Document DBR8DxpVjqkv6Yvr6bLV4xOd
JENNAT CORPORATION
A HUBLDIABT or UNION CARBIBK CORPORATION
Quality EmuLion IPolymeit
12840 SOUTH CRAWFORD AVENUE
ALSIP, ILLINOIS 60658
Chicago 928*4100
Suburban 389-7000
UCAR 874-HS SUMMARY PROCEDURE
1. Charge monomers to mix tank in order shown and circulate while charging.
2. Set up for addition of monomer through the steam inlet, below the liquid surface.
3. Close reactor drain and charge hot W-2V. Turn agitator on at 50 rpm.
4. Charge B-71, dry to reactor. 5. Adjust reactor temperature to 79*C. Allow 5 to 10 minutes to line out at 79*C.
6. Charge C-57, dry to reactor.
7. Two minutes after C-57 is in, start monomer feed at 4.0 gallons per minute, for 30 minutes.
8. As reactor temperature increases, crack jacket cooling valve to maintain
80-81#C. This usually requires a 40 to 44*C jacket cooling
water return.
9. Increase the feed rate to 7.0 to 7.5 gpm (about 60% on flow controlling temperature at 00-81*C.
meter) while
10. Increase the agitation as follows:
1000 gallons feed, up to 59 rpm
1500 gallons feed, up to 60 rpm
11. After 900 gal. of feed start delayed catalyst feed.
12. During the latter stages of the run, slow the feed rate as necessary to maintain 80-81*C reaction temperature* Jacket cooling return is usually 20 to 25*C at this point.
13. When monomer is all in, rinse the mix tank with 15 gallons M-M and pump to the reactor, unless another "800" series latex follows*
14. Hold at 80-85*C for thirty minutes, post heat.
15. Transfer to cooling tank and cool to 60*C, use Wilden Pump with portable straine
16. Prepare C-56 - W-21 emulsion by mixing in a 10 gallon container. Slowly add the mixture to the cooling tank by dipping from the container with a 1 gallon jug.
17. Prepare R-231 solution in M-8 tank, and feed to the cooling tank over a 30 minute period. Note cooling tank temperature before and after R-23I addition Flush M-8 tank with 3 gallons W-21.
If U-874HS is to be made into UCAR-1531 OMIT U-874HS step 18
and refer to UCAR-153 Seminary Procedure. 18. Cool batch to 25C. Add 40 lbs. Rapol Defoamer, sample to lab.
UCC 025336
*22864
CODE UCAR Latex 874-HS
POUNDS 22,400
3 ill eh i !o;______
Maieri ai : UCAfl LATEX 153
T ank:
________ _____
Operator: __ _______________
Date: GALLONS
___________
-- -
--1 r
CHOKED j
i t
i
i
oo
UN
CN
W-21 Adjustment Sakclite Ink Resin "M-3" 0-149 Rapol (Premix)
4 Drums Code T-104
40
r, .. ___________ !|
1 .|
. 1!
W-21 (Premix) - ' -- - 1 > 1 ..... 1 --
- ' 11
C -------------------------- ---------f
Surrgnary Procedure
1. Prepare UCAR Latex 874-HS. (Refer to UCAR 374-HS Summary Procedure.)
2. Procede to step 16, transfer to cooling tank (? 80-85C. Turn cooling off.
3. Procede through steps 17 and 18, (addition of post catalyst system.) $ 70-75C.
4. Hold at approximately 70C for 15 minutes, sample to Lab. Add 250 lbs. W-31 to cooling tank.
5. Cool to 55 to 60C. Turn cooling off,
6. Add 40 pounds Rapol (D-149) in 5 gallons VJ-21, slowly. This must be added before the A-3 Ink Resin.
7- Add 1.-21 adjustment as per lab instructions.
.
8. Set agitator on ;iHiqh Speed".
..
9* Pump in the "Bakel'ite M~3M resin slowly. This must be added over a one hour period. Fast addition produc.-rc seeds Loo high to filter out.
10. Mix one hour at 53 to 55C. Use 4 drums H-3 ink tlesin -,(;ode T-104
11. Cool to 35C and add 5-0 lbs. F-225 in 3 gal. water.
1?, :
to hob.
.
P-11 7/23/75
UCC 025337
I
W21 HOT _
COLD STEW TOTAL
9 27 11 30 1010
UCAf; 879-HS
Batch Nb. Date: Reactor
CODE
POUNDS
GALLONS
CHECKED BY
M-ll Mi >: Tank
RCULATE WHILE CHARGING
M-13 " M-16 "
" "
W-21 "
"
L-77 "
M-6 O M-11
" "
" (Silicone) " "
1300 256 175
30 1 Full Gal. 75 232
1300 1607
W-21 Hot to Reactor
c0l-c B-71 Dry H<zi W-21 30 Gal-Steam Cond.
cc
- - C-57
867 17
' 30 67
867
W-21 Cold Cat TK C-57
30 30 5
W-21 Cold Mix TK. Flush C-56 W-21 Cold
35
15 45 5 50
R-23I
23
W-21 Hot
20 887
Post Add F-225
5
W-21 Cold
3 53 122666--------
W-21 Hot Hx Flush
20 907
--
_ ______ ....
.
No t e: OK to substitute M-7 for H-13 if M-13 not available - use 219 lbs.
UCC 025338
11-7-75