Document 9JKDkaQVeNgXgzkVDyJ5YyJ75
COMPANY CONFIDENTIAL RESEARCH AND DEVELOPMENT REPORT
ANNISTON PLANT
OTHER LOCATIONS
D. C. Armstrong - W.G.K. R. A. Munch - South Second C. R. Coleman - Ruabon A. F. Regan - Newport S. Setoh - Tokyo N. Arasaki - Tokyo M. E. Gibbs - South Second
> GENERA^. OFFICE
"*fl. S. Bergen D. B. Hosmer W. A/Kuhn P./G. Benignus ZA G. Bryant /C. M. Williams
( D. Danna H. 0. Hehner
rfeport No.
Job No.
Oat*
3
370-502 7-19-68
_____
ANNISTON PLANT
W. B. Papageorge J. C. Landwehr V. R. Haupt W. H. Howard W. B. Dunlap H.L. Williams R. A. Haydel S. 0. Kemp
Title:
1968 Quality Report on Bayer, Prodelec and JCanegafuchi Dielectric Fluids
Personnel: Problem:
7S. 0. Kemp - G. W. Mill *
Continue Surveillance on Dielectric Fluids in Competition with Monsanto Aroclor
Justification: Protection of Domestic and Foreign Sales
Summary:
At the Aroclor quality meeting in March 1967 it was proposed that a second marketing quality survey be made on materials competitive with Monsanto
Aroclor. The first survey made in 1966 indicated superior quality for
Bayer and Prodelec materials. This 1966 conclusion was not supported as expected by the second survey. It should be remembered that the 1966 test valves and those covered in this report are based on drum samples
of the material.
q Bayer Clophen A-30 resistivity tested only 800 x 10 ohm-cm as compared with 15,000 x 109 in 1966. Prodelec Pyralene 1499 which in 1966 tested
1200 remained low at 700 x 10 . Thermal Chemical Stabilities of the two products competitive with Aroclor 1242 remained low at 0.14 and 0.16 ppm Cl
respectively.
--^
The data collected on Kaneka Kanechlor 300 is included in the report; however the samples were not in the original manufacturer's containers and are not indicative of Kaneka quality.
Bayer Clophen A-50 and Prodelec Pyralene 1476, both competitive with . Aroclor 1254 show fair quality. The Bayer material showed the most signif icant electrical property change (1967 Resistivity 150,000 x 109 1968 Resistivity 6,500 x 109).
DSW 200611
/bs STLCOPCB4058675
Research and Development Report No. 3 Job No. 370-502
-2
Ba ckground
Beginning in 1966 a program designed to evaluate competitive electrical grade chlorinated biphenyl products was initiated. Since that time three reports have been issued on competitive quality. The first complete report on French, German and Japanese sources on the Aroclor 1242 and 1254 equivalents was issued in 1967. Based on that report and decisions made in the 1967 Aroclor meeting it was decided that more information was needed and consequently a second series of drum shipments were obtained. The second series of shipments were ordered in late 1967 and received at Anniston during mid 1968.
The drum quantities ordered were specified to be "standard manufacture's shipping containers". Unfortunately the Kanegafuchi material was not obtained as specified, but was drawn from a Kanegafuchi customer storage tank. Therefore, little credence should be placed on the Kanechlor results.
Discussion
Bayer
There is only one significant difference observed in competitive Aroclor quality comparing 1966 and 1968 results. The latest test results show that both Bayer Clophen A-30 and A-50 are marketed with electrical properties inferior to what the 1966 test results would indicate. This fact was originally quite disturbing and it was the author's opinion that the dielectric was contaminated during sampling of the drums for test purposes. The 800 x 10^ ohm-cm resistivity reported for Clophen A-30 was the highest resistivity result obtained from three separate sampling and testing operations. In two of the test series the test cell was precleansed and tested with Aroclor 1242 having a resistivity greater than 20,000 x 109 ohm-cm. The electrical quality of both Bayer Clophen A-30 and A-50 was definitely much lower than the first data (1966) indicated. It must be remembered however; that the data was gathered from two spot checks two years apart.
The stability test results for Bayer products remain low and are Indicative of good quality.
Prodelec and Kanegafuchi
Test results of Pyralene 1499 and 1476 agree quite well from both sets of data, 1966 and 1968. Pyralene stabilities are good and electrical properties are of average quality.
Kanechlor 300 test results, as pointed out previously, must be taken with certain reservations. The material was not received in the original manufacturer's containers, but was sampled from a Kaneka customer's storage tank. The test results do indicate good stability and fair electrical properties.
DSW 200612
STLCOPCB4058676
Research and Development Report No. 3 Job No. 370-502
-3-
Conclusions
The quality of competitive materials as deduced from the 1966 test results was somewhat misleading. Certainly Bayer and Frodelec have good quality dielectric on the market, as does Kanegafuchi, but It does not appear that any tremendous advantages or sales points are Inherent In either of their products compared with the comparable Aroclor.
Recommendations
Quality data accumulation on competitive dielectric liquids should be continued to avert situations where the quality supplied by competition is not known. It is recommended that at least every two years a survey of competitive quality be reported.
/bs
DSv\f 200613
STLCOPCB4058677
Research and Development Report No. 3 Job No. 370-502
-4-
Table 1
Comparison of Materials Competitive With Aroclor 1242 1968 Result/1966 Result
Property
Bayer Clophen A-30
Kaneka Kanechlor 300
Prodelec Pvralene 1499
Color, APHA
10 /<5
10/10
10 /<5
Acid No.
0.001/0.001
0.001/0.001
0.001/0.002
Ref. Ind. @ 25C
1.6240/1.6237
1.6251/1.6248
1.6246/1.6245
Sp. Gr. @ 25C
1.381/1.378 ~x
1.391/1.390
1.387/1.387
Moisture, ppm
62/63
94/24
51/35
Free Chlorides, ppm
0.009/0.009
0.018/0.009
0.018/0.009
HST, ppm Cl
0.07/0.11
0.11/0.11
0.11/0.16
Mon. Stab., ppm Cl
0.03/0.06
0.03/0.06
0.06/0.06
TC Stab., ppm Cl
0.14/0.07
0.16/0.08
0.16/0.12
Resist, x 10^
ohm-cm @ 100C Power Factor, %
1 KC 60 cycles
800/15,200
0.25/0.06 2.01/0.22
500/9,600
0.36/0.13 3.81/0.55
700/1200
0.26/0.33 2.40/4.60
Dielectric Constant @ 100C
4.81/4.90
4.88/4.82
4.89/4.87
Distillation, C by wt. 10% by wt. 90%
327/327 349/348
328/331 350/352
329/330 346/352
Type Drum
Galvanized
Galvanized
Steel-lined
DSW 200614
STLCOPCB4058678
i
Research and Development Report No. 3 Job No. 370-502
-5
Table II
Comparison of Materials Competitive With Aroclor 1254 1968 Result/1966 Result
Property
Bayer Clophen A-50
Prodelec Pvralene 1476
Color, APHA Acid No. Ref. Ind. @ 25C
15/7 0.001/0.001 1.6373/1.6365
30/10 0.002/0.002 1.6378/1.6380
Sp. Gr. @ 25C Moisture, ppm
1.496/1.490 30/30
1.499/1.503 47/30
Free Chlorides, ppm
0.009/0.009
0.009/0.018
HST, ppm Cl
0.11/0.07
0.07/0.14
Mon. Stab., ppm Cl
TC Stab., ppm Cl
Resist, x 10^ ohm-cm @ 100C
Power Factor, % 1 KC 60 cycles
0.06/0.10 0.39/0.28 6500/150,000
0.17/0.09 0.96/0.28
0.07/0.18 0.50/0.32 3200/3200
0.22/0.14 1.80/1.50
Dielectric Constant @ 100C
4.23/4.37
4.22/4.23
Distillation, C by wt. 10% by wt. 50% by wt. 90%
367/365 373/373 384/387
367/368 374/376 385/387
Type Druai
Galvanized
Steel-lined
SW 200615
STLCOPCB4058679