordinary fibers added for their hinging effect, ing or complete rupture of the mass In which
etc., may be prepared of higher water/solids ra they are embedded.
tios. by weight or volume, to such degTee as the
The foregoing constitutes the specification of
resulting attenuated forms of the synthesized my application Serial No. 277,298. filed March
Leplsll crystals are capable of entering Into a 18. 1952, now abandoned, of which this appli
unified structure of the desired continuous uni cation is a contlnuation-ln-part.
formity and strength.
76 It has also been found, as disclosed In my Is*
42 014 1081
13 14
-<uad "United States Patent No. 2441.127. that Phase A. 2CaO.SIOj.nHjO with respect to sub
equlmotecular proportions of reactive lime and stantially tht complete reactive Ume component
-remctlve silica, dispersed la water and subjected of the mixture, and to cause the resulting high
Co reaction conditions of elevated temperature CaO:SiOj ratio Ume silicates to react progres
end pressure (17J.3* to 201" C. and above) win S sively tnd successively with the reactive silica
react substantially quantitatively to produce, component of the mixture and with each other, to
synthetically, crystalline Xonotllte. havlnr the effect the formation of Lepisil. 4CaO.ISiOi.3HjO
molecular composition 5CaO.JSIOj.HiO. These and Xonotllte, SCaO.SSlOaHjC.
-crystals are of a lath-like habit of rrowth and
Such reaction results in an integrated. Inti
are capable of Intergrowth In the form of shaped -n mate and uniform mixture of the dispersion of
and integrated masses, in a wide rmne of sppar- pistelike crystals of Lepisil as formed and the
ent densities, which depend Inter alia upon the formed long, thta lathlike crystals of Xonotllte
concentration or water/sollds ratios, by volume, forming a characteristic open, porous, crystal-
of the reactive Ume and reactive silica compo.nents In the original and reacted reaction mix*
Une structure which Is strong, resilient, refrac tory to high temperatures and of low heat con
. lures.
ductivity throughout the soUd. Integrated mass
.As disclosed in applicant's eopendlng appUca* tlons and patent abovt mentioned--the proce dure of providing and preparing a reaction mix-
as a whole. These novel properties and charac teristics ire due partly to the physical properties
and relationships of the crystals, their dispersed
sure of finely divided reactive lime, finely divided 29 intergrovth. and also their individual respective
.reactive silica and water (in which the water chemical compositions, and unique thermal char-
-component Is saturated with the dissolved lime acterisucs end heat conductivities. Lepisil, being
at the outset and so maintained) and subjecting highly hydrated presents a high thermal eapao-
-to reaction conditions of temperature and pres ity and resistance to the reception and transmis
sure. effects the reaction between the lime, silica 13 sion of heat. Xonotllte, being of low hydration
.and water components uniformly and eom- la resistant to very high temperatures, strong
-pietely, -with stoichiometric conversion to Lepisil and relatively Inert both chemically and physi
1Cs0.5S10i.5Hj0 (If the reactive CaOrSIOi ratio cally. Both are formed in fine grained crystil-
provided la 4:5) or to Xonotllte, 5CaO.58iOs.lHjO Une structure. Interspersed by finely divided, dis
Of-the reactive CaOrSiOs ratio provided is 5:5) 39 persing tnd dispersed voids.
substantially exclusive of residual lime or silica
Advantage can be taken of the procedure dis
-or reaction by-products.
closed In U. S. Patent 2434.303 to Neo 3. Serials,
By the present invention It U d'seovered that whereby raw mixtures of the stated range of
iif a-reaction mixture of finely divided reactive Ca0:S10i ratios can be Indurated and dried la
-Ume-and finely divided reactive silica and water 33 a greatly shortened period of Ume over that re
.is provided in which the reactive CaOiStOi ratio quired for the conventional method of separate
.is between 4:5 and 5:5 (and the water eompo- autoclaving and separate drying steps In the
-nent la saturated with respect to the Ume com- process.
,-panent in solution at the beginning and so mam-
The product obtained consists exclusively of
ruined)--then substantially all of the Ume com- 40 Integrated Lepisil and Xonotllte crystals, and
ponent may be progressively and continuously consequently free from any other by-products
.dissolved and reacted with the silica component or additional bonding madia. The overall appar
-initially to form the reactive Intermediate com- ent density of the charge and of the Integrated
:pound Phase A--2CaO.S10usHjO, and through products formed thereof, will be determined by
a sequence of reactive hydrous silicate* of Ume. 43 the water/sollds ratio of the original mixture,
to the formation of Lepisil 4CiO.5SIOj.JHjO, and since a fine void structure results from the expul
^crystallization of XonotUte 5Ca04S10aJIi0.
sion of water from the highly dispersed crystal
It Is to be understood that in order to structure.
.produce these contemplated products wherein
The dispersion of the solid reactants in the
'the two compounds 4CaO.5SiOj.5HjO and 80 aqueous reaction mixture may be provided and
:5CaOJSiOj.HrO are found present therein In ln- sustained throughout the reaction and ultimate
rgrated form and In controlled predetermined integration of the charge as a whole by the addi
-quantity, the starting slurry must be one where* tion of suitable suspending agents tnd more
theznolar ratio of lime to silica Is the major eon- especially Snely divided fibrous materials, of the
trolling factor with respect to the final results 83 order of .1 to 3 microns In diameter, such as
.to be obtained In the end product and through splculated asbestos, cellulose or the like as set
the reaction of the slurry during a given period .of Ume and at a given pressure.
forth In U. 3. patent to Lewis H. D. Fraser. 2,469479 of May 10, 1949, Reissue 23429 May 9.
In accordance with tppUcanfs present inven- 1950. .lion, therefore, a reaction mixture la prepared w While the immediately foregoing description of finely divided reactive lime (Including reactive and discussion of the LeptsU-XonoUite mixtures, -compounds of Ume and silica of high CaO:S!Os reactions and resulting products la related to the rUo such as those of the type of Portland use of quartz as the siliea component It Is to be
cement) finely divided reactive slUcs, Including u understood that when using tripoll. silicic acid 'quartz, silicic acid and like hydrous mica com or other forms of silica as the starting material,
pounds and reactive compounds of Ume and siliea, similar progressive reaction will be initiated and
of the type of Portland cement, and water--In pursued by following applicant's present proce
which the water component is Initially saturated dures. In such cases, a longer period of time
with, respect to the Ume component in solution to may be required to effect completion of the reac
and In which the CaOrSiOs ratio la above*4:5 tion to Lepisil and/or to Xonotllte, due to the
and below 5:5--and the temperature la raised physical effects of the originally hydrated and
to the minimum reaction temperature of the more gelatinous condition of the reactive silica
mixture (about 175' C. and 130 p. a 1, aba; 115 component, but the ultimate product will consist
P- a 1. gauge) to form with quartz the compound 7> substantially of Lepisil and XonotUte crystals.
42 014 1082
{
j I {
a,uaa,98
15
IS
integrated with each other and without residual
2. A hydrous ealcium sUleate product in shapra
lime or allica or by-products of the reaction.
form, consisting essentially of a combination
As previously stsud herein the primary pur two continuously Integrated crystalline strue-
pose of this present Invention Is the production tures. said comaxed structures having voids m
of an end product for use as either building cr excess of the solid* and its said structures hsrr.
thermal insulation wherein at least two com the compositions 4CaO.5SiOi.5KiO and
pounds are combined in predetermined propor tions suitable for certain desired end purposes.
5C*0.SS10i-HjO
The percentage of the individual compounds present in the end product are predetermined and controlled through control of the molecular
lo
3. A reaction product, consisting essenctsCe of dispersed finely divided fibers and duperjjM
thin platy crystals, having a composition at
ratio of lime to silica In the startles slurry. Tor example. In the use of tripoll. as the form
4CaO.SSiOi.5KiO and characterized by a unique X-ray diffraction pattern having a very strooi
of silica to be used, the foUowtnt Table I Indicates line d-- 1U A. and a strong line at d--2J$ i
the procedure to be followed to produce end prod ucts in which the percental* of the compounds present therein are predetermined and controlled. This table also indicates specific examples of
and dispersed lath-llke crystals, having a compo sition of SCaO.55iOi.HjO. said crystals being in
tegrated in continuous random arrangement relative to each other.
procedures In accordance with the present Inven tion far the preparation of Intefrated Lepisll-
*ii
4. The method of forming an integrated hrdroui calcium silicate product which comprua
Xonotlite refractory insulation, the time intervals providing an aqueous mixture consisting Kien-
given therein beln those necessary in an ordi tially of reactive lime and reactive silica, wherein
nary Indurating cylinder.
the molar ratio of lime to silica is within tbs
Tabit /
a
range of from at least 4:5 to less than 5:5, ms amount of water in the mixture being within the
Produet
Pvvmtrv tpxt)
4C>*0Hr9O0.10* perm&t
BjcyOto, ipaeiroro*n.!
flUrorttvtoOf CoO/9 0*
Tint. In. Cidfl
ik.
range of about 7.0 to .75 times the aggregate weight of the solids, subjecting said mixture to a temperature and pressure la excess of nsvc. and 130 p. s. i. abs. respectively, maintaining am
slurry at a temperature and for a period of ob*
necessary to effect substantially quantitauvs re
UmrDi o
98T009 m
I0I0.lt1.*l9 1.0
r-or 0
ii
u
C82393i tl1tod9
rs a
1n9o
action between the reactive lime and silica com ponents. therety to produce an amount of at
least two crystalline structures in Integrated fora, the percentage of each structure being de
pendent upon the molar ratio of lime to silica ua
From Table I above it Is sppsrent that a* the the slurry, om crystalline structure having tba
molecular ratio increases the time for ccnvenion composition 4CaO.5SiOi.5HjO and one banc*
to a completely crystalline product at a given pressure also Increases in some proportion there
AO
the composition 5CaO.5SiOj.HjO, said structures being integrated with each other and drying aid
to. An indurating pressure of 225 p. s. L (gauge) product.
or 240 p. s. i. (aos.) and temperature of 203* C.
5. Method of making a new hydrous caldua
appears to be a commercially practical pressure economically common to all CaO/S.Os ratios but
pressures and their corresponding temperatures
beyond inis may be also utilized. The time intervals required at a riven pressure
to obtain a completely crystalline product are mmewhat shorter vhen quarts is used than when
tripoll or silicic acid is employed as the source
of silica. It should be understood that the present dis
closure Is for the purpose of illustration only and that this invention includes all modifications and equivalents which fall within the scope of the
;o u
silicate product comprising the steps of dispers ing finely divided reactive lime and finely dmdad reactive silica in the form of quartz, in tbe mo lecular proportions of approximately from 4 to 5 to less than 5 to 5. the amount of water in tbe mixture being within the range of about 7.0 to .75 times the aggregate weight of the solids, and
wherein the dispersion Is maintained by finely
divided fibers, and subjecting the said dispersion to temperatures and pressures within the range
from 150* C. and 89 p. s. L aba. to approximately 203' C. and 240 p. s. L abs. respectively for a pe
riod of time varying with respect to temperature,
appended claims.
to effect substantially quantitative reaction be
The use of the terms, "silica." "reactive silica" tween the said reactive lime and reacuvv
or "siliceous material" in this present specifica components to form in integrated Ions a
tion and/or any of the claims, contemplates the hydrous calcium silicate having the formula
inclusion of silica in any of Its known forms, to 4CaO.5SiOi.5HjO and a hydrous calcium silimM
either free, combined or chemically combined as silicates.
having the formula 5CaO.5SiOi.HjO. 6. The method of forming an integrated hy
I claim:
drous calcium silicate product which eompn**
1. An integrated porous hydrous calcium sili providing an aqueous slurry consisting essential!!
cate product, consisting essentially of two crys u of sclids in the form of reactive time, reacave
talline structures, one of said crystalline struc silica and a suspension agent for said solids w
tures having the composition 4CaO.5SiOi.3HiO, the form of highly spiculated fibers, wherein the
and the other crystalline structure having the initial molar ratio of lime to silica la at leant Oi
composition 5CaO.5SiOi.HiO being present and but less than 1.0. the amount of water in me combined with said first mentioned structure, the TO mixture being within the range of about 7.0 to
said crystalline structures being continuously in .75 times the aggregate weight of the solids.
tegrated with each other In random dispersion, jeering said sljrry to a temperature and pres*
and forming a three-dimensional network Inter In excess of 175' C. and 130 p. s. 1. abJ. resp**"
spersed with voids, the aggregate volume of the tiveiy. maintaining said slurry at a tempera--'^*
voids being in excess of that of the crystals. 7 and lor a period of time necessary to eflect sub*
42 014 1083
2,083,9M
n is
ttantiallT quantitative reaction between the re- of the solids. molding said slurr/. subjecting
active lime and silica components, thereby to said molded slurry to a minimum temperature
produce a crystalline end product containing a and pressure of about ITS' C. and 130 p. s. t. abs.
crystalline compound in internted form, the respectively, maintaining said slurry et raid tem-
percenuce of such compound present In sa:d end s perature and for a period of time consonant with
product being dependent upon the initial molar the particular nc locular ratio cf the solid; exist-
ratio of lime to silica in the slurry, the one said ing therein to effect substantially quantitative re-
eryitaUina compound having the composition action fcetceen the reactive lime and silica cotn-
4Ca0.SS10i.5Hi0 and drying said product.
ponents thereof, thereby to produce a crystalline
7. The methed according to claim 8 cherein 10 end product containing a crystalline compound
said compound baa integrated therewith, a in Integrated form, the percentage of such com-
crystalline compound having the composition pound present in said end product being depend-
5CaO.5SlOj.HiO formed upon any upward varia- rot upon the Initlil molar ratio cf lime to silica
uon of said Initial molar ratio above 0J.
in the slurry, the said crystalline compound hav-
I. A reaction product, comprising dispersed 13 ing the composition tCaC SSiOi-SHrO and drying
finely divided fibers end dispersed thin piety said product.
crystals, having a composition of
14. The method according to claim 13 cherein
4CaO.3SiOs.SHK3
said compound has integrated therewith. a crys
and presenting a surface area of at least approd- talline compound having the composition
raately SO square meters per gram, said fibers and SO crystals being In continuous random arrange
SCsO- SSIOs HKD
ment relative to each other.
formed upon any upward variation of said initial
9. A hydrous calcium silicate, having the molar ratio above 4:5.
chemical composition represented by the for
15. Method of making a new hydrous calcium
mula 4CaO 5S10r.5&0 which la further charmu- *3 silicate, comprising the steps of dispersing finely
tented by being of lamellar crystalline structure, divided reactive lime and finely divided reactive
free from extraneous water, lime and silica and silica in the form of quarts, in the molecular pro
free from other reaction products thereof.
portions of approximately 4 to 5. in water, the wa
10. Method of making a new hydrous calcium ter to solids ratio being not more than 25:1 by
silicate, con rising the steps of dispersing finely M volume under saturated conditions relative to the
divided reactive lime and finely divided reactive lime component in solution, end subjecting the
silica in the form of quartz, in the molecular said dispersion to temperatures within the range
proportions of approximately 4 to S. in water, the from 150* C- to approximately 200* C,, while
water to solids ratio being not more than 26:1 maintaining the dispersion substantially quies
by volume under saturated conditions relative to S3 cent during the reaction for a period of time
the lime component in solution, and wherein the varying with respect to temperature, to effect
dispersion Is maintained by finely divided fibers, substantially quantitative reaction between the
and subjecting the said dispersion to tempera said reactive lime and reactive silica components
tures within the range from ISO* C,, to approxi both to form a hydrous calcium silicate having
mately 200* C.. while maintaining the dispersion 40 the formula 4CaO-5SiO*-5HiO and to Integrate
substantially quiescent during the reaction for a the same.
period of time varying with respect to tempera
18. Method of making a new hydrous calcium
ture. to effect substantially quantitative reaction silicate comprising the steps of dispersing finely
between the said reactive lime and reactive silica divided reactive lime and finely divided reactive components both to form a hydrous calcium sill- 45 silica in the form of quarts, in the molecular pro
cate having the formula 4CaO.S5tOi.SHsO and to portions of approximately 4 to 5. in at least seven
Integrate the same.
times their aggregate volume of water, under sat
11. A hydrous calcium silicate, having the urated conditions relative to the lime component
chemict! composition represented by the formula tn solution, tnd subjecting the said dispersion to
4CaO-SSiOi-5HK> which is further characterized jo agitation and to temperatures within the range by being of lamellar crystalline structure. In the from 125* C.. to approximately 200* C.. for a peri
form of integrated crystals, free from extraneous od of time varying with respect to temperature,
water, lime and silica and free from other reac to effect substantially quantitative reaction be
tion products thereof.
tween the said reactive lime and reactive silica
12. The reaction product having the compeal- u components to form a hydrous calcium silicate
tlon 4Ca0-5S10>-5H>0 and free from unraacted lime, in the form of thin platy crystals presenting
having the formula tCaO-SSiOi-SHrO. GEORGE L. KAL0U5EX.
a surface area of approximately 53 squere meters per gram and characterized by a unique X-ray
Reference* Cited In the file of this patent
diffraction pattern having a very strong line at go
UNTIED STATES PATENTS
d-ll.2 A. and a strong line at d--2.95 A. and fur
ther characterised by being Integrated end by tn endothermic reaction at 260*s:10*--C.
13. The method of forming a shaped integrated
Number 2.215,891
3,449.379
hydrous calcium silicate product which comprises W
Name
Cato
Thompson et al.____ Sept. 24, 1940
Fraser........................ May 10. 1949
OTHER REFERENCES
providing an aqueous slurry consisting essentially
Flint et el.: "Formation of Hydrated Calcium
of solids in the form of reactive lime, reactive BUIcates at Elevated Temperatures and Pressures.'*
silica end water, wherein the Initial molar ratio N. B. 8. Jour, of Research, vol. 21. pages 617-83*.
of lime to silica is above 4:5 brt less then 5:5.
Flint et al.: "X-ray Patterns of Hydrated Cal
the amount of water In the mixture being not TO cium Silicates." N. B. 3. Jour, of Research, vol.
greeter than about 7.0 times the aggregate weight 31, pages 225-221.
42 014 1084