Document DMwDMmLovmdNQOaE3YLa9N2M
CSL-140A (Supersedes CSL-140)
Report from the
.
COATINGS SERVICE LABORATORY
ADHESION OF LACQUERS TO ALUMINUM FOIL
Requirements of good coatings fox aluminum foil -- adhesion, fastdry, flexibility, printability, and light stability -- can be obtained from lac quers based on nitrocellulose or ethyl cellulose.
Adhesion i6 particularly difficult to achieve on aluminum because o: the 6xnooth, dense, impervious surface of the metal; and aluminum foil usually nresentc an even more difficult problem because the oil residues which have "been baked into the surface during processing are not usually removed. Thus, coatings that have good adhesion to untreated foil are rel atively uncommon.
Good adhesion to untreated aluminum foil has been obtained in our
laboratory with lacquers and inks based on Hercules Ethyl Cellulose and
Nitrocellulose. This report presents results obtained from two programs;
the first section covers studies made with nitrocellulose lacquers and the
second reports studies with ethyl cellulose lacquers.
'
A. ADHESION OF NITROCELLULOSE LACQUERS
The Hercules Coatings Service Laboratory investigated the adhe
sion of four nitrocellulose-based formulations to two types of untreated
foil - "Reynolds Wrap" foil 6old for household use, and a heavy-duty foil
used as an overwrap on cigarette cartons. The coatings were applied with
a No. 150 hand gra.vure roller, flash-dried a few seconds, then, force-dried
2 minutes at 180 "F,
'
Nitrocellulose lacquers modified with a poly(vinyl acetate) resin were found to have strong adhesion to Reynolds Wrap. This untreated foil is particularly difficult to coat because a special oil, which causes poor adhesion of coating materials, is applied after processing to protect its surface (formulations Hi and H2 in Table I). These same lacquers, sur prisingly, had only fair adhesion to the foil used to overwrap cigarette cartons: here the processing oils were baked on the foil surface. Two other lacquers, onemodified with a polyamide and the other with Neolyn 23 resin (formulations #3 and H4 in Table 1), adhered to the overwXap foil surface more strongly than the commercial coating presently used. ^
g. ^ 9
2
Z o
...... ftx.fy'L.. A POLYMERS DEPARTMENT HERCULES POWDER COMPANY WILMINGTON, DELAWARE
WATER_PCB-'
HERCULES
Technical Data
CSL-140A Page 2 of 6
Table I
ADHESION OF LACQUERS TO ALUMINUM FOIL
Vehicle Solids
2<a)
2(a>
3 (a)
4(a)
RS* Nitrocellulose, 1/2 sec. SS* Nitrocellulose, 1/2 sec. Polyfvinyl acetate) (Gelva V-25) Polyamide (Versamid 940) Neolyn 23 resin
Dicyclohexyl phthalate Santicizer 141
- - * 50
25 20 50 -
60 40 . -
-
- - - 36
- - 36 -
1^ 40
- '14
- - 14 -
. Total
100 100 100 100
Physical Properties
Scotch Tape adhesion' ' to:
Reynolds W rap {untreated foil)
'rO*
G
-. p
Untreated foil used for cigar-
ette carton overwrap
pp GG
Shellac-treated foil
p F. -
G
Blocking, 130 F. 2 p. s. i. at 40 hr.
Face-to-face
B B NB NB
Face-to-back
NB NB NB NB
5_ t>0 e
0 U r* 0
t-L H
U
H
Hr*
w
Hr* H0 O
-
p
-
-
-
* Hercules Trademark
Legend: B = block; NB = no blocking; G = good; F = fair; P =poor.
(a) Solvent Systems: Toluene Ethyl alcohol Ethyl acetate Butyl acetate
For Formulations 1 & 2 43 17 13 27
. 100
For Formulation 3 50 20 15 15
100
For Formulation 4 - Dissolve Versamid 940 in a 50:50 mixture of toluene and ethyl alcohol. Add this solution to a nitrocelluloseplasticizer solution dissolved in solvent^),
(b) Adhesion test method - Adhesion was tested by firmlypressing Scotch Brand Acetate Film Tape No. 800 on the coating. The tape was re moved by pulling it back at an angle of 180 ". Adhesion was noted as:
Good. - no failure occurred when tape was removed abruptly"^
Fair - failure occurred when tape was abruptly removed. No failure oc
curred when tape was pulled back slowly.
Poor - failure occurred when tape was removed slowly.
Very poor - no force was required to remove coating.
MON-MT-003200
' App h?
WATER_PCB-SD0000018081
HERCULES
Technical Data
CSL-140A Page 3 of 6
*
B. ADHESION OF ETHYL CELLULOSE LACQUERS
Hercules Ethyl Cellulose N-10, modified with Aroclors 1254 and 5460 (lacquer H 1, Table II), produced a coating having excellent adhesion and flexibility on both lightweight and heavy aluminum foil. Aging of the lightweight coated foils for two months did not impair film adhesion prop erties. This formulation was at least as good as the betteT of two commer cial foil lacquers, on lightweight foil {Table IV), and superiox to both on heavy-gauge foil (Table V).
Two other experimental lacquers (#4 and #6, Table II) had good to
I excellent initial adhesion on lightweight foil, about .equivalent to the better of the two commercial coatings. On two months' aging, however, some
"loss of adhesion resulted (Table IV). On heavv-gauge foil, #6 lacquer was
I unsatisfactory, but $4 was Bomewhat better than the commercial products
(Table V).
"
Special tests involved additions of 0. 25% phosphoric acid to deter mine if adhesion could be improved by the etching action of the acid on the foil. Little if any effect was observed (Tables IV and V).
A report from the trade had previously stated that adhesion was ad versely affected by addition of certain dyes such as Calco Fast Spirit Red B. This report was not substantiated by these tests.
.The most effective modifiers for improved foil lacquers based on ethyl cellulose were:
1. Aroclors 1254 and 5460. 2. Triphenyl phosphate and Resimene 681.
'
Five experimental ethyl cellulose lacquers (#1 through #5', Table II) were tested at 1-mil film thickness for initial adhesion and flexibility on lightweight aluminum foil. The results, compared with four commercially coated foils, were used to select most promising compositions for further testing. Results are'in Table HI.
The two best lacquers (#1 and #4, Tables II and III) were coated along with a third composition (#6, Table 1) in nominal film thickness of 0, 2 mil on both lightweight and heavy-gauge aluminum foil. Results on lightweight foil axe in Table IV, and on heavy-gauge foil in Table V. See page 6 for description of test methods used as reported in tR'ese tables.
ftpp \o-
' M
MON-MT-003201
WATER_PCB-SD0000018082
I.
R l l 1 I 1 1 R
r
R *
R R
HERCULES
Technical Data
CSL- 140A Page 4 of 6
Method Of Film Ca-Bting
On lightweight foil, the coatings weie cast with a Hercules casting knife, air-dried 5 minutes, force-dried 5 minutes at 190 "F.., and airdried overnight.
The heavy-gauge foil was dip-coated, air-dried 5-10 minutes, forcedried 5 minutes at .190 F. , and air-dried overnight.
. Table II
ETHYL CELLULOSE LACQUER
COMPOSITIONS FOR ALUMINUM-!FOIL COATING
Solids
1 > n 4
Hercules Ethyl Cellulose N-10
60 60 60 50
Hercules Ethyl Cellulose N-14
-- - -
Aroclor 1254
20 - - -
Aroclor 5460
. 20 - - -
Super Beekacite No. 1001. Tricresyl phosphate Triphenyl phosphate
- 28 -
-
- Oe - -
- D/ 10 25
Staybelite Ester No. 10
- -
30 -
Santiciz.er B- 16
- - '-
-
Resimene B8I
- - - 25
Paraplex RG-Z
-- - -
100 100 100 100
Solvent
Xylene
80 80
-
80
Toluene
--
80 -
Isopropanol
20 20
-
20
Ethyl acetate
20
5 50 -
-
25 25 100
80 20
o/ 50 -
-
-
-
40 10
100
80 20 *
Table HI
ETHYL CELLULOSE FILM PROPERTIES
Commercially
Lacquer No,
Coated Foils
Adhesion - Initial
1 2 345
12 3 4
Tape test (method A)
E G GE F G G G G
Fingernail test
E EGE F G G G G
Flexibility (180 crease at 75F. )
Initial
1
E E E E E .E E E E
Nominal film thickness Aluminum foil gauge Lacquer solids, %
3 mil\ 0. 35-0, 40 mil
33
Legend: E = excellent, no effect; G - good, very slight effect; F = fair, moderate effect; P = poor, noticeable effect.
orrOnv > h?"
5
z o
WATER PCB-SD000001
HERCULES
Technical Data
t
CSL-140A Page 5 of 6
Table IV
ETHYL CELLULOSE FILM PROPERTIES ON LIGHTWEIGHT FOIL
Adhesion - Initial Tape test (method C)
Lacquer additive - none acid^ dye(k)
-------------------------------------------acidIf*-'- -i_dye^)
Adhesion - 2 Months Aging Tape test (method C)
Lacquer additive - none acidU) dyeS1o, ) acid^ -i- dye^
Lacquer Number
1 ~T_ IT
E EG E EE E EE E__________E G
Ep E PF E P o E P p
Commercial Lacquer
FG FE PE T> E
P JL PE PE PE
Flexibility- (1 BO ' creaBe at 75 F. ) Initial Aged 2 month
Nominal film thickness Aluminum foil gauge Lacquer solids, %
E EE E EE
EE E TT
0. 2 mil 0. 35-0.40 mil
14-25.5
Legend: Same as in Table III on page 4.
(a) 0. 25% phosphoric acid based on lacquer solids. (b) 2, 6% Calco Fast Spirit Red B dye based on lacquer solids.
Table V
ETHYL CELLULOSE FILM PROPERTIES ON HEAVY-WEIGHT FOIL
Adhesion - Initial
Tape test (method B except as noted)
Lacquer additive - none acid^
.
dye^c)
acid^) + dye(c)
Flexibility (180 crease at 75 F.)
Initial
`
Lacquer Number 1 46
E E p\a/ E EP E EP E PP
E EE
Commercial
XY
G P(1 a) GPP E-
EE
Nominal film thickness Aluminum foil gauge Lacquer Bolide, %
0. 2 mil 3. 5-4,5 milt
14-35.5 "
Legend: E = excellent, no effect; G = good, very slight effect; F = fair,
moderate effect; P - poor, noticeable effect.
(a) Tape te6t method C.
(\<pp
.Id
(b) 0.25% phosphoric acid based on lacquer solids. (c) 2. 6% Calco Fast Soirit Red B dve baBed on laccuex eolid6.
MCfN-MT-003203 .
WATER PCB-SD0000018084
I 0
*
I
i
i
I
I
r
i i
i
i
i
i i
i
I
HERCULES
Technical Data
CSE- 140A Page 6 of 6
ADHESION TEST METHODS
Tape Test Method A
Three inches of 1 -inch wide Scotch Tape wa6 applied and smoothed over the coated foil. After 30 to 60 seconds, it was rapidly pulled away from the surface. Adhesion was estimated by noting the amount of lacquer removed by the Scotch Tape,
Tape Test Method B
Same as -Test A, except that a 1,000-gram weight was rolled over the Tape after application.
Tape Test Method C
Same as Test A, except masking tape was U6ed in place of Scotch
Tape and a 200-gram weight was used. This method is not as severe a
test as Method B.
.
Fingernail Test
An area of the coated foil was crosshatched in approximately 1/8 to
3/16 inch squares with a razor blade. Adhesion was estimated by ease of
removal when scratched with the fingernail.
.
Af>p' s .
\
MON-MT-003204 1
WATER_PCB-SD0000018085