Tho Aroclor* dielectrics are a range of chlorinated diphenyls pro duced by Monsanto for tho manufacture of impregnated paper capacitors. These products are generically known as `askarele', that is, synthetic fire resistant insulating liquids which, if decomposed by an electric arc, evolve only non-explosive gaseous mixtures.
The Aroclor liquids were first used in the United States in 1931 and to-day they are extensively used in the capacitor Industry throughout the world. Monsanto has been producing Aroclor at its Newport plant since 1951.
There are three grades of Aroclor, identified by their code numbers:
Aroclor 1242 (Commercially known as Trichlorodiphenyl) the most
. economically attractive, is essential for outdoor capacitors in a low
temperature environment, but is the most difficult to handle
in production.
'
Aroclor 1248 (Commercially known as Tetrachlorodiphenyl) is a
compromise between the economic advantages of 1242 and the ease
of handling of 1254.
.
`
Aroclor 1284 (Commercially known as Pentaohlorodiplienyl) is tho easiest to handle in production and is sometimes chosen for capacitors to operate in exceptionally hot environments, but does not gain the maximum economic advantage.
Advantages of using Aroclor Reduced size capacitors are possible for a givon rating; fluorescent lighting units are a particular application in which this is utilised.
Reduced raw material cost arising from tho smaller quantity of paper and foil needed in manufacture.
Aroclor is a Registered Trado Mark.
**I628 3
TOWOLDMONOQ26269
m'
(Kqotm
INTRODUCTION '
Tho Advantages of Aroclor
PROPERTIES
Composition Physical Properties
Viscosity Vapour Pressure Chemical Properties Electrical Properties Permittivity Loss Tangent D.C. Resistivity
CONSTRUCTION OF AROCLOR CAPACITORS
Paper
Assembly of Capacitors
PRODUCTION OF AROCLOR CAPACITORS
Earth Treatment Impregnation
'
PERFORMANCE OF AROCLOR CAPACITORS
A.C. Capacitors D.C. Capacitors
TOXICITY AND HANDLING PRECAUTIONS
K 17 17
18 18 18
20 20 20
APPENDIX A
Laboratory Measurements on Aroclor
APPENDIX B
Compatibility Testing Method
23
0221b*9
i wn; who
TOWOLDMONOQ26270
Reduced labour content becauso of the fewer windings required. Increased through-put from a given plant capacity With existing labour force. Higher stress operation of capacitors Is possible because of a more uniform permittivity in the capacitor. Longer lifo capacitors are produced because of the high stability and resistance to oxidation of Aroclor. Small fire hazard because Aroclor is fire-resistant.
0221630 4
TOWOLDMON0026271
'Values for the most Important properties of the Aroclor dielectrics
are given in the Table.
.
Typical properties of the Aroclor dielectrics
(These values do not constitute a specification)
Property
Aroclor 1242
Aroclor 1248
Aroclor 1254
Relative Density at 20/20C
Pour Point ( C)
Viscosity at 80eC (cS)
Coefficient of expansion *C
Specific heat at 75*C (Jig *C)
Thermal conductivity at 75*0 (W/m *C)
Evaporation loss (%) <2 h at 125C)
Flash Point (*C) ASTM D93/62
Fire Point
Refractive Index n
Inorganic chlorides (ppm) ..
.
Acid number (mgKOH/g)
Water content (ppm)
Permittivity at 20'C and 50 c/s
Permittivity at 1009C and 50 c/s
Loss tangent at 100T and 50 c/s
D.C. resistivity at 100C and 500 V/mm
after 1 min. electricification (T ft cm)
Dielectric strength at 2Q9C (kV)
(B.S. 148:1959)
1-385 -19 35 0-00068 1-24 0-1039 012 154 (min) None 3-6240 01 (max) 0 01 (max) 85 (max) 697 483 0018
1-456 -7 62 000070 1-16 01003 007 154 (min) Nono 1-6295 0-1 (max) 0-01 (max) 35 (max) 658 467 0015
1-549 410 102 000066 108 0-09743 003 204 (min) None 1-6370 01 (max) 0 01 (max) 35 (max) 604 4-25 0010
60 60 (min)
70 60 (min)
80 70 (min)
0221631
Composition Aroclor is made by the chlorination of diphenyl to predetermined chlorine contents which are indicated as a percentage by the last two digits in thocode number e.g. Aroclor 1218 oontains 48 % chlorino by weight. Each Aroclor contains a range of Chlorodiphenyls with differing numbers of hydrogen atoms substituted by chlorine, and in each of these chlorodiphenyls thcro is abundant isomerism,
Physical properties Viscosity The viscosity-temperature characteristics of tlio Aroclor liquids aro shown in Figure 1. It can bo seen that Aroclor 12^1 is tho most viscous at all temporatures and Aroclor 1242 tho least. Tho differences betweon tho three grades aro greatest at lower tympora-
t,
TOWOLDMONOQ26272
turo and bccomo less as the temperature is raised, As previously explained, Aroclor consists of a number of homoloffuos and conse quently each grade does not have a sharply defined molting point, but remains liquid over a wide temperature range, Instead, their viscosities increase smoothly but sharply as the temperature is reduced. Aroclor 1212 has the lowest pour point of all three grades.
Vapour pressure It can be seen that Aroclor 1242 has the greatest vapour pressure at a given temperature and Aroclor 1254 the least, and this needs to be considered when deciding the temperature of Aroclor during degasification and impregnation. The vapour pres sure of Aroclor varies with absolute temperature according to the usual logarithmic law. The variation of the vapour pressures of the Aroclor dielectrics with temperature is Shown in Figure 2.
Chemical properties The chemical inertness of Aroclor is outstanding. The liquids are not oxidised by exposure to air or oxygen even under extreme condi tions of temperature and pressure, nor do they react With moisture. When subjected to a bomb test at 140'C in oxygen at a pressure of 250 p.s.i.g. (17 kg,'em*), there was no evidence of oxidatioh as Judged by development of acidity or formation of sludge. They Can withstand many years of service in electrical equipment at high temperatures without oxidation.
Aroclor is manufactured to a rigid specification ensuring a low Initial value for free acidity and free chlorides. Tests have shown that these low values are maintained even when the liquids are heated for prolonged periods in the presence of air and moisture at temperatures of 100'C.
Aroclor 1242 is slightly sensitive to ultra-violet light, which can result in the formation of traces of ionic contaminants. Tho other grades are relatively unaffected by exposure to light.
Aroclor undergoes no decomposition at temperatures up to 175 C. At much higher temperatures, or when subjected to arcs, the prin cipal decomposition products are carbon ahd hydrogon elilorido.
Laboratory tests and practical experience have shown that phosgene,
chlorine, or hydrocarbons are not formed as decomposition products of
Aroclor.
.
0221632
Electrical properties The laboratory methods used to moasure the electrical properties of the Aroclor dielectrics aro described in Appendix A. 1
Permittivity (Dielectric 'constan!')Tho pormittivity of Aroclor is high er than that of mineral oil, which accounts for the site reduction
iI 6
TOWOLDMONOQ26273
and increasoin stress that is possible. Stresses of 15 to 17 V/pm are common with Aroclor and higher values aro reported.
Since chlorinated diphenyls are polar compounds, their permittivi
ties are highly temperature-dependent. This is illustrated in the
upper part of Figure 4, which shows the variation with temperature
of the permittivity of each of the three grades of Aroclor. These
readings were taken at a frequency of 50 c,'s and an electric Btress of
1 V/nm.
,
'At the lowest temperatures, all three grades have a permittivity of about 2-8, since, because of the very high viscosity, there is no con tribution from dipole orientation polarizability. As the temperature is increased, the permittivity begins to increase when the viscosity becomes sufficiently reduced to allow the molecular dipoles to orientate themselves in the alternating electric field. The tempera ture at which this increase in permittivity begins is dependent upon both the grade of Aroclor, being lowest for Aroclor 1242, and the frequency of the applied field.
As the temperature is further increased, the permittivity passes through a maximum, and then decreases. This "decrease in permit tivity with increase of temperature is due mainly to the disturbance of the alignment of the dipoles by thermal agitation. The maximum permittivities attained vary with the grade of Aroclor, being great est for Aroclor 1242 and least for Aroclor 1254. With Aroclor 1242 the permittivity of this series reaches a maximum, and a further reduc tion in chlorine content causes a reduction in permittivity, as shown in Figure 3."
A1 though tlio permittivity ofAroclor1242 is ofa high order .continued research on these products has revealed the possibility of obtaining even higher permittivities with this class of material. It ip likely therefore, that the final word has not been written on this subject and that improved products will become available in this fiold in the course of the next few years.
022X633
Loss 1'angenl The loss tangent, or power factor, of Aroclor is also highly temperature dependent. This is illustrated in the lower part of Figuro 4, which shows how the loss tangents plotted here on a logarithmic scalo of each of the three grades of Aroclor vary with temperature.
Tho curve for each grade of Aroclor consists of a peak due to absorp tion associated with tho transition in permittivity, followed by a region whoro the loss tangent steadily increases with temperature. In this latter region, tho loss tangent follows tho increaso in fluidity with increasing tomporaturo and is highly dependent upon tho purity of tho Aroclor. Tho tomporaturo at which tho peak ocours is about 19 ' bolow tho pour point.
TOWOLDMONOQ26274
* I 111 'I I *
V` ?
I ;i
Tho loss tangent of Aroclor is greater than that of fresh mineral oil, but by seloction of a paper of lower density tho los? tangent of tho impregnated capacitor can be minimised without sacrificing tho economic advantages. Furthermore, the internal tetnporaturo does not rise beyond acceptable values.
D.C. Resistivity The values quoted in the table are typical for Aroclor as produced, but they can be improved by vacuum dehydration and values of 20 to 60 T ft cm at 100'C are common. The values for Aroclor 1212 and 1248 are lower than 1254 because a given amount of contamination reduces the d.c. resistivity more With a liquid of lower viscosity and higher permittivity.
The variation of the d.c. resistivity of the 3 grades of Aroclor with
temperature is shown in Figure 5.
ill
022163*
TOWOLDMONOQ26275
f.
;: ; vI
'V >
ii-ji
! !.'*ti,
i.j i'
t:
i\
*l
9
TOWOLDMONOQ26276
02Z1635
PERHITT1YITT
TOWOLDMON0026279
i
! I. I
)I
!? i i,
TOUJME REJISTrTITT ( T A tn )
TOWOLDMON0026281
.,
Tho pormlttiwlty of papor Impregnated with Aroclor
TOWOLDMONOQ26282
TOWOLDMONOQ26283
CONSTRUCTION OF AROCLOR CAPACITORS
Paper Kraft paper Is strongly recommended since It has nearly 5 times the acid neutralising properties of rag tissue.
The permittivity of impregnated paper depends upon the density of tho paper as well as the permittivity of the impregnant. This rela tionship Is shown if Figure 6 for the 3 grades of Arocjor and for mineral oil, the values being calculated at a temperature of 20C. Since paper impregnated with Aroclor 1242 has the highest per mittivity, the least area of windings is needed to obtain a given value of capacitance and the greatest economy is obtained.
It is advantageous to use low density paper Since it has been shown both theoretically and practically that such paper gives the least , dielectric loss in a capacitor. This effect arises from the distribution of electrical stress between the cellulose fibres and the impregnant and is in addition to, and independent of, apy losses in t}ie impreg nant itself.
Most manufacturers of capacitor tissue are familiar with Aroclor and have developed suitable grades for use with it.
Assembly of capacitors It cannot be emphasised too strongly that every material that comes into contact with Aroclor must be carefully checked for compati bility. Aroclor is a good solvent for many thermoplastics and elastomers and the resulting solution has a high dielectric loss tangent. Materials which must be considered include the major insulation, tho lead-through insulators, any means of scaling the container and tho residues from tho manufacturing process e.g. fluxes left after soldering.
Tho windings should bo sealed with a suitable adhesive such as gum arable or Gloy. Connection tags if of copper should bo tinned, other wise stainless steel can bo used. Soldering should bo kept to a minimum and whero possible tho special cored solders which have been developed by manufacturers for uso with Aroclor should bo employed. Opaquo bushings must bo used because of tho slight light sonsltivity of somo grades of Aroclor, particularly Aroclor 1242.
TOWOLDMONOQ26284
o22 1 b ^
PRODUCTION OF AROCIOR CAPACITORS
Although tho production of Aroclor impregnated capacitors is generally similar to that of oil impregnated units, and similar plant may be used, there are several differences in detail And these are described in the following sections.
If an oil plant is to be changed to Aroclor, no special cleaning is necessary, although it is advisable to rinse the plant first with Aroclor which is subsequently discarded. It must be noted at this point and always borne in mind that Aroclor has a very Considerable detergent effect. That is to say that since the density is pearly twice that of oil, any dirt existing in the system will be washed out due to the greater density effect of the Aroclor.
Earth treatment The main difference between Aroclor and oil capacitor impregnation
. plant is the earth treatment section. Aroclor, as received in drums,
is suitable for filling into capacitors after vacuum treatment but it
is generally advisable to have an earth treating facility available to
treat any Aroclor which could become contaminated during tho
process cycle. For example if capacitors are filled by a flooding
techniquo, then Aroclor which is unused and which is returned to
the system will be found to be slightly contaminated and earth
treatment is advised. For this to be fully appreciated, it must be
realised that the Aroclor liquids are more susceptible to contami na
tion than their mineral oil counterpart. Because of their higher
solvent action and higher permittivity, the contamination level
which would be acceptable in mineral oil and which is commonly
encountered in an impregnation plant will bo unacceptable for
Aroclor. The earth treatment can be carried out in two principal
ways. In the first place tho earth is contained in a column and the
liquid is circulated until the contamination is removed. Alterna
tively, activated earth is added to tho liquid in a container and it is
stirred to ensuro intimate mixing and then the earth is filtered
through a normal paper filter. In both cases either Fullor's Earth or
Alumina may be used and each must bo activated. It has been found
by experience in laboratory tests that tho earth may bo over
activated and tho optimum temperature is about 150'C for 6 hours.
If this is then added in quantities to tho material to bo treated, it is
0221644
onsured that tho fresh activated earth is used each tlmo and tho
--
TOWOLDMONOQ26285
treatment may bo more easily controlled In this way In the mixing technique. However, there still exists tho problom of separating the earth and here tho column technique has a considerable advantage, since circulation through the column does not necessitate further filtration. This method has the disadvantage that the column gradually becomes less active during its life and there is not always tho same degree of control over the treatment process.
Impregnation it is customary to store the capacitor liquid in a large tank the size , of which depends on whether the material is delivered in drums or tankers. It is strongly recommended that these storage tanks be lagged and heated since at low temperatures difficulty would be
, encountered in pumping the Aroclor 1254 and in certain extremes of temperature even Aroclor 1242 can become unpumpable. After transfer from the storage tank the liquid is first earth treated and mixed with any unused liquid drawn back from the capacitor impregnation tank, if applicable. The treated liquid is then sub jected to vacuum drying and de-gassing in exactly the same way as with mineral oil and after this process it is passed to the final storage vessel where it is held before being passed to the impregna tion section. Aroclor capacitors may be vacuum impregnated by a manifold technique in which the liquid is piped individually to each capacitor can and this is perhaps more editable for the larger power factor correction capacitors. Alternatively, they map be filled by a flooding technique which is more applicable to the smaller fluores cent lighting capacitors. Here the capacitors can be loaded in wire cages and completely immersed in the liquid in the samo way as with mineral oil. For the actual impregnation cycle the following temperatures are recommended:
Aroclor 1242
70- 80C
Aroclor 1248/1254 90-100'C '
The lower impregnation temperatures are recommended for Aroclor
1242 since as this process is carried out under vacuum the losses will
be greater with a liquid which is more volatile!
.
After the impregnation cycle has been completed the vessel should be cooled to below 50'C before being opened and this is to avoid tho unpleasant fumes of Aroclor escaping into tho work-shop. The capacitors should then bo sealed as quickly as possible and degreased beforo final painting and testing.
Toxicity precautions and the handling of Aroclor is dealt with in a separate section but workors handling tho liquid, or capacitors coated with it, are advised to wear rubber gloves oil use barrier cream. '
TOWOLDMONOQ26286
PERFORMANCE OF AROCLOR CAPACITORS
A.C. capacitors at If a capacitor is continuously energised before and whilst subjected
low ambient temperatures to a low temperature environment it operates satisfactorily because
the heat produced in the dielectric balances the heat lost from the
case. A self-compensating process exists such that if the tempera
ture of the dielectric falls the losses increase, and more heat is
generated to establish a new equilibrium. Tests have shown that a
capacitor impregnated with Aroclor 1254 can operate continuously
energised in ambient temperatures down to -60C, and it was found
that such capacitors satisfactorily survived whilst installed out
doors during the winter 1962-3.
If, however, a capacitor is subjected to a low temperature environ
ment first and then energised it may be damaged by discharges
occurring in voids formed by the contraction of the dielectric before
it has time to heat up sufficiently. Cases when this might occur are
in street lighting capacitors during winter, or capacitors installed
in a plant that has been shut down during Winter holiday periods.
For this reason, the following minimum ambient temperatures are
suggested for the 3 grades:
Aroclor 1254 - 7C
'
. Aroclor 1248 -28'C
Aroclor 1312 -38'C
For operation at still lower temperatures a blend of Aroclor 1254
and trichlorobenzeno has been used.
:
D.C. capacitors Aroclor is also used in d.c. capacitors but it has been found that at the high stresses used tho service life of tho capacitor tends to bo reduced if tho working temperature is raised above 40 C. This can be
' ovorcomo by using stabilisers in tho Aroclor to overcomo the slight electrochemical degradation which tends to take place. Generally tho effect is proportional to tho quantity of stabiliser used and up to 1 per cont of anthrnquinono or 2-ethyl anthraquipono and 2 per cent of azobonzeno liavo boon used.
20 022T`>1,t'
TOWOLDMONOQ26287
. '' *
I
I
ii1
) '
M
i : \
5 ; i O
: i'
.1. >i
< -4
\; \
5u ii
T
TOXICITY AND HAHOUHG PRECAUTIONS Aroolor made by Monsanto has been used for over 30 years without causing any toxic effects, but it must be handled with care. These precautions should be observed: 1 Avoid shin contact. Protect the hands, preferably by oil-resistant gloves. 2 If skin contact should occur, wash off with soap and water. 3 If hot Aroclor must be handled in a closed or confined area provide exhaust ventilation or wear an approved respirator. 4 If Aroclor gets in the eyes, flush with large amounts of water. In the event that irritation persists refer the patient to a Physician. 6 Infrequent exposure to Aroclor vapour will not cause any ill effect, but prolonged exposure to a high vapour concentration should be avoided. If these precautions are neglected acne may develop and excessive exposure may cause liver damage.
0221647
TOWOLDMONOQ26288
LABORATORY MEASUREMENTS ON AROCLOR
ThoMonsanto There are many test cells available for measuring the electric dielectric test cell properties of liquid dielectrics, but since most of these were de
signed for use with mineral oil, Monsanto has designed a test cell especially for use with Aroclor. This design of cell is used in our laboratories and is available for sale to customers. It is essentially a three terminal cell with cylindrical stainless steel electrodes separated by a 1 mm gap. Figure 7 shows details of the construction of this cell.
The procedure for Great care must be taken to ensure careful cleaning for Aroclor cleaning and filling the cell measurements with this or any other cell. The Monsanto cell is
designed for easy cleaning and accurate assembly.
The Monsanto cell is first cleaned by a series of thorough washings
as follows:
' 1 A wash with benzene
2 A thorough washing with detergent and hot tap water
3 Repeated rinsing with hot tap water
4 6 rinses in distilled water
'
. 6 2 rinses in analytical grade acetone
During the wash with the powder detergent a soft hair brush is used and all parts of the electrodes are thoroughly brushed. The cell is then dried in an air oven at 130 0 for 30 minutes. Finally it is rinsed twice with the Aroclor to bo measured before filling a third time, when tho electrical measurements are taken.
Measurements The temperature at which the electrical properties are mado is measured by, a thermometer resting in the central well of tho coll. For routine tests a temperature of 100'C is used.
Permittivity and loss tangent are measured first with a transformer bridge at a stress of X V/gm and at mains frequency of 50 c 's. D.C. resistivity is then measured with an electronic megohmeter one minute after the application of a stress of 0-5 V/gm, If repeated readings of d.c. resistivity aro performed on tho samo quantity of Aroclor in tho coll, a gradual increaso is noted. It is therefore recommended that if a repeat measurement of resistivity is re : qulred, tho coll bo emptied, thoroughly cleaned, and then refilled.
22 0221648
Process control measurements For operating an Impregnation plant, it is convenient to be able to measure tho electrical properties of the Aroclor without the neceseity of taking samples, and a cell can be incorporated in the system
e.g. in a flow line. It should be arranged that there is a turbulent ' flow of Aroclor through the gap between the electrodes except when a measurement is being taken so that adequate cleaning of the electrode surfaces occurs. To obtain the Same value Of d.c. resis tivity with a plant cell and with a laboratory cell it is necessary for the Aroclor to be (1) stationary whilst the measurement is made, ^ (2) subjected to the electric field for one minute, and (3) at the same temperature.
COMPATIBILITY TESTING METHOD Procedure if the material is available in a laminar form or is a surface coating,
a piece 25 mm square is cut from a sheet. Other materials are selected so that the sample taken is present at the satne concentration as in . the finished article. .The sample is put into a glass jar that has previously been cleaned and dried in the foilowing sequence: 1 Wash in benzene 2 Wash with hot water and detergent 8 Six rinses with distilled water 4 Rinse twice with analytical grade acetone 6 Dry in an oven at 130"C for 1 hour To this jar, and to a similar one without a specimen within it, are added 50 ml of Aroclor. The Jars are then closed with ground glass lids and aged in an oven at 100'C for 7 days. After ageing, tlie Jars are removed from the oven and the Electrical properties of the Aroclor in both the specimen jar and tho control jar are measured at 100C according to the method described in Appendix A. Tlie specimens are examined for swelling or other signs of deterioration, and any colour change of the Aroclor is noted.
Results The Aroclor in which tho Bamplo has been immersed must not ex perience a decreaso in resistivity below 10 tcrohm cm. Information on materials which havo been tested is available on request.
TOWOLDMONOQ26290
Technical Service
Tho technical service staff of ^fonsanto is always ready to provide additional informa tion on the use of the materials indicated in this roport, and to assist manufacturers in the solution of particular problpms ensuing from their application.
0221650
Front cover illustration by courtesy of Industria Condensatori Applicazioni Elettroelettroniche Milano
Every effort has been made to ensure that the information in this publication is reliable, but as the conditions under which it may bo applied arc beyond our control.-wo cannot accept responsibility for any results of its use.
Form No. P.n,674-El-Cl> Published by Monsanto Chemicals Limited, Printed In England by Vaillkhnrd & Farnsworth Ltd. Nottingham
TOWOLDMONOQ26291