Document DGxKDxNkNdOg8GxNVq75n8qRO

<r. THK PKOPKK HANDUNO OP AROCl-OBS ANl) THKIK KJXTUKPS IN THK E1FCTH1CAI- 1NDUSTHX MONS CJ73S6 A, rtt jz rfoA/s A^r-. Cur*. La& ' < MCNS 077397 ( THE PROPER HANDLING OP AR0CLGR3 AND THEIR MIXTURES IN THE ELECTRICAL INDUSTRY ( P. 0. Benlgnus 12/1/54 Monsanto Chsmloal Co. Organic Dlv. Sales Dept. 800 N. Delmar Blvd. St. Louis, Mo. I HONS 077398 Introduction Chapter 1 Chapter 2 Chapter 3 Chapter *1 Chapter 5 Chapter 6 Chapter 7 Chapter 8 Chapter 9 INDEX The Proper Handling of the Aroolora and Their Mixturea in the Electrical Induatry. Procedure for Unloading Tankcers of Aroolora and Their Mixturea. A. Description of the Cars. B. Procedure for Unloading the Cara. A. oeneral Description of Storage Tanks. B. Detailed Description of Storage Tanks. Gasketing and Pump Packing. Sampling. Laboratory Analysis and Procedure for Treating Aroclors and Their Mixturea. Test Procedures. Typical Properties. Earth Treatment of Aroclors and Their Mixtures in the Electrical Industry Prior to Use. Dermatology and Toxicology. Attachmenta: Drawing No. 31-20848, Dome Detail. Drawing No. 31-20847, The Tank Car. Drawing No. 9C-8i70-5> The Horizontal Storage Tank. Drawing No. D-13362, The Vertical Storage Tank. Drawing No. 9C-8248, The Breather. Drawing No. 9C-8278, The Varec Oauge. Drawing No. 9C-8* 17"8, The Unloading Platform. MONS 077399 I THE PROPER HANDLIHQ OP AROCLORS* AND THEIR MIXTURES IN THE ELECTRICAL INDUSTRY INTRODUCTION Monsanto's Aroclors*, especially the chlorinated biphenyls Including types 121(2, 1248, 1254, and 1260, used alone or In combination with chlorinated benzenea, are commonly used die lectric materials of the Askarel^ class. Askarel Is a generic name referring to liquid dielectrics derived from hslogenated aromatic hydrocarbons possessing excellent chemical and dielectric stability and flre-reslstance over the temperature ranges and operating conditions required of transformers and capacitors In the electrical industry. The properties of Aroclors and their mixtures, used as dielectrics are described In detsll In chapter 7 entitled, "Typical Properties". These dielectrics are manufactured under very carefully controlled conditions In order to meet the strict and exacting electrical requirements and properties. The electrical Industry's use of these fluids has been largely In acoordanoe with the Oenerel Electric Company's patents and developments. AroclorB - Monsanto's chlorinated biphenyls and chlorinated polyphenyls, Registered u.S. patent office. 1F. M. Clark, "Electrical Insulation", Chem. Eng. News 25, 2977 (1947). --------------------------------- 1 RONS 0 7 ?4CC I Resulting from the wide use of these materials In the Industry, trade names have been established to Identify them by different manufacturers of electrical equipment. Listed alphabetically the trade names lnolude, "Chlorextol," Allla-r Chalmers; "Dlaclor," Sangamo Electric; "Dykanol," CornellDublller; "Elemex," Line Materials; "Hyvol," Aerovox; "Inerteen," Westlnghouse Electric; "Noflamol," Wagner Electric; and "Pyranol," General Electric Company. The purpose of this bulletin Is to assist the industry with the proper and safe handling of these dielectric materials In their operations. < 2 MCNS 077401 CHAPTER 1 PROCEDURE FOR UNLOADING TANKCARS OF AROCLORS AND AROCLOR MIXTURES A. Description of the Cars Aroclor and mixtures of Aroclors with chlorinated benzenes are Bhlpped by Monsanto In tMO types of Insulated tankcars both of which are either aluminum lined or zinc-tln metallized. One type of car has heating colls Inside of the tank and these are In direct contact with the product. The other, a more widely used type of car, la a double-shell tank with heating colls between the Inner acd outer shells. The steam coll connections are at the bottom of the oar. Both types of tankcars are tested for 60 pounds pressure and their steam colls are tested for 200 pounds gauge pressure. The cars are top-unloaded by displacement with dry air con taining 10 mg. H2O/CU. ft. maximum. There are two or three connections on the tankcar dome depending on- the type of car. Where three connections exist, one Is a two Inch diameter unloading line which extends to the bottom of the car, the second Is a one Inch diameter air Inlet connection and the third la a two Inch diameter preasure safety vent, which is a thin lead disc adjusted to release any pressure In excess of 60 pounds gauge. This safety vent Is hooded for protection against dust, dirt or accidental bumping. Where only two connections exist on the dome, one Is the two inch diameter unloading line and the other Is the safety 3 MOMS 077*02 vent. On these cars. It Is necessary to remove the safety vent and Introduce the displacement air through that connection. Drawing No. 31-20848 shows in detail the dome of a tankcar with three connections. "A" Is the two Inch unloading line which extends to a small sump at the bottom of the car. "B" is the one Inch air Inlet connection. "C" Is the hooded safety vent. The car dome cover with fitted bolts Is shown In the center. It Is fitted with a Oarlock 901 asbestos gasket or an aluminum envelope Ooetze gasket. This drawing also shows a bottom opening In the car. This can be opened only from the Inside of the car and ltB purpose Is for cleaning operations. It has no use at all In unloading the car. ( Drawing No. 31-20847 shows the over-all dimensions of the 8,000 gallon Aroclor tankoar. B. Procedure for Pnloadlng the Cars The oar should be spotted at an unloading dock similar to the one shown by Drawing No. 90-8178. The car must be level and the brakes set properly. "STOP-Tankcsr Connected" signs should be placed fore and aft the car to warn switching crews. If It Is rslnlng or snowing or the humidity Is extremely high. It Is not advisable to open the car. In case the car must be sampled and opened during bad weather, a canvas osnopy must be placed over the dome of the car. It Is preferable to unload the care under roof or Inside the factory. Unless It Is absolutely necessary because of following described situations 4 HGNS 077403 the dome cover should not be opened until ready for sampling. The dome cover Is sealed with a standard railroad wire and seal, and Monsanto should be notified If this seal Is found broken upon receipt of the car. The first step In unloading Is to Inspect the dome and clean around the dome oover to remove all loose dirt, water or snow. Wiping rags and a brush should be used to clean before the dome oover and connections are opened. Then, the screwed hood over the air-inlet valve should be removed and this valve opened fully and left open while heating the car. A Weston or metal encased thermometer should be Inserted through this alr-lnlet valve opening and the tempera ture of the Interior of the car determined. If the car temperature Is below the caution temperature shown in the following Table 1, It will be necessary to take the special step of inserting a "halr-pln" heating coll through the dome of the car to preclude rupturing the tankcar seams during the heating period. Table 1 Product Aroclor 1260 Aroclor 1254 Aroclor 1248 Aroclor 1242 Pyranol 1467 Pyranol 1470 Pyranol 1481 ASTM Pour Point *C. Temperature *C. Below which Caution Must Be Used in Heating + 30 + 10 + 4o + 20 -T +5 - 19 - 10 Pre-heating Is not required* Pre-heating Is not required* Pre-heating Is not required Except If the material has cooled below -10*C. and crystals of scavenger have separated. Then, the material should be heated to 70*C. (158*?.) until complete solution has been accomplished. 5 MOKS 077404 If the dome of the car la to be opened for the pre-heating operation. It la necessary that it be covered with a clean oanvas. Extreme care must be taken to avoid getting dirt or moleture Into the car. Due to the relatively high vlaooslty of some of the Aroclors at low temperaturea, It la neceaaary to form a column of molten material from top to bottom of the car, In the center, to pre vent hydraulic preaaure build-up which may rupture the tank ahell If there la too rapid looallzed heating when employing the main ateam colla. When pre-heating la required, a satisfactory vent hole can be made by Inserting a "halr-pln" coll (1/2 Inch diameter brass, galvanized, or stainless steel pipe) Into the open dome of the car and Introducing steam through the coll until there Is a column of fluid Aroclor from top to bottom. After the vent hole la melted through the material to the bottom of the car, the halr-pln coll should be removed and the dome cover replaced and bolted. Steam la then Introduced Into the main colla. It Is recommended that the 8team pressure be limited to 100 pounds gauge pressure, particularly In the case where the colls are In direct contact with the Aroclor. The steam coll outlet should be trapped or throttled with a valve. It will require eight to twenty hours to bring the material to pumping temperature - depending upon weather conditions. It 6 HONS 077^05 la essential that the air Inlet valve be open during the heating period In order to vent the tank. Some calculations have been made to Indicate the heat requirements for an Aroclor car. Data for an 8,000 gallon car of Aroclor 1254 are: Specific Gravity Specific Heat ; 1.5 = 0.26 BTU/lb./O p. Heat requirement for heating Aroclor from 30C. (86^.) to 110C. (230F.) 1b: 8000 x 1.5 x 8.33 x 0.26 x (230-86) : 3,774,000 BTU. For heating from 30C. (86?.) to only 75C.(167"F.), the heat required 1b 2,110,000 BTU. A nine horse power boiler operating at 80 psig produces 263 lbs./hr. of steam with no reused condensate. Returning con densate at 200*F. will increase the steam output to 296 lbs./hr. at 80 psig. In the first case, heating to 110C., the over-all heat trensfer coefficient is assumed to be too low to utilize the 100# capacity of the boiler. A value of 1500 for UA with an average 4T of 134F. indicates that the useable steam la 202,000 BTU/hr. or 226 lbB./hr. steam at 80 psig. In the second case the A T is lower and the entire out put of the boiler is useable. Table II sums up the approximate time calculated to heat Aroclor 1254. 7 HONS 077*06 ( TABLE II Wine HP Boiler 100$ oap.(no reused condensate) lbs .Steam/Tir. 263 30-110`C. -- 30-75C 9 Hr a 75$ cap. (no reused condensate) 100$ cap. (condensate 9 200"F.) -- 296 18 hra.(86$cap) 12 Hrs -- 8 Hr a 75 cap.(condensate @ 200F.) -- 18 hrs.(76$cap) 11 Hrs Calculations on a five horse power boiler give heating times of the following order: Five HP Boiler lbs .Steam/hr . 30-110" 30-75'C. 100$ cap. (no reused condensate) 146 28 hrs. 16 hrs. 100$ cap.(oondenaate 9 200F.) 164 25 hrs. 14 hrs. Aroclor oars oan be heated by ateatn (80-100 pBlg) to the proper handling temperaturea In a reasonable time by using a boiler source capable of produotlng 200,000 to 300,000 BTU/hr. The tinea given here are approximate and will act aa a guide until experience shows the exact time for this operation. 8 MCNS 077*07 The proper handling temperature for the varloua fluids la given In the following Table III, which Indicates corresponding viscosity values: TABLE III Product Handling and Pumping Temperature C. Approximate Viscosity. S.U.S. Aroclor 1260 95 - 130 100 - 43 Aroclor 125^ Aroolor 1248 Aroclor 1242 75 - 110 50 - 85 35 - 75 100 - 42 100 - 40 100 - 40 Pyranol 1481 30 - 75 100 - 40 Pyranol 1467 20 - 55* 100 - 40 Pyranol 1470 15 - 45* ' 100 - 40 If any of the scavenger la out of solution, then the material must be heated et 70C. (158* P.) until It has dissolved. Selection of pumping temperatures for any dielectric not shown on this list or which may be developed in the future should be based on a viscosity of about 100 Seybolt Universal Seconds for average pumping and about 40 S.U.S. for fast pumping. When the material has been heated to pumping temperature, a one-half Inch diameter pipe "cross" arrangement containing a pressure gauge, air Inlet, pressure relief valve to relieve at 30 PSIG, and vent connections, should be connected to the dome air Inlet pipe. Then the unloading line should be connected. 9 HONS 0J7408 (At this point a sample Is taken as described In Chapter 4,) Dry* air Is then Introduced Into the tankcar and pressure built up to 15 pounds gauge. The two Inch valve cock on the stand pipe is opened and the discharge pipe observed to be sure the liquid Is being unloaded. To protect the seams In the tankcar, the pressure must not exceed 30 pounds. The oar will begin to un load at about 12 pounds pressure. When the oar Is empty, the air pressure will drop off rapidly and air will blow out of the vent on the receiving tank. The air flow may be stopped at this point and the tankcar pressure released through the vent valve on the "cross" arrange ment. After Inspecting the car to be sure that It has been completely unloaded, all connections and dome cover should be closed tightly. It Is essential that the empty tankcar be sealed Immediately after the car is unloaded In order to keep the oar filled with dry air during return shipment. As a final step. It Is desired that a standard railroad wire seal be In serted through the slotted bolts of the car fittings. Steam should be released from the car colls and all condensate re moved from the colls by blowing with air with the steam trap by passed. All connections must be replaced as received. Adequate care should be taken In preparing and sealing the car for re turn shipment. *It Is essential that the displacement air used for unloading be dried thoroughly by some dehumldifylng unit such as soda lime, activated alumina or similar 10 HONS 077A09 dehydrating agent drying unit. It may be neceasary to recharge the dehumldlfylng unit each time that a car la unloaded. For unloading a tankcar of Aroclor within three houra, 15 atandard cubic feet a minute of air at 15 pounds per square Inch gauge pressure and a -10F. dew point should be supplied. If the dry air unit la to be used only for unloading tankcars. a small single tower dryer unit containing a self-contained reactivating heater Is suggested. Two manufacturers of air dryers of this type are: C. M. Kemp Mfg. Co., 405 E. Oliver Street, Baltimore 2, Maryland and Pittsburgh Lectrodryer Corporation. Foot of 32nd Street, Pittsburgh, Pennsylvania. 11 MOMS 077410 CHAPTER 2 STORAGE TANKS A. Qeneral Description. The storage tanks should he a minimum of 10,000 gallons and preferably 12,000 to 15,000 gallonB capacity to accommodate the normal 8,000 gallon tankcars. It is preferable to locate the tanka above ground where they are easily accessible for any changes or repairs. Under ground location presents difficulty In this respect. Especially in cold dllmates, It la preferable to locate the tanks Inside of a building. The tanks should be located conveniently with reference to the tankcar unloading facilities and the area where the dielectric Is used. Although Aroclors are non-corrosive to metals, corrosion or rusting of iron and steel equipment (by oxidation) may ocour resulting In contamination of the products. The re sistance of Aroclors to materials of construction Is given In Monsanto Technical Bulletin O-P-115, entitled, "The Aroclors," Page 6. Stainless steel tanks are very satisfactory but relatively expensive. Stainless steel pipe Is relatively difficult to fsbrlcate and it Is difficult to make tight leek-proof connec tions . Storage tanks may be of steel construction If properly metallized with sinc-tin or aluminum on the Interior sufaces 12 coming in contact with the Aroclors. The metallizing should be done according to the following procedure: 1. Clean an area of the surface by sand blasting, or a similar method, to give a perfectly clean and roughened surface. The area cleaned should not be greater than can be completely metallized within a few hours after cleaning. 2. If zinc-tin metallizing la used, a coating of zinc 0.005 Inches thick should be sprayed on to the cleaned surface. This Is followed immediately by a coating of tin 0.007 Inches thick. 3. Aluminum metallized surfacing should be about 0.01 inch thlok. The detailed procedure for metallizing and cleaning Is outlined as follows: a) Sand blast, b) Coat with iron, 0.005 inches thick. (The purpose of this coating Is to provide a rougher and better bond for the finish coat of aluminum or the zlnc-tln combination.) c) Apply the selected finish coat, d) Fill the tank with tap water and warm It with steam. (If an open steam line Is used, do not allow the steam to Impinge directly onto the metallized aurfaoe of the tank.) e) Drain the tank, f) Fill with cold water and drain, g) Wipe dry with clean diaper cloth or other fabric relatively free of lint, h) Heat the tank to at least 100C. (212"F.) to expell moist air. It would be beneficial to heat the tank, allow It to cool and pull dry air through It using a dehumldlfylng breather In the air line,heat again etc.,until the tank Is full of com paratively dry air. 1) Spray about 100 gallons of new, 13 MOMS G77412 electrical grade Aroclor (not high In vlacoalty) or electrical grade trichlorobenzene onto the Inner walls of the tank, washing the walls thoroughly. J) Attach the circulating pump, the lines used, and the filter press fitted with dry paper and circulate the fluid through the system and the tank. Install new dry filter paper several times in the press during this drying and cleaning operation. Discard the dielectric fluid used for cleaning, k) Partially fill the tank with new Aroclor dlelectrlo and analyze It electrically and chemically to determine whether it meets specifications. If all tests are met, then fill the tank with the dielectric. The tanks should be Insulated using, preferably, glass ( foam beads as supplied by Dow-Cornlng or Libby-Owens-Ford. The suggested thickness of the glass Insulation Is one Inch minimum to two Inches maximum. The glass Insulation may be covered with tar material commonly used for weatherproofing. Another type of Insulation which may be used Instead of the glass Is B5$ Magnesia-Wool whloh should be covered also with the weatherproofing tar. The advantage of the glass Insula tion is that it Is not moisture sensitive as Is the case with Magnesia-Wool. If the storage tank Is located outdoors, It Is best that the insulation be covered with riveted or bolted tin sheeting painted with aluminum paint, nils type of metal surface weathers well and la cleaned easily. All piping must be i galvanized and screwed fittings must be back brazed to assure 14 HONS 077A13 tightness. All handling pipe lines must be traced with steam lines and Insulation applied over the two lines In order to keep the handling lines and the material up to the desired pumping temperature. Usually a one-fourth Inch copper steam line running parallel with the handling line will suffice. Under very severe conditions of low temperatures, It would be desirable to wind the steam line around the handling line about two turns to the foot. The tanks muBt be provided with ample pressurized heating coll surface to supply sufficient heat to the material to bring It to the proper temperature for pumping and handling as Indicated In Table III. Heating colls should be either metallized steel, or preferably steel colls which have been galvanized after fabrication. It Is recommended that the steam pressure on all heating colls should not exceed 100 pounds per squsre inch gauge; lower pressures may be used where practicable. It Is essential that all steam colls be completely free from even minute leaks since this will In troduce water Into the product. The steam oolls may be introduced as "halr-pln" colls through a manhole at the side and bottom of the tank, or as Is most often done, inserted through the manhole at the top of the tank and then located near the bottom. External heating colls located in the Jacket of the tank may be used but this construction Is more expensive and less efficient than the Internal oolla. 15 HONS 077*14 The storage tanks may be fitted with a stirrer, either through the top, side, or bottom of the tank and the propeller blade should be located near the bottom of the tank. However, Insertion of a stirrer through the side offers possible source of a leak and since these materials are homogeneous, It la not essential to provide such agitation for the purpose of mixing. Adequate circulation can also be accomplished by using a centrifugal type pump. Qear pumps or other equipment where wear or chipping of metal parts may Introduce contamination should not be used. The pumps must be of the type designed to handle hot oil. All wetted pump parts should be either stainless steel or bronze. The oentrlfugal pumps must be provided with a deep stuffing box and proper packing used, as described In Chapter 3. As examples of pumps found com pletely satisfactory for this service, reference la made to Worthington Worthlte pumps. Blackmer pumps, and Dayton Dowd Type C pumps for handling hot oil. Also, a very satisfactory arrangement for mixing or circulating and pumping the fluid from the storage tank 1b to use a vertical sump pump such as a Taber pump. All storage tanka must be amply provided with a dehumldlfylng breather such as BOda lime, activated alumina, etc., units. This Is essential to prevent moist air from ooming In contact with the dielectric. A moisture content above 35 ppm 16 HONS 077415 adversely affects the electrical resistivity of these pro ducts. Provision Bhould be made to preclude possible leakage of the drier material back Into the Btorage tank and the drier should be inspected periodically to make sure that It Is open and not plugged. B. Detailed Description. Drawing No. 90-8170 shows the detailed construction of a horizontal 15.000 gallon storage tank for Aroclor and Its mixtures which has been found completely satisfactory. The various nozzles on this tank are used as follows, con sidering them In order from left to right on the drawing: 3" nozzle 24" nozzle Inlet for recirculation For future agitator If required (not used) 3" nozzle For soda lime or calcium chloride breather connection 36" manhole Por Inspection, etc. The float gauge la located In tie center of this manhole. 3" nozzle 24" nozzle Not used Por future agitator If required (not used) 3" nozzle 3" nozzle 18" X 26" Oval Nozzle Not used Filling Inlet connection For sump pump 3" nozzle Por thermometer well (see detail) The two 24" nozzles were originally Installed for Installa tion of agitators. If required. However, it has been found 17 unnecessary to use agitators In the storage tanks, and these nozzles could be omitted. It has been found that circulation of the fluid by the sump pump, snd Into the nozzle at the opposite end of the tank, for several hours gives satisfactory blending of the tank contents. For pumping the dielectric from the storage tank, a Taber Pump Co. all bronze 2-1/2" X 2" vertloal sump pump with monel shaft has been found to be quite satisfactory for the applica tion. The liquid level gauge used In the storage must be gas-tight. The storage tanks are equipped with Vapor Recovery Systems Co.'b "Verec," gas-tight, automatic tank gauge as shown by Drawing No. 9C-8278. The Btorage tanks should be provided with an operating platform suitable to the customer's conditions of operation. The dshumldlfylng units used as breathers on the storage tanks can be constructed as shown by Drawing No. 9C-8248. The upper portion of the chamber Is charged with anhydrous soda lime or another drying agent. Periodic Inspection of the dryllng agent will show the formation of a cake of damp material on top about 1 to 1-1/2 Inches deep. This cake should be removed and fresh material recharged. Any suitable construction similar to that shown on Drawing No. 9C-82<l8 may be used for the breather units. Drawing No. D-13362 shows design detail of a 15,000 gallon 18 MCNS 077417 I vertical storage tank. The vertical type tank Mould seem especially desirable when Insufficient space Is available to accommodate the horizontal type tank. < 19 MOMS 077418 ( CHAPTER 3 OASKETINO AND POMP PACKINO Aroclors and their mixtures Boften and swell natural rubber and many of the synthetic "rubber" materials. Such material not recommended for use. Include Hycar P, Koroseal, Perbunan, Neoprene, etc. These materials are known sources of con tamination. Suggested types of packing and gasketing materials Include: 1. For Welded Flanged Pipe Connections: Oarlock Packing Co., No. 901 or No. 7021, 1/8 inch asbestos fiber sheet. A ring of thin aluminum drawn tightly at the flange connections may be used satisfactorily also. 2. For Pumps: Oarlock No. 234, No. 431, and Cheveron No. 7050-C are satisfactory packings. Likewise, Durametalllc's spiral asbestos fiber may be used. Johns-Manvllle and others have oomparable packing materials. 3. For Valves: Oarlock No. 117 braided packing or Its equivalent Is suggested. 4. other Resistant Materials: It is indicated that duPont's Teflon, poly tetrafluoroethylene Is not attached by hot (130*C.) Aroclor and is to be reoommended as a gasket material. Dow-Cornlng's Silastic, Silicone 180, Is very resistant to Aroclor and Is suggested for gasket purposes. 5. In some cases oork Impregnated under pressure with Chrysler's Cycloweld 55-9 or Armstrong Cork Co.'s 1162-J and cured at 170* C. may be used as a gasket material. These are baked phenolic type coetlngs. 6. Pipe Thread Compounds: When necessary to use pipe thread compounds, the following should be satis factory If oare is taken to prevent the pipe compound from getting on the Inside of the pipe. (a) Plastic Lead Seal-- manufactured by Durametalllc Corp. (b) Ordinary white lead 20 MOWS 077419 Usually It Is not necessary to use pipe thread com pounds since all screwed pipe fittings should be sealed by back brazing. 7. All new lines and fittings Siould be cleaned thoroughly by steaming (for two hours) and dried with air or heat. 21 MOhS 077420 ( CHAPTER 4 SAMPLING METHODS 1.) The ASTM Standard Method for sampling electrical Insulating oils Is described In ASTM Designation: D923-49. This describes glass and metal thlefs for sampling drums, cans, and tankcars. A specially designed thief or bomb for sampling tankcars is described, also. A very good Instrument of this type is the stalnless-Bteel Bacon Bomb Thief with which samples of the liquid can be drawn from any level of the tankcar. The ASTM procedure describes sample containers, their cleaning and storage. Under general precautions, the ASTM mentions that, "Samples of the fluid shall not be taken until the oil Is at least as warm as the surrounding air, because cold oil may condense enough moisture from a humid atmosphere to affect seriously Its insulation properties. (In the case of tankcar lotB, on some occasions there may be no choice, as it may be necessary to procure samples from a tankcar when the tempera ture Is not above the surrounding air. On such occasions, the temperature of oil and air, also the humidity If possible, should be noted In the report of test results.) it Is undesir able to do any sampling when the relative humidity of the atmosphere exceeds 75 percent, and samples shall never be taken In the rain." 22 HONS 077421 At the plants of several electrical manufacturers using Aroclor dielectrics, the practice is to switch the tankcars directly into the plant building or under roof before sampling and unloading. These precautions in handling are taken to avoid any contamination of the fluidB which are manufactured under very strict specifications. For example, the specification for ionlzable chlorides allows no more than 0.10 parts per million. Also, moisture may not exceed 30 to 35 parts per million. Tankcars are cleaned and prepared under close inspection before they are filled. When filled, and analysis Bhows the material in the car to be satisfactory, the car is then sealed with a standard railroad wire and seal Inserted through the slots of the dome fittings. Likewise, after the tankcars have been unloaded in the Industry, It la requested that the dome fittings should be sealed with a railroad wire and seal. Drum packaging Is made with new and carefully Inspected drums, only. These drums are lined with specially selected baked phenolic coatings. An example is NESCO No. 3 lining offered by the National Enameling and Stamping Company, Long Island, New York. Contents of drums should not be heated by direct application of flame or strip heaters. Radiant heat from Bteam colls or hot air in a heated room is to be preferred. 2.) Monsanto Methods used for sampling tankcars differ somewhat from the ASTM procedure. The modified techniques are 23 HONS 077422 used because of their greater simplicity and they have been entirely satisfactory as employed over many years. A sample is never taken when it is raining or snowing or when there is any ohanoe of contaminated atmosphere moving in the direction of the car. However, in case of an emergency, during Inclement weather, a canopy is placed over the car dome before sampling. A satisfactory sample bottle is a five pint, round amber glass, paoker type container fitted with a 38 millimeter Bake- llte screw cap with an aluminum or tin cup liner. Bottles of this description can be purchased from the Northwestern Bottle Company, 3144 North Broadway, St. Louis, Missouri according f to their No. a-7253* Only new bottles and caps are used. When a shipment of bottles is received, the bottles are capped immediately and stored in their receiving cartons, prior to use, the exterior of the bottles is wiped with a clean cloth. The simplest sampling device used is a clean stainless steel or aluminum dipper. However, this is not a generally preferred device because it permits sampling the car from the near surface, only. The sampling device commonly used consists of a stainless steel tube, seven feet long with one end bent into a hook, to serve as a handle and on the other end there is a stainless steel bucket with a perforated bottom. This bucket is about l Inches inside diameter and 6 inches deep to hold the five pint bottle. 24 MOHS 07 This bottle Is held firmly by a stainless steel collar made to slide along the shaft of the sampling device. This collar has a clamp attachment for fixing it tightly into place where desired around the neck of the bottle. When a car is to be sampled, a new sample bottle is clamped firmly in the bucket. All dirt is brushed and wiped away from the car dome area using a clean rag. The car dome is opened and the cap is then removed from the sample bottle. The sampling device is Inserted into the car so that the neck of the bottle is at least twelve to eighteen Inches below the surface of the fluid. The sample taken is discarded as its purpose is to rinse the bottld. A portion of the sample la used to rinse the interior of the bottle cap. This procedure is repeated until a minimum of three rinses.has been made; each time the sample taken is not put back into the car. These rinses should be discarded. Then the sample is taken and the cap of the bottle is screwed down tightly. When the sample has been obtained, the car dome is re placed, immediately. HQhS 077424 The exterior of the sample bottle is wiped with a clean cloth and when returned to the laboratory it is further clean ed with a cloth dampened with pure trichlorobenzene. If the sample 1b to be shipped, the cap is taped with Scotch Tape. The sampling device is also cleaned with pure trichloro benzene and is stored in a dust free, air conditioned room. 25 CHAPTER 5 LABORATORY ANALYSIS AND PROCEDURE FOR TREATING AROCLORS AND THEIR MIXTURES WITH EARTH A sample of the Aroclor or Aroelor mixture taken from the tankoar, or drums, as described In Chapter 4, Is analyzed In the laboratory to determine Its quality In accordance with the property values given In Chapter 7. For capacitor use, usually the Important properties tested are resistivity, power factor and moisture. For trans former use dielectric strength, resistivity, moisture, and free chlorides are the Important properties. If the sample is out of line with the shipping specifica tions, It Is Indicated that the sample has become contaminated. In this case, another sample is to be taken and the properties redetermined. If still out of specifications, the sample should be given treatment with earth. Treatment of the dielectric with conditioned Attapulgus earth will bring the electrical properties to the maximum attainable values. While there Is complete agreement on the benefits derived from treating with conditioned earth, there Is difference of opinion on details of the method, arising from factors such as the following. No doubt, there are differences In the aborbent power of various types of dlatomaceous earth with respect to removing moisture, impurities and additives such as stabilizers or scavengers from the dielectric 26 MOMS 077*^5 materials. The size of the earth particles, temperature and conditions of activation of the earth, the concentrations used and the temperature, the degree of agitation and time Interval at which the dielectric Is given earth treatment are all possible variables whloh are still being studied In various laboratories. The method used by Monsanto for treating the fluid with activated earth In the laboratory Is: The absorbent Is minuB 200 mesh Attapuigus* earth ac tivated Just prior to use by heating In shallow trays for four hours at 400 C. (752 P.) or for at least twelve hours at 250 C. (482 F.). At least one quart of the dielectric sample Is placed Into a clean two liter Pyrex beaker or three necked flask. The beaker or flask should be cleaned Just prior to ubs In a manner similar to the procedure described In Chapter 6, Method No. 11,751 "Procedure for Cleaning of Electrodes, 0. E. Cell and Accessories". The flask or beaker 1s fitted with a glass or stainless steel agitator. Heat Is applied using either a hot plate or a Olas-Col mantle and Is controlled by a thermostat such as a Penwal thermo switch with a stainless steel sheath. About 0.1 to 0.2% of the activated earth, based on the weight of the liquid Is added. *Attapulgus Division, Minerals ft Chemloals Corp. of America, 210 WeBt Washington Square, Philadelphia 5, Pennsylvania. 27 MONS The more viscous dielectrics such as Aroclors 1248 and 1254 are heated at about 70 to 80 C. (158 - l,o P.) and the less viscous materials such as Aroclor 1242 and P/ranols 1481, 1467, and 1470 are heated at about 50 to 60 C, (122 to 140 F.). After heating and stirring the sample for about four hours, It Is filtered using a clean Pyrex glass suction flask and a Buchner funnel fitted with a Whatman No. 1 or No. j filter paper. This apparatus and the bottle Into whieh the treated sample of dieleotrlo Is transferred should have been cleaned In a manner similar to the oleaning procedure des cribed In Chapter 6. The earth treated and "up-graded" sample Is then ready for final analysis of Its electrical properties. 28 MOMS 077*27 CHAPTER 6 TEST PROCEDURES A. general Information, The Monsanto test methods described here with the special equipment used are some of the control tests employed to main tain the quality of Aroolors for dleleotrlo use. They are suggested as a guide for test work needed to Indicate the quality of the dielectrics used In the manufacture of electrical goods. The most significant eleotrlcsl tests made on Aroolors for oapaoltors are: 1. Dielectric constant. 2. power Factor 3. Resistivity For transformer use the most significant tests of Aroclor mixtures are: 1. Dielectric Strength 2. Resistivity In both caaeB a significant chemical test Is corrosion chlorides. The following ternm are defined: Dlelectrlo Constant: The dielectric oonstant (sometimes oalled specific Induc tive oapadty) of any substance Is equal to the ratio of the capacitance of a condenser when that substance is used as the 29 HOMS 077428 dielectric to the capacitance when there la a vacuum between the conductors (for all practical purposes air at ordinary pressures may be used Instead of a vacuum). Dielectric Strength; Dielectric Strength Is the rupturing strength of an Insulating material when subjected to voltage atresB under specific conditions and expressed In kllovoltB. Breakdown varies with the shape of the eleotrodes and does not Increase directly In proportion to the thlokness of the dielectric. Power Factor: The power factor of a dielectric Is the ratio of the energy loss In the dielectric to the "apparent power" In the dielectric. Resistivity: Resistivity is electrical resistance offered to the passage of a steady current. The volume resistivity In ohms centimeter of an oil Is the ratio of the d-c potential gradient In volta per centimeter paralleling the current flow within the sample, to the current density in amperes per square oentlmeter at a given Instant of time and under prescribed conditions. Volume resistivity is expressed In ohm-cm. The analytical procedures described In detail Include: 1. METHOD NO. 11,751, "PROCEDURE FOR CLEANING OF ELECTRODES, 0. E. CELL AND ACCESSORIES." 2. METHOD NO. 11,608, "DIELECTRIC CONSTANT AND POWER FACTOR." 30 MOWS 077429 3. METHOD NO. 11,605, "DIELECTRIC STRENGTH." ft. METHOD NO. 11,607, "RESISTIVITY." 5. METHOD NO. 10,126 "CORROSION AND CHEMICAL STABILITY." 6. METHOD NO. 10,110, "INOROANIC CHLORIDES." 7. METHOD NO. 10,087, "ACID NUMBER." 8. METHOD (MODIFIED) NO. 10,620, "MOISTURE (WATER)." B. Detailed Instruction and Testing Methods. 1. METHOD NO. 11,751, "PROCEDURE POR CLEANING OF ELECTRODES, O.E. Cell and Accessories." a. The electrode Cleaning Procedure: 1) Place the electrodes In hot eleotrlcal grade Trichlorobenzene for ten minutes. 2) Wash with unheated TCB. 3) Rinse twice with methanol and twice with tap water. ft) Plaoe the eleotrodes in hot 10$ Trl Sodium Phosphate solution. Soak and heat for ten minutes. 5) Wash thoroughly with tap water. CAUTION: After Step 5--DO NOT TOUCH THE ELECTRODES WITH HANDS! 6) Wash with distilled water twice. 7) Dry In drying oven for et least two hours at 120*C. b. The 0. E. Cell Cleaning: 1) Reclean the Cell before use, when more than 8 hours have elapsea since the previous oleanlng. 2) Follow the procedure for the electrodes starting at Step ft. 31 MOHS 0 7 7430 c. Cleaning of the Accessories: 1) Apply the same cleaning procedure as given for the electrodes (Steps 1 to 7) to prepare the glass spacer and beaker for next test. 2) Clean the thermometer In the Bame manner as the electrodes, except for Step 7. 3) Place the wet thermometer (after Step 6) directly in position In the Temperature Heating Unit (Modified Fisher isotemp Oven) and allow to dry. METHOD NO. 11,608. "DIELECTRIC CONSTANT AND POWER FACTOR. I. Adjustment of Controls on Electrical Apparatus A. On Panel No. 1 (Top Panel, Amplifier and Null Detector; a. Turn the 4-way (main power) switch on the upper right hand side to the #3 position to determine the Dielectric Constant at 1000 oycles. Turn this switch to the #2 position for measurements 6U cycles. b. Allow the equipment to warm up 10 minutes. c. Turn "GAIN CONTROL" to 6. d. Depress "INPUT 0.03V." button. B. On panel No. 2 (Oscilloscope) a. Turn "INTEN." to about the 12 o'clock position CAUTION: Do not allow a high intensity spot to remain stationary on the screen for any length of time. b. Using "HOR. POSITION" and "VERT. POSITION" controls center the Image on the screen. c. Adjust "FOCUS" for sharp line. d. Turn "FREQ, SELECTOR" to 100KC. e. Turn "FREQ. VERNIER" to 80. 32 HONS 077*31 .f Turn "VERTICAL INPUT" to " 10 VOLT MAX." g. Turn "VERTICAL INPUT" to " 10 VOLT MAX." h. Turn "HORIZONTAL GAIN " to about 20. .1 Turn "SYNCHRONIZING" to + 20. J. Turn "SYN". To "EXT. SYN." k. Turn "GEN." to "SWEEP GEN. " C. On Panel No. 3 (Capacitance Bridge) e. Turn "RANGE SELECTOR" switch to "100 C" for 60 cycle measurements and to "1 Kc" for 1000 cycle measurements. b. Turn "METHOD SWITCH" to direct. c. Turn "DISSIPATION FACTOR" selector switch to "0" . D. On panel No. *1 (oscillator) a. Disregard this panel for measurements at 60 cycles. . b. On 1000 cycle measurements, depress the No. 10 "MULTIPLY BY" button. c. Set "FREQUENCY DIAL" to 100. d. Turn "OUTPUT" dial so that pointer is at the end of the arrow. e. Depress the "UNBAL. 5000 OHMS" button. When all of the above adjustments are made, the eleotrlcal apparatus is ready for measurement of Dielectric Constant and Power Factor. II. Determination of Constants for the Apparatus 1. Carefully assemble the cell which has been cleaned and dried within the last 8 hours. Refer to Method No. 11,751 for the procedure to use m cleaning tne ceils. 33 MONS C77432 2. Place the cell assembly In the Fisher oven which has been adjusted to 25"C. 3. Connect the back wire Inside the oven to the lead on the Inner cylinder of the cell end the front wire to the lead on the outer cylinder of the cell. 4. Connect the cable from the capacitance bridge to the terminals on top of the oven so that the Inner wire of the cable goes to the back terminal and the outside mesh casing of the cable (the ground) goes to the front terminal. 5. Remove the thermometer from the top of the oven before going on with the test. THT8~Ts important. 6. Hake all adjustments on the electrical apparatus as directed In Part I. of this method. 7. Balance the bridge by rotating the "CAPACITANCE" and "DISSIPATION FACTOR" dials on Panel No. 3 until the wide vertical band on the oscllllscope Is adjusted to a minimum width. 8. Record the sum of the readings on the "CAPACITANCE" dial and vernier and call this value A. 9. Remove the beaker containing the cell from the oven and fill it with C. P. benzene to a level 0.737 Inches (oa. 3/^ inch) above the top of the concentric cylinders of the cell. 10. Adjust the temperature of the benzene to 25C. while stirring with a thermometer. 11. Replace the cell In the oven (at 25C.) and make the same electrical connections as In Steps 3 and 4. DO NOT Interchange connections. 12. Balance the bridge again as In Step 7. 13. Record the sum of the readings on the "CAPACITANCE" dial and vernier and oall this value B. 14. Calculate the cell constant by the following equation: Cell Constant, K - B - A ,(thle la usually 2.27 - 1.0 around 70 uuf). 34 NONS 0 7 7433 15. Remove the cell from the oven and balance the bridge as in Step 7 with the "CAPACITANCE" and "DISSIPATION" "FACTOR" dials. 16. Record the sum of the readings on the "CAPACITANCE" dial and vernier and call this value F. (capacitance of connecting oable). 17. Calculate the CELL LEAL CAPACITANCE by the following equation: CELL LEAD CAPACITANCE, 0 A - F - K (this Is usually around 3 uuf.) WHERE: A - CAPACITANCE OF ENTIRE SYSTEM IN AIR (SYSTEM CONSTANT) 0 - CAPACITANCE OF THE CELL LEADS (CELL LEAD CONSTANT) F - CAPACITANCE OF CABLE AND WIRES WHICH CONNECT THE CELL AND CELL LEADS TO THE BRIDGE. (CONNECTOR CONSTANT) K - CAPACITANCE OF THE CELL ALONE (THE CELL CONSTANT) Tabulate the system Constant (A), the Cell Lead Con stant (a), the Connector Constant (F), and the Cell Constant (K) on a place of stiff paper and post them near the instrument where they can be easily referred to for comparison and calculations. These constants must be checked at least once every three months and In all cases where the Dielectric Constant and/or Power Factor are out of specification. III. Measurement of Dleleotrlo Constant and Power Factor on Aroclors, I'yranois, inerteens, ana Tri-Tetrschlorobenzene Bienas. A. Teat Run on Cell to Determine Whether It 1b Clean and properly Aligned. 1. Carefully assemble a cell which has been cleaned and dried within the past 8 hours. 35 MONS 07743* NOTE: Refer to method No. 11,751 for procedure to uee In cleaning cells. 2. Adjust the oven control to hold at a temperature of 100C. for all materials except Tri- Tetra Blends. If a Trl- Tetra blend 1b to be tested, adjust the oven to hold a temperature of 25"C. 3. Place the empty cell aasembly in the oven and connect the back wire inside the oven to the lead on the inner cylinder of the cell, and connect the other (front) sire to the lead on the outer cylinder. 4. Connect the cables from the capacitance bridge to the terminals on top of the oven so that the inner wire of the cable goes to the back terminal aS3 the outside metal casing (ground) goes to the front terminal. 5. Allow 15 minutes for the cell to reach temperature equilibrium inside the oven. 6. Remove the thermometer from the top of the oven be tore felting any measureoenfs-on the-bridge. This is Important. 7. Make all the adjustments on the electrical apparatus as directed in Part I of this method. 8. Balance the bridge by rotating the ''CAPACITANCE" and "DISSIPATION FACTOR" dials on Panel No. 3 until the wide vertical band on the oscilloscope Bcreen is adjusted to a minimum width. 9. Record the sum of the readings on the "CAPACITANCE" dial and vernier and compare this value with the SYSTEM CONSTANT determined in Part II of this method. IMPORTANT: IF the value obtained in Step 9 does not agree with the system Constant A (Part II) within 5 uuf, the cell must be re-cleaned, re-dried, re-assembled, and the test run for the System Constant must be repeated. NOTE: Although the above test run must be made prior to each analysis, the value obtained in Step 9 la not to be used in calculations but is to be used only as a-check on the cleanliness and alignment of the cell. 36 MCNS 077435 B. Procedure for Testing Materials 10. Remove the cell from the oven and fill the beaker with the material to be tested to a level 0.737 Inches (oa 3/k Inch) above the cylinders of the cell. 11. Adjust the temperature of the sample to 100C. (use hot plate) for all materials except Tri-Tetra blends. For Tri-Tetra blends, adjust the tempera ture of the sample to 25C. using an loe-water bath if necessary. NOTE; Stir sample continuously with a thermometer while adjusting the temperature. 12. Place the cell and sample in the oven and make the same connections from the cell to the bridge as In Steps 3 and 4. DO NOT interchange connections. 13. Allow fifteen minutes for the cell to reach tempera ture equilibrium inside the oven. 111. Remove thermometer from the oven before taking a measurement. This Is Important. 15. Make the adjustment of oontrols on the electrical apparatus as directed In Part I of this method. 16. Balance the bridge by rotating the "CAPACITANCE" and "DISSIPATION FACTOR" dials on Panel No. 3 until the wide vertical band on the oscilloscope screen la adjusted to a minimum width. 17. Record the sum of the readings on the "CAPACITANCE" dial and vernier, and call this value X. 18. Record the sum of the readings on the "DISSIPATION FACTOR" dial and switch. Call this value D. Calculations; Dielectric Constant = X -F -0 K Where; X - Capacitance reading from step 17. F - Connector Constant (Determined In Part II) 0 - Cell Lead Constant (Determined In Part II) K - Cell Constant (Determined In Part II) 37 MCKS 037436 % Power Factor - f x D Where: f - Teat Frequency (60 cycles or 1000 cycles) fp: frequency of "Range Selector" on panel No.3 D = Dissipation Factor reading from Step 18. NOTE: When D (dissipation factor) Is less than 0.1. the dissipation and power factors differ by less than 0.0005. Therefore, for our measurements, power factors and dissipation factors are equal. Precision: (Reference: General Radio Manual for Model 716-C Capacitance Bridge) a. Capacitance readings are precise to + 2 uuf x multi plier reading (+ 0.2% of full scale for each range) when the dissipation factor is less than 0.01. b. Dissipation Factor (Power Factor) readings are precise to + 0.0005 or + 2$6 of the dial reading whichever la larger, foF values less than 0.1 for D (Dissipation Factor). Apparatus A. Oscilloscope: Heathklt Model 0-6 B. Constant Temperature Heating Unit: Fisher Isotemp oven. Model 13-245A, modified to lnolude Inter wall connectors. C. A. C. Generator: Oeneral Radio type 1302-A. D. Amplifier and Null Detector: General Radio type 1231-B with type 1261-a power supply. E. Capacitance Bridge: General Radio Co. Capacitance Bridge type 716-C. F. Test Cells: 0. E. type, ooncentric cylinder electrodes Catalog # 1,559,663. 0. Class B driver transformer: This la used for 60 cycle measurements to exolte the bridge directly from the domestic power line. It has 50 volts output with a 4800 ohm resistor In service. H. Tuned Circuit Filters: Oeneral Radio Type 1231-P2 (400 and 1000 cycle) and 1231-P3 (60 cycle). These filters aid In obtaining a more accurate frequency for the measurements by removing harmonics, noise, hum, etc. 38 MONS 077*31 3. METHOD NO. 11,605, "DIELECTRIC STRENGTH". a. Apparatus and General Information The electrical equipment neoessary to provide high voltage to permit the determination of dielectric strength of liquid dielectric at commercial power frequencies la basically quite simple. The equipment assembled in the laboratory conslts of a high voltage transformer of good design and with a current capacity of 2.43 KVA and with equip ment for control of the voltage and a means of measuring the voltage and to provide safety for the operator. It is enclosed in a steel grey crackle finished cabinet measuring 42" high, 22" wide, 17" deep and set on truok casters for easy mobility. Protective equipment incorporated in this apparatus prevents the application of high voltage unless all safeguards are complied with. The door on rear of cabinet must be closed. The cover over the oil must be all the way down and the voltage control must be at 0 position. Failure to comply with these requirements will prevent any action when the red button is depressed. The teat cup: Transformers, Voltmeters, and Accessories 39 MOMS 077438 The askarel testing cup type No. 2214809 supplied by General Electric Company la mounted on the top rear of the cabinet. It la protected by a heavy plastic cover, hinged at the rear for accessibility to the receptical. It la equipped with safety contactor so placed that the circuit energizing the high voltage contactor oannot be completed unices the protective cover Is completely lowered and In place. It Is Impossible for the operator or anyone else to touch :he tasting cup when high voltage Is applied. The High Voltage Transformer manufactured by the Kelly-Koett Manufacturing Co. la of the closed core, oil Immersed, shell type design. Rated 9 81,000 volt 9 4)0 tnlllempera. It was recovered from a used X-ray machine, purchased quite inexpensively. An auto transformer from the same X-ray machine la connected so as to limit the out-put voltage of the high voltage secondary to 50,000 volts. The primary of the auto transformer lc connected to the secondary of a 2-1/2KVA powerstat variable auto transformer supplied by the Superior Electric Company. 40 CNS 077*39 Power to the poweratat Is controlled by a 4 con tact 30 amp. solenoid circuit breaker. The voltmeter mounted on top near front edge Is connected across the poweratat secondary and Is calibrated to read direotly in Kilovolts In the range of 0 - 50 K. V. The overload circuit breaker consists of a small relay connected between one side of the high voltage transformer secondary center tap and ground. It is adjusted to break contact on a current drain of about 50 mllllampers. The circuit for the coll of the solenoid circuit breaker is wired through the oontacts of this relay. Safety and Operating Controls. 1) Door interlock switch located on rear door. 2) Test oup cover Interlock awitoh. 3) Powerstat switch mounted on rear of unit arranged so that high voltage contactor cannot be cloaed unless poweratat Is at zero position. 4) Main power switch on front panel. 5) Poweratat voltage oontrol on front panel. 6) High voltage contactor push button on front panel (red) 7) Signal lamps mounted on top around voltmeter. Purpose and operation described in method of use. 41 MOtls 0 77*40 b. Procedure. 1) Ascertain that the temperature of the material under test is 25 (+ 0.5) C. NOTE: Testing at other temperature is likely to give variable results which may be misleading. 2) Shake the sample container so aa to thoroughly mix the askarel before filling the test oup. NOTE: This operation is especially Important with used Aroclor as the impurities may settle to the bottom and the test may be misleading, 3) Rinse the testing cup three times with small portions of the sample to be tested. 4) immediately after final rinse, fill the cup to a height of not less thsn 20 mm. (0.787 in.) above the top of the electrodes. 5) Rock the cup a few times in order that any entrapped air may escape. Close cover over oil test cup. 6) Allow to stand 3 minutes. CAUTION: THIS IS IMPORTANT. ------------- 7) Turn main toggle switch on front panel to "ON" (or up) position. Both green and amber pilot lights on the top at either Bide of the voltmeter will now glow. NOTE: The green signal light is connected across the 11b volt ln'put and denotes that line voltage has been applied to operating control circuit. Amber light is connected in series with sensitive BWltch located under high voltage contactors and connected to its armature. It indicates that high voltage oontaotor la in its rest position and away from contacts energizing auto transformer. 8) Turn voltage oontrol (large knob on front) to extreme counter-clockwise position. 9) Depress red button on front. This energizes high voltage transformer and circuit breaker and is indicated by amber light going out and 42 HONS 077441 the red light directly over voltmeter will llghTT 10) Watch the voltmeter and, while holding the button "IN", turn the voltage control at such speed that will cause voltage as Indicated on voltmeter to rise at a rate of 3 K. V. per second. 11) Note and Record the voltmeter reading at breakdown. 12) Repeat the test until two successive break downs occur on each of two fillings of the *.teat cup which do not differ by more than 10 Report the average value of these two readings (Step 12) as the Dielectric Strength. If the limit of the instrument Is reached before breakdown, report the Dielectric Strength as 50 K. V. at 25*0) Cleaning of the test cup; After the test Is completed, drain the cup. Flush the cup with benzene. Then fill with Aroclor 1248 and let stand until the next analysis. NOTE: An exception, when samples of oil from the plant are are brought In for test, the cup must be thoroughly cleaned with benzene and carbon tetrachloride before and after running the test. The electrodes: The testing cup has two electrodes. Both electrodes are movable and have twenty threads to the Inch with Index notches on both the electrodes and the lock nuts. To set the Qap: 43 MQNS 077*42 Arrange one of the electrodes and the lock nuts with the Index marks In line. Move the other electrode until It cornea In firm contact with the first electrode and lock It. Now unscrew the electrode with the Index marks In line (Step 1) two oomplete turns and lock It. This wlllfeave a gap of 0.1 lnoh between faces of the eleotrodes. Cleaning of the electrodes and the test cup free of oarbon ooatlng: The following ASTM method of cleaning shall be followed when It Is apparent from visual Inspec tion that the electrode discs of the cup are ooated with carbon. Wipe clean with dry calendered tissue paper the electrodes snd the test cup. CAPTION; It Is Important to avoid touching the electrodes with the finger or with portion of the tissue caper which has been in contact with hands. Rinse the electrodes and cup with dry lead-free gasoline, Stoddard Solvent (or dry, waterwhlte Kerosene) until they are entirely clean. Care 44 HONS 077443 should be taken not to touch the electrodes or the Inside of the cup after cleaning ao as to avoid possible contamination. METHOD NO. 11,607, "RESISTIVITY". a. Apparatus: general Radio Company Megohm Bridge Type 544-b. This la a combination of Wheatstone bridge and vacuum tube voltmeter for Indicating null. The direct measurement of resistance up to 1,000,000 megohms Is made possible by the use of a vacuum tube detector whloh absorbs negligible amount of power. The voltage applied to the unknown resistor is held approximately constant, regardless of the value of the unknown resistance. This condition Is necessary to measure resistance properly. The aocuracy of the Instrument In the range en countered In the measurement of Aroclor resis tivity, 100 to 1000 megohm Is + 6ji. The Instrument Is equipped with a 115 volt AC. power supply which supplies all operating voltages for the bridge Indicating circuits and In addition supplies 500 V DC for application to the material under test. 45 MOKS C77444 The Instrument le completely enclosed In e waxed finish shielded oak cabinet measuring 8-1/2" wide, 22-1/2" long and 8" high. Approximate weight--26 pounds. Teat Electrodes: Two concentric nickel cylinders with feet, obtained from General Electric Company. The Inner electrode has outside diameter of 2.8" and a height of 3.25" cm, *rJLJZtJi. K -- jW Jkl*. with area of 184 sq.^ height of 3.25" with area of 198 sq. cm. The distance between electrodes Is, therefore, 0/1" or 0.254 cm. By theory, electrode constant (K) area/length la 191/9.254 or 752 where average area Is 191 sq. cm. Also K s 36 rr x 10" x C (in farads with air as dielectric) or 11.29 x C (lnuuf. with air as die lectric ). Glass Plate: Pyrex about 3-1/2" diameter with concentric grooves to assist In spacing electrodes. Obtained from General Electric Company. Heating Unit: . Assembled In the laboratory and la the same unit 46 MONS 077A45 described in Dielectric Constant Apparatus (see Method No. 11,608; Equipment). Procedure: 1) Assemble the test cell. Place the recently cleaned (within the last 8 hours--see Method No. 11,751> Step 9) electrodes In an 800 ml. beaker. 2) Measure the oapacltanoe of the test cell (Cc) according to Method No. 11,608 (Dielectric Constant and Power Factor measurements) 3) Fill the cell assembly until the liquid level Is 3/4 lnoh above the top of the electrodes. ^t) Heat the assembly on the hot plate to 100 (+ 0.5)"c. 5) Place the assembly Inside of the testing oven. 6) Attach top lead (+) on the megohm bridge to Inner electrode. 7) Attaoh other lead to outer electrode. 8) Throw the three switches at the top of the megohm bridge to "ON" position. 9) Allow 10 minutes for assembly to reach tempera ture equilibrium Inside the oven. DANCER: Make sure control knob Is In "CHECK" position. Otherwise, painful shock will result If leads are touched. 10) Bring the galvanometer pointer to zero by turning the "ZERO ADJUST" knob In the direction In which the pointer of the galvanometer should move. 11) Turn the control knob to"CHARQE" position for one minute. 12) Turn the control knob to "OPERATE" position and return the galvanometer pointer to zero by adjustment of the "MULTIPLY BY" swltoh and the megohm dial. 47 HONS 077446 13) Read after one minute. Calculation; Resistivity* - Megohm dial reading (Step 12) x "Multiply By" reading (Step 11) x capacltanoe of cell (Step 2) In uuf. x 11.29 x 0.001. Report the result in units of 10^ ohm-cm, values of resistivity are qualified by designation of temperature and voltage. These are for this test, 100C and 500 volts DC. NOTEi It Is Important that the product under test, electrodes, and beaker be at uniform temperature for this determination. Temperature variations In different parts of the sample Hill oause the galvanometer zero to change constantly and give misleading results. CAUTION: Inasmuch as measurements must be made at a potential of 500 volts DC a shock hazard exists In the handling of this apparatus. With the oontrol knob in the charge and operate poeltlon full voltage of the bridge (500 volts) Is applied to the and low terminals and through the test leads to the eleotrodea. Do not attempt to handle the eleotrodes or the test leads unless the control knob Is In the 48 MENS 077447 ( "CHECK" position. Possible penalty for failure to observe this preoautlon -- Painfull Shook. 5. METHOD NO. 10,126 "CORROSION AND CHEMICAL STABILITY." a. Apparatus: 0. E. Corrosion Apparatus oonslsts of the following: 1) A Corrosion Flask - It Is a 300-ml. pyrex flask with a ground glass 24/40 Joint equipped with a 12-inch straight tube as an air cooled con denser. The alr-oondenser Is painted on the outside with aluminum. 2) The Corrosion Apparatus: A transits box 32" long x 8" wide x S>" deep. The top of the box represents a spilt transits board with holeB cut to fit the flasks. The box Is heated by two 500-watt, 15 volt O.E. Strip heaters with off-set terminals at one end (23.5" overall length). The heating length of the.heatlntr element la covered by a copper strip 19-1/2" long x V wide x 1/4" thick. The temperature Is controlled by an automatic thermostat with temperature setting indicator. b. Procedure: 1) Roll a rectangular (2" x 4") piece of aluminum foil so that It will pass through a ground glass 24/1(0 Joint of the oorroslon test flask. CAUTION: Be careful that after rolling the specimen does not touch Itself at any point. 2) Wash the aluminum foil (Step 1) scrupulously with acetone, distilled water, acetone, benzene, and chloride-free ether. 3) Then place the foil on a clean watoh-glass and dry in an oven at 110C. for 30 min. After cleaning handle the specimen with tongs or forceps only" 4) Weigh accurately on an analytical balanoe 49 MONS 077448 the specimen (Step 3) at room temperature. 5) Drop the weighed aluminum foil into the chloride free corrosion flask of the "Q.E. Corrosion Apparatus." Rinse out flask with sample and rinse end of condenser with sample. 6) Add 200 ml. of the product under test to the aluminum foil (Step 4 and 5). 7) Set the corrosion flask in the corrosion test apparatus . 8) Attach a 12-inch straight-tube air-cooled con denser, the outside of which is painted with aluminum. 9) Cover the exposed part of the flask with aluminum foil. 10) Heat the flask for 6 (+ 0.1) hours at 210 (+ 5) *C. 11) At the end of the heating period, detach condenser from the flask before removing it from the hot plate. 12) Remove the flask from the hot plate and cover all of the flask with aluminum foil (when the flask is not on the hot plate). 13) Without removing the aluminum foil covering of the flask, analyze the product (Step 6) remaining in the corrosion apparatus for: a) Appearance. Color, and Condition. b) Inorganic (Free) Chlorides--Apply Method No. 10,118 o) Acidity (Acid Number) - Pollow Method No. 10,087 14) With a pair of clean, straight nlchrome tongs, remove the aluminum foil specimen (Step 5), wash thoroughly, dry and weigh accurately on an analytical balance in the same manner as before (Steps 2, 3 and 4). Report the oorroslon as loss or gain in weight to the nearest O.OOOl g. and the Chemical Stability, as indi cated by the analysis of the products "After Corrosion Test", in the same way as reported for the original (as received) material. 50 HONS 077449 6. METHOD NO. 10,118, "INOROANIC CHLORIDES." a. Preparation of Standards: 1) Make a primary standard of 100.0 ppm by weighing 0.1648 g. C.P. NaCl into a chloride-free 1 liter volumetric flask. Dilute to the mark and mix thoroughly. Make a 10.0 ppm standard by diluting 100 ml.- of the primary standard to 1 liter, and mixing well. Por every 0.1 ppm standard, dilute to 10 ml. of the 10 ppm standard to one liter and mix well. A 0.1 ppm beam Is considered the very faintest beam perceptible to the eye between 15-45 seconds after adding the AgNO? solution. If the beam Intensity Is not vialbleJat all, or If easily visible (too strong), discard the solutions and make new standards. 2) Weigh 20.0 g. C.P. AgNO? Into a chloride free dark bottle. Add 20 ml. C.P? HNOq (ohlorlde-free). Dilute to 200 ml. with water? 3) All solutions should be freshly prepared every two weeks and stored In glass-stoppered Pyrex bottles. b . Light Source . Employ the 2 battery Penllte flashlight, having a 3-4 mm. light aperture. New batteries must be used frequently In order to perceive beams properly. c. Procedure: 1) Thoroughly rinse two separatory funnels with chloride- free water three or four times. Then take an aliquot from each funnel In a test tube which has been rinsed with ohlorlde-free water. Test these aliquots for Tyndall beams by adding 3-5 drops of AgNO, and allow ing 45 sec. for full beam to evolve. Absolutely no dust or chloride beam should be present. (If beam Is present rinse all equipment with 1:1 HNO? and repeat step 1). 2 2) When funnels are beam-free, drain out all the water except 50 ml. in one and 25 ml. in the other. Heat the water In both funnels to boiling. (Hold stopper while heating as steam may cause stopper to fall.) 3) Transfer 50 ml. of the sample from the sample bottle at a temperature of gS-lOCrC. Into the separatory 51 MONS 077450 funnel containing the 50 ml. of boiling water. (As a precautionary measure, pour some of the sample from the sample bottle Into a waste beaker before adding the 50 ml. to the funnel.) Stopper the funnel and shake vigorously for at least 1 minute, venting frequently through the stopcock. (Care must be exercised at all times to touch neither the lower part of the funnel stem nor the ground part of the stopoock) Allow the layers to separate and drain off the sample Into the aecond funnel containing the 25 ml. of boiling water. (As before, drain off a few ml. of the sample Into a waste beaker before draining the sample Into the aecond separatory funnel.) It may be necessary to heat the sample when transferring the sample to the second funnel; e.g., Aroclor 12o0. Repeat step 4 and allow the layers to separate. Then drain off the sample Into a waste beaker. Combine both water extracts In one funnel and shake thoroughly. Take approximately a 10 ml. aliquot of the water extract out through the bottom of the funnel Into a 3/4" x 6" test tube. Again, first allow a few ml. to drain out before taking the aliquot. (The test tube used should be rinsed with chloride-free water several timeB before using.) Add approximately an equal portion of chloridefree ether. (The ether Is tested by shaking a portion of It with chloride-free water and testing for Tyndall beam at the end of 45 sec. If beam Is present, wash ether several times with chloridefree water until washings show no beam after adding 3-5 drops AgM^). Shake the ether-water mixture until the emulsion In the sample disappears and the water layer is completely beam free before adding AgNO?. If emulsion is difficult to break, add sample dropwise through the ether and then shake. Add 3-5 drops of 10$ AgNOq solution and test for chloride beam for 45 sec .exactly. If no beam Is present at the end of 45 seconds, report ss <0.1 ppm. The very faintest of beams Is considered 0.1 ppm. If beam Is stronger It will be necessary to 52 HCIHS 077451 compare with standards of 0.15, 0.20 up to 1.0 ppm, adding the 3-5 drops of AgNO? and comparing at the end of 45 sec. J * The method of precise to the nearest 0.1 ppm. Report results to the nearest 0.1 ppm. METHOD NO. 10,087, "ACID NUMBER." a. Reagents: 1) Nitration grade benzol. (This may be obtained from reserve samples of benzol which have been analyzed for Depts. 223 and 233) 2) Anhydrous methanol. 3) A saturated solution of phenol red (phenol sulfonphthaleln) In methanol (approx. 0.l). 4) A 0.01 N solution of KOH In methanol. (This solu tion Is prepared by the Service Section). b. Procedure: 1) Place 100 ml. of benzol, 100 ml. of methanol and 0.5 ml. (pipette) of phenol red Indicator Into one of two clean dry 500 ml. Erlenmeyer flasks. 2) Neutralize carefully with the 0.01 N KOH (to be first definite pink color.) 3)' Pour the mixture back and fohth between the two flasks several times. If the solution Is still neutral, divide It equally between the two flasks, If not, repeat steps 2 and 3. 4) Weigh (+ 0.05 g.) Into one of the flasks a 75.0 + 5.0 gT sample and titrate with the 0.01 N, KOH until the sample matches the blank. c. Calculations: Acid No. (mg. KOH/gram Baraple) : ml. 0.01 N KOH x 0.56 Sample Weight Report the results to the nearest 0.001 If they are below 0.1, otherwise to the nearest 0.01. The method la precise to + 0.002 for acid numbers below 53 MONS 077452 0.01 and to + 0.01 in the range of 0.1 to 0.01. NOTE 1; To convert mg. KOH/gram to mg. NaOH/gram, multiply by 0.715. METHOD (MODIFIED) NO. 10,620, "MOISTURE (WATER)". a. Introductory Comment: The Karl Plscher Reagent titration method uaed In the analytical laboraoory Involves use of an analytical balance to weigh accurately about one drop of water used In preparing the standard. Since an analytical balanoe may not be available, the method has been modified and usea a purchased standard water solution as described below. Also, In the laboratory a "Dead Stop" potentlometrlc method for determining the end point Is often used. However, as this equipment may not be available, the procedure described below uses the visual Indicator change for determining the end point. b. Apparatus and Reagents: 1) Karl Plscher Burette, Automatic Pyrex No. 5750, 25 ml. capacity. Ace Olass Company, Vineland, New Jersey. 2) Water Standard In Methanol. No. SO-W-2 (1 ml.: 1 mg. HgO) Plsher Scientific Company, 2800 Jeffer son Avenue, St. Louis, Missouri. 3) Karl Plscher Reagent Solution No. SO-K-2. Plsher Scientific Company. c. Standardization of Karl Plscher Reagent. Into a 500 ml. clean, dry Erlenmeyer flask, place about 100 ml. "Anhydrous" methanol (commercially available, 99.95$). Add Karl Plscher Reagent to this blank until the first color change from lemon yellow. It Is not necessary to read the burette at this point. Carefully pipette 50 ml. of standard water solution into the blanked methanol. Refill the Karl Pisoher burette. Titrate the solution with gentle swirling to mix, until the same color Is obtained as was obtained for the blank. Now read the burette. 54 HONS 077453 Moisture value of K. F. reagent in terms of grams HgO per ml. = (Moisture value of stand- (Ml. Standard H2O solution) (ard water solution in gm. (per ml. stated on label ml. Kan Fischer Reagent " d. Solvent Mixture: Since the solubility of the different askarels variea, the following solvent mixtures are suggested: Material Pyranol 1478 Pyranol 1488 1467 Pyranol 1481 Pyranol 1495 All Aroclors AnhydrouB Benzene 0 ml. 100 ml. 100 ml. 100 ml. 110 ml. Anhydrous Methanol 300 ml. 200 ml. 200 ml. 200 ml. 190 ml. Procedure, "Visual End Point" 1) Place 100-300 ml. of dry solvent mixture (c) In a dry 500 ml. ggs. Erlenmeyer flask. 2) Titrate the solvent with K. F. reagent to the visual endpoint, l.e., the first change from the yellow to reddish orange that persists for 30 seconds . Refill the burette 3) Using a beam balance, weigh to the nearest 0.1 gram by difference, a sample containing 0.03 to 0.06 grams HgO Into the flask. 4) Stopper and shake until the sample is in solution. 5) Titrate the aolution with K. F. reagent to the endpoint described In Step 2. Record the volume of K . F. reagent used. Calculation: % H?0 - ml. of K. F. reagent x HgO factor x 100 Sample Weight References: Mitchell, J. and Smith, D. M., Chemical Analysis, Vol. 5, Aquametry, Interaclence Publishers, Inc., New York, (1948). 55 HONS 077454 CHAPTER 7 TYPICAL PROPERTIES The 1200 series members of the Aroclor family are chlor inated biphenyls, and are made by chlorinating biphenyl to approximately the percentage of chlorine, by weight, indica ted by the last two digits of the serial number. For example, Aroclor 1254 Is approximately 54? chlorine on a weight basis. Accordingly, these Aroclors are not single or simple compounds. They are a mixture of Isomeric compounds composed predominate ly of the chemical compound Indicated below as being their approximate equivalent: Aroclor 1242 Aroclor 1248 Aroclor 1254 Aroclor 1260 Trlohloroblphenyl Tetrachloroblphenyl Pentachloroblphenyl Hexachloroblpheny1 For transformer use and some capacitor use where lower viscosity Is required for better low temperature operation than offered by the above Aroclors, these products are mixed with pour point depressants, particularly trichlorobenzene resulting In various Oeneral Electric Company Pyranols described briefly as follows: Transformer Pyranol 1467* 60? of Aroclor 1260 40? of Elec. Grade Trichloro benzene 0.125? of Tin Tetraphenyl Transformer Pyranol 1470* 45? of Aroclor 1260 55? of Elec. Grade TrlchloroTetrachlorobenzane Mixture 0.125? of Tin Tetraphenyl Use of trl-tetrachlorobenzene mixture and tln-tetraphenyl scavenger Is subject to G.E. patents and license: Royalty arrangements should be checked before using, questions about license concerning the use of anthraqulnone stabilizer for DC capacitors should be referred to Western Electric, 195 Broadway, N. Y. C. 56 MONS 077455 Capacitor Pyranol l48l 755* of Aroclor 1254 255* of Elec. Orade Trlchlorobemene Detailed properties of all of these products are given as follows: AROCLOR 1242 PROPERTY TYPICAL Vise. 9 37.8*C. (ASTM D88) Specific Oravlty 9 25/15.5C (ASTM D287) Color, APHA Condition Acidity, mg. KOH/g. Pour Pt., *C. (ASTM D97) Inorganic Chlorides, ppm. Refractive Index 9 25* C. Distillation Range (ASTM D20) Corrected for stem and barometric pressure Corrosion 82 - 92 seconds Saybolt Universal 1.381 - 1.392 100 max. Clear 0.01 max. -14 or lower 0.10 max. 1.6245 - 1.6265 10% 325*C. min. 90J* 366"C. max. After heating with aluminum for six hours at 210*C + 10*C, the aluminum must not be corroded either on visual or weight in spection and the Aroclor 1242 should meet the following specs: Water Content, ppm Resistivity 100*C. 500 volts DC 9 0.1" gap Dielectric Constant 100*C. 9 1000 cycles (ASTM D924) Plash Point Cleve. OpenCup* Plre Point *C.* Sulfates (ASTM-D117-31)* Fixed chlorine content(Carlus)* Specific Heat 9 25*C. * Evaporation 9 100*C for 6 hrs.* Dielectric Strength (KV) - (ASTM D877) * Color, APHA Acidity, mg.KOH/g. Inorg.Chlorides,ppm Condition 35 max. 150 max. 0.01 max. 0.10 max. Clear 500 x 10^ ohm-cm., min. 4.7 - 4.9 160*C., min. None to boiling point None 41.5 - 42.55* 0.29 0.4j* max. 35 Min. *Not determined unless by special request. 57 HONS 077456 AROCLOR 128 PROPERTY TYPICAL Vise, 9 54.4' C.fASTM D-88) Spec. Oravlty @ 65/15.5'C. (ASTM D-287) Color, APHA Condition Acidity, rag. KOH/g. Pour Point *C. (ASTM D-97) Refractive Index 9 20'C. Distillation Range (ASTM D-20) 73-80, sec. Saybolt Universal 1.404 - 1.414 100 max. Clear 0.01 max. -7 1.630 - 1.631 343 - 373'C. Water Content, ppm. Resistivity 100*C. 500 volts D.C. 9 0.1" gap Dielectric Constant, 100'C. 1000 cycle Dielectric Strength 25*C * Flash Point, (C.O.C.) * Fixed Chlorine (Carius)* Specific Heat 9 25 C.*- 35 500 x 10^ ohm-cm, min. 4.6 4.6 193* C. 47.5 - 48.5* 0.27 Not determined unless by special request. 58 RONS 077457 AROCLOR 1254 PROPERTY TYPICAL Vlso. 9 98.9'C. (ASTM D68) Specific Oravity 9 65/15.5*C. (ASTM D207) Color, APHA Condition Acidity, mg. KOH/g. Pour Pt. C. (ASTM D97) Inorganic Chlorides, ppm. Refractive Index 9 250C. Distillation Range (ASTM D20), Corrected for stem and Barometric pressure Corrosion 44 - 48 secs. Saybolt Universal 1.495 - 1.505 100 max. Clear 0.01 max. .7 - 12 0,10 max. 1.6370 - I.6390 10* 366 - 378C 50* 372 - 383'C. 90* 363 - 396C. After heating with aluminum for 6 hours 9 210*C, plus or minus 10'C, the aluminum must not be corroded either on visual or weight Inspec tion and the Aroclor 1254 should meet the following specifications: Color, APHA 150 max. Acidity, mg.KOH/g. 0.01 max. Free Chlorides, ppm. 0.10 max. Condition Clear Water Content, ppm. 35 max. Resistivity 1004C., 500 v.D.C. 9 0.1" gap 500 x 10^ ohm-cm., min. Dielectric Constant, 100*C 4.15 - 4.35 1000 cycles Dielectric Strength 25*C * 35 KV., min. Bum Point (ASTM D92)* - Higher than 350*C. Sulfates (ASTM D-117-31)* None Plxed Chlorine content (Carlus)* 55 + 0.5* Evaporation 9 100*C. for 6 hrs.* 0.4* max. Stability * There shall be no liberation of chlorine or chlorides when the material Is heated 9 100TC. In glass vessels in contact with air for periods of at least one month. Ageing Characteristics* No loss In resistivity over origin al value on heating In air for 96 hrs. at 100*C. Specific Heat 9 25*C. 0.26 Not determined unless by special request. MONS 077458 59 AROCLOR lg60 PROPERTY TYPICAL Vixc. 9 98.9#C.(ASTM D88) Specific Gravity 9 90*C./l5.5*C (ASTM D287) Color, APHA Condition Acidity, mg. KOH/g. Pour Ft., *C. (ASTM D97) Inorganic chlorides, ppm. Refraotlve Index, 25*C. Distillation Range (ASTM D20) Corrected for stem and barometric pressure. Corrosion 72 - 78 seconds Saybolt Universal 1.555 - 1.566 150 max. Clear 0.01 max. 25 - 3** 0.10 max. ' 1.6455 - 1.6470 10)t 385 - 398'C 50)t 390 - 404'C. 90jt 400 - 420*C. After heating with aluminum for 6 hrs. 210*C. + 10*C., the aluminum must no? be corroded either on visual or weight In spection and the Aroclor 1260 should meet the following specs: Water content, ppm. Resistivity, 100*C. 500 volts 9 0.1" gap Dielectric Strength 50*C.* Dielectric Strength 100"C.* Dielectric Constant 100*C. 1000 cycles* Bum Pt. (ASTM D92)* Sulfates (asTM D117-31)* Fixed chlorine content(Carlus)* Evaporation 9 100*C. for 6 hrs.4 Stability * Specific Heat S 25*C. Color, APHA 150 max. Free Chlorides, ppm. 0.10 max. Acidity, mg.KOH/g. 0.01 max. Condition Clear 35 max. 500 x 10^ ohm-cm. 30 KV., min. 30 KV., min. 3.6 - 3.8 min. Higher than 350*C. None 50 + 0.5* 0.2$ max. There shall be no liberation of ohlorlne or chlorides when the material is heated 9 lOO'C. In a glass vessel In contact with air for periods of at least one month. 0.23 Not determined unless by speoial request. 60 MONS 077459 PVRANOL l48l PROPERTIES TYPICAL Viscosity 9 37.8'c. 70 - 02 secs. Saybolt Universal Spec. Oravlty 9 15.5/15.5*C 1.525 - 1.535 Color, APHA 150 max. Condition Clear Acidity, mg. KOH/g. 0.01 max. Pour Pt., *C. -15 or lower Inorganic Chlorides, ppm. 0.10 max. Refractive Index 9 25C. 1.6205 - 1.6215 Distillation Range - Corrected for stem and barometric pressure First drop 205*C. rain. 2556 max. Below 270"C. 906 380 - 395-C. Corrosion Test - Change In Weight 0.00 Color, APHA 200 max. Acidity, after test, mg. KOH/g. 0.01 max. Free Chlorides, ppm. 0.10 max. Condition, after test Clear Water Content, ppm. 35 max. Resistivity 9 100*C, 500 volts, DC, 0.1" gap rt 100 x 10y ohm-era., min. Dielectric Constant (100'C., 1000 cycles) 4.1 - 4.6 61 HONS 077*60 PYRANOL 1467 PROPERTIES TYPICAL Vise. 0 37.8*C., (ASTM D88) 54 + 2 sec. Saybolt Universal Specific Oravity 9 15.5/15.5`C., (ASTM D-207) 1.560 - 1.568 Color, APHA 150 max. Condition Clear Acidity, mg. KOH/g. 0.01 max. Pour Point, *C. (ASTM D-97) -32*C. or lower Inorganic Chlorides, ppm. 0.10 max. Refractive Index 9 25*C. Distillation Range (ASTM D20) 1.6137 - 1.6147 1st drop - 200C. min. Corrected for stem and Below 270*C. - 40* max. barometric pressure Corrosion 90* - 395 - 4l5*C After heating with aluminum for 6 hrs. at 200-220C., the aluminum must not be corroded either on visual or weight in spection and the Pyranol should meet the following Specifications: Color, APHA 200 max. Acidity,mg.KQH/g. 0.01 max. Inorganic Chiorides,ppm. 5 max. Condition Clear Water Content, ppm. 30 max. Resistivity, 100'C. 500 volts, 0.1" gap 100 x 10^ ohm-cm., min. Dielectric Strength, 25*C. 35 KV., min. Dielectric Constant, 100*C., 1000 cycles* 3.7 - 4.0 Tin Tetraphenyl* 0.125* + 0.01* by weight Burn Point, (ASTM D92)* None up~to Bolling Point Fixed Chlorine* 59.1* min. Arc Formed Oases* Less than 1.0* (Oxygen Free Liquid 9 25*C.) Total eombustlble gases including carbon monoxide, hydrogen and volatile hydro carbons . Not determined unless by special request. 62 MCNS 077461 PYRANOL 1470 PROPERTIES TYPICAL Vise. 9 37.8'C. (ASTM D88) 41-45 Sec. Saybolt Universal Spec. Gravity 9 15.5/15.5*0., (ASTM DS87) 1.563 - 1.571 Color, APHA 150 max. Condition Clear Acidity, mg. KOH/g. 0.01 max. Pour Pt., TC., (ASTM D97) -44C., or lower Inorganic Chlorides, ppm. 0.10 max. Refractive Index 9 25C. 1.6075 - 1.6085 Distillation Range (ASTM D20) Corrected for stem and barometric pressure First drop 210*C., min. 3556 238 - 255'C. 55* 275 - 345C. 65* 380 - 4C0"C. 95* Corrosion 390 - 4l5'c. After heating with aluminum for 6 hrs. 9 200-220*C., the aluminum must not be corroded either on visual, or weight Inspection and the Pyranol should meet the following specificatIons: Color, APHA 200 max. Acidity, mg.KOH/g. 0.01 max. Inorg. Chlorides, ppm. 5 max. Condition Clear Water Content, ppm. 30 max. Resistivity, 100'C., 500 v., 0.1" gap 100 x 10? ohm-cm., min. Dielectric Strength, 25*C. 35 KV., min. Dielectric Constant, 100*C,, 1000 cycles* 3.8 - 4.3 Tin Tetraphenyl* 0.125* 0.01* by weight Burn Point, (ASTM D92)* None up to Bolling Point Fixed Chlorine* Arc Formed Oases* 60.5 + 0.5 Less than 1,0* (Oxygen Free Liquid 9 25*C.) Total combustible gases In cluding carbon monoxide, hydro gen and volatile hydrocarbons. Electrical Stability* After heating for 96 hrs. 9 100'C In a closed container, the resis tivity should not decrease more than 10*. Not determined unless by special request. 63 HONS Q77<*62 CHAPTER 8 EARTH TREATMENT OP AROCLOR IN THE ELECTRICAL INDUSTRY PRIOR TO USE. Aroclora and their mixtures supplied to the electrical industry must conform with most strict requirements specifi ed by the Industry as shown In Chapter 7. Since these products are sensitive to contamination from traces of Impurities, they require careful handling In the industry when sampling or storing or using the materials to Impregnate capacitors or fill transformers. Comnon oontamlnants to be avoided include moisture, lonizable Impurities, metallic Impurities, such as rust or corrosion products from storage and handling equipment, and contaminants suoh as oils (mineral oils), lubricating oils or greases common ly used In equipment or other processes In the electrical Industry. Care must be taken to avoid contamination from contact with Improper gaskets or packing materials. Including natural and synthetic rubber and moat plastic exclusive of certain silicones and Teflon; rosin solder fluxes, etc. may also Intro duce traoes of deleterious Impurities. Die dielectrics are also susceptible to the harmful aotion of ultra-violet light and, therefore, exposure to direct sunlight should be avoided. The adverse effect of lonlzable Impurities Is especially pronounced In the low viscosity Aroclora suoh as Aroclor 1242 64 MCNS 077463 or Aroclor mixtures such as Pyranol 1481. In the case of more viscous fluids, such as Aroclor 1254, the ionizable impurities are not so free to move about in the fluid and, consequently, the more viscous fluids can be handled with less oare than required for the thinner fluids. This 1b especially pertinent in capacitor manufacturing. When using the thinner type Aroclors to make capacitors that offer superior low temperature operation, the following types of trace contamination affecting the electrical properties of the dielectric have been experienced, Occasional droplets of perspiration from operators, when winding the capacitor cores, have fallen onto the paper causing contamination in the finished units. Small amounts of Glyptal resin and simi lar sealing compounds used to seal tiny leaks in the vacuum Impregnating equipment or storage tanks have caused contamina tion. Alse, small amounts of mineral oil entering the system have caused similar trouble. A small droplet of any of these materials in one or several liters of the thinner type fluids results in noticeable contamination, whereas it may not have as much adverse effect on the more viscous dielectrics. To be certain that the fluids are free from traces of contamination, it is standard practloe to treat them with con ditioned diatomaceous earth and then to filter immediately be fore use. Treatment with this earth by removing trace contam inants results in "up-grading" the electrical values, e.g., 65 HONS Olios'* the volume-reslstlvlty may be brought up considerably beyond the specification minimum or the normal values of the dielectric as received. Likewise, Improvement In power faotor may be accom plished. The earth treatment recommended for use by the electrical manufacturers is qualitatively the same as used In the produc tion of the Aroclors and their preparation for shipment to the electrical Industry. Treatment of the Aroclors with earth by the electrical manufacturers Is a step required to assure that traces of Impurity or contamination that may have been Introduced during storage or handling In the electrical Indus try have been removed and that maximum electrloal values have been attained Immediately before the dielectric Is Introduced Into capacitors or transformers. It is Impractical for the manufacturer to furnish these dielectrics to the customer at the maximum attainable electri cal qualities because even with careful packaging, shipping, sampling and handling In the electrical Industry, these fluids may easily pick up traces of oontamlnants from opened tankcars, drums, pipe line, pumps, etc. However, as supplied according to the specifications, the fluids are readily "up-graded" by the earth treatment. The type of dlatomaceous earth used Is known as Fuller's Earth, supplied by the Florldln Earth Company, Warren, Pennsyl vania, or the Attapulgus Division, Mineral It Chemicals Corp. of Amerloa, 210 West Washington Square, Philadelphia 5, Pa., 66 MCNS 077465 or their equivalent. Usually a minus 200 mesh size, regular volatile. Is used and the quality should be specified as for use by the electrical Industry. (Code 73122) Hie earth as received needs to be conditioned and acti vated, after which It should be stored only a minimum length of time (about a day at the most) and In hermetically sealed containers, prior to use. It Is desirable that the earth be used Immediately after It has been aotlvated. Activation should be done by heating the earth contained In stainless steel shallow trays for four hourB at 400 C. in a muffle furnace. If a muffle furnace Is not available or the capacity by this method may not be great enough, the earth can be activated by heating at least twelve hours In an elec trically heated oven at 250 C. Another method used Is to pan dry and activate by heating at 100 C. and using a strong vaouum, about 6 on. of mercury. This latter method is used In connection with transformer work and the former methods are usually used for capacitor work. In the place of pan drying, rotary driers may be used but their action should not be so severe as to break the earth par ticles to the extent of producing powder which Is difficult to handle In the subsequent filtering operations. It Is the consensus that the earth should not be heated above 400 C. as this may cause collapse of the particles. 67 HONS 077466 The amount of earth used la usually O.ljf to 0.3 based on the weight of the fluid. Larger amounts of earth can be ueed If the fluid Is oompoaed of only Aroolor or a mixture of Aroclor and chlorinated benzene or other pour point depressants. However, larger amounts of highly active earth. In the range of 2% or 356, would be expected to selectively adsorb scavengers or stabilizers from the fluids containing these additives. This Is especially of concern In handling the transformer fluids which usually contain scavengers suoh as tin tetraphenyl. For transformer work it Is suggested that the earth be condi tioned and mildly activated by heating it at 100 C. under vacuum, about 6 mm. of mercwy. Not more than about 0.1% of earth based on the total weight of the transformer fluid should be used. For treatment with earth, the fluid is put Into a suitable tank fitted with an agitator, heating coll, and a oover. The proper amount of freshly conditioned earth Is added and the mixture Is agitated thoroughly and heated for about four hours. The more viscous dielectrics such as Aroclors 1248 and 1234 are heated at about 70 to 80 C. (158 to 176 F.) and the less viscous materials suoh as Aroclor 1242 and Fyranols 1481, 1467, and 1470 are heated at about 50 to 60 C. (122 to 140F.). After about four hours contact the material is filtered through a Sparkler or Sweetland or a comparable filter press previously fitted with filter paper liners such as supplied by 68 MGNS 077*67 Carl Schleicher and Schuel Co., Inc., 116 West 14th Street, New York, N. Y. The paper la usually 25 mils thick and must be dried at 100* C, to remove moisture, prior to use In the filter press. The filtered dleleotrio material is then ready for Impregnating capacitors or filling transformers. In some cases, especially for AC capacitor work where the dielectric does not require addition of stabilizers and ac cordingly there is no danger of removing such additives by repeated earth treatment, good practice is to use continuous earth treating, circulation and filtration with constant read ing of the resistivity of the filtered dielectric. In Chapters 1 and 2 selection of proper materials of construction for the tankcars and storage tanks was discussed. It Is equally important to seleot proper materials of construc tion for the processing tanks used In the capacitor and trans former Industries and also for the impregnating chambers used In making oapaoltors. It is preferable that this equipment be made of stainless steel or aluminum, or. If It Is of steel construction, the Interior should be either zlnc-tln metallized or aluminum lined. While Iron or steel equipment Is not regarded as desirable for handling the fluids, this type of construction Is used In some of the plants. Here the possibilities of rusting or corrosion cannot be overlooked. If the equipment Is kept free from water and If a film of clean dielectric adheres to the . 69 MQNS 017A68 surface of the metal, e.g., when the tanks are empty, then satisfactory operation can be experienced. However, a number of factors must be kept In mind and to cite an example, reference is made to the Impregnation of capa citors by the chamber method. The moisture content of the paper uBed In the capacitor cores may easily Introduce several gallons of water Into the average Impregnating chamber. This water is removed from the capacitors prior to Impregnation - usually by heating the chamber to about 130s C. under efficient vacuum, 100 microns or less. If the chamber Is not made of the preferred materials of construction, slight corrosion may ocour and the film of fluid on the Interior surface of the tank may be contaminated and In turn Introduce traoes of Impurities Into the treated and clean dielectric subsequently Introduced Into the ohamber for Impregnating the capacitors. In fact, because of this possibility of contamination. In some operations the capacitors are conditioned and dried preparatory to Impreg nation in a separate oven or chamber and when thoroughly dried they are then transferred Into a second chamber used for Impreg nation. In the case of relatively large size capacitors, such as power factor correction units, a manifold pipe system may be used to handle each unit Individually rather than by the batch-chamber method. The unimpregnated capacitors are placed Into an oven and vacuum Is applied to the Individual units attached to the manifold. 70 HONS 0 7 7469 When conditioned and dry, the dielectric la Introduced into the unit through the manifold. Care must be taken that moist air or contaminants do not collect In the branch through which the dielectric Is Introduced. In addition to removing moisture, another purpose of the heat and vacuum conditioning treatment given the capacitor units prior to Impregnation is to remove traces of Impurities such as residual solvent from the metal cleaning operations and from solder flux, eto. The fluid Is Introduced hot Into the evacuated capacitor units. Die more vlsoous Aroolors, such as 1248 and 1234, are usually Impregnated at 83* to 130* C. The less viscous and more volatile dielectrics such as Aroclor 1242 and mix tures of Aroclor with chlorinated benzene may be introduced best at lower temperatures -- about 30* C. optimum, 60* maximum. Table IV indicates desirable minimum resistivity values of the dielectric materials when earth treated and ready for capacitor Impregnation and similar values of the material following the process. TABLE IV Dleleotrlc Aroclor 1254 Aroelor 1242 Pyranol 1481 Volume Resistivity Ohm-cm at 100* C. and 500 volts DC. Prior to After Impregnation Impregnation 2,500x10s 1,500x10? 600xl09 500 500 x x 10 10 9 9 400 x 109 71 MQNS 077470 In the caae of new and freshly filled transformers using Aroolor dielectric mixtures, it seems reasonable that the power factor of a sample of the fluid drawn from the trans former should be In the range of about 5 to 12 percent, measured at 60 cycles and 100* C. With field service of the transformer the power factor value Is expected to Increase somewhat. However, such a power factor Increase alone does not seem to have harmful effect on the operation of the transformer. A more usual measurement used for transformer fluid la volume-reslstlvlty. This value of the new dielectric prior to filling the transformer should be about 500 x 10 ohm-cm at 1,000 cycles and 100* C. The similar value of the fluid taken from a new transformer should be at least, about, 50 x 10 ohm-cm and no lower than 25 x 109 ohm-cm. With long field service volume-reslstlvlty values de crease somewhat but seem to level off around 10 x 10 ohm-cm, with satisfactory transformer operation. However, If the volume-reslstlvlty of the fluid falls below 10 x 10 ohm-cm, the matter should be looked Into. 72 HONS 077471 CHAPTER 9 DERMATOLOGY AMD TOXICOLOGY Skin patch teats using Aroclor 1254 (biphenyl Chlorinated to the extent of 54 by weight) applied to gauze and placed In contact with the skin showed no primary Irritancy or sen sitization. The tests were conducted under competent medical supervision and the standard procedure recommended by Drs. Louis Schwartz and Samuel M. Peck, Reprint No. 2552, Public Health Reports, Vol. 59, No. 19 (April 28, 1944) was used. If Aroclors are spilled on the skin, the skin should be washed In the usual manner with soap solutions. If accidental burns oocur from contact with hot Aroclors, the bum should be treated the same as any ordinary burn. Aroclor adhering to the burned area need not be removed Immediately unless treatment of the burn demands It, In which case use soap and water or repeated washings with a vegetable oil. At ordinary temperatures Aroclors have not presented Industrial toxicological problems. If Aroclors are used at elevated tempenatures In open systems, methods must be designed to exhaust any vapors arising. Experimental work on animals Indicates that the maximum safe concentrations of vapors In workrooms la In the range of 0.5 to 1.0 milligram per cubic meter of air. This applies to all of the liquid Aroclors. Laboratory technique merely requires keeping the hands 73 MOMS 0 7 74 72 free of the liquid and handling It under a well ventilated hood. Localized or spot ventilation together with general work room exhaust le recommended for plant operations. When sampling tank cars, canvas gloves and safety glasses or goggles should be worn. No special clothing le required, but the worker's garments should be laundered at least weekly and ohanged In case Aroclor or Aroclor mixtures Is spilled on the olothes accidentally. If workmen are exposed to Aroclor vapors at relatively high levels, as may be the case when opening a heated capacitor Impregnating chamber, a respirator should be worn during these short Intervals. The many years of satisfactory and safe use of Aroclors and their mixtures with chlorinated benzenes In the electrical Industry for impregnating oapaeltora and filling transformers has demonstrated the Industry's ability to handle these fluids without hazard to the workmen. It Is a simple matter and In line with good "housekeeping" and personal cleanliness to exercize the suggested and required precautions In all cases. 74 HONS 077473 PPHapwpnpaavp -it* _ S^n * * I * a# ? f.-^JSf SitS. 5''..ijrsi, ''. | _ S'jM'T-* **7* * x-4 fe* ri * mr-SRs:*:--.^y: s, .L_ 1 r^a ** . : -r'js^ei8;-.4. * "~ ft*? g-~g---v igsggagg T^:jiaiMrai3MKf..^-.T 1 *0*S 077474 HGNS 077*75 MOMS 077477 HOMS 077479 HONS 077480