Document 99G0JdO36N47j4OBB0kYZDLXp

PLAINTIFF'S loomin' FD-256 b -I <T> t\ r? l tr. S BO C 0 0 0 BP ' PRODUCED BY FORn r \ c--. - N # V ".... LAND * SIA Am SPACE Society of Automotive Engineers, Inc. TWO PENNSYLVANIA PLAZA. NEW YORK. N. Y. 10001 --------------------------- (Stt) S91-S700 -- Cattl* Addraaa: SOCAUTOENO, N.Y. November 26, 1973 Mr. A.E. Anderson Scientific Res. Staff Ford Motor Co. P.0. BOX 2053 Dearborn, Michigan 48121 Dear Mr. Anderson: We are happy to inform you that your paper, "Asbestos Emissions frcrn Brake Dynamometer Tests" (730549) has been approved by the Engineering Activity Board for publication in the 1973 SAE Transactions. This selection has been made on the following criteria; 1. Long term reference value. 2. Technically new, innovative or constructive review. 3. Professional integrity. 4. Clear presentation. . Your work has been honored because it met high standards on these criteria. A copy of the paper is enclosed for your checking for any correc tions that should be made before publication. Please note any corrections in the margins and return the paper to me by December 10. We have received no written discussion of your paper. If you have received any, would you please send it and any closing remarks that you would like to make along with the corrected paper. The material will be printed in Transactions following the paper. Again, our congratulations. Sincerely, BG/di Enclosure _ t. . Brenda Goldberg, Editorial Associate Publications Division PRODUCED BY EORn TECHNICAL Sgg NEWS BRIEFS gggg m!teiMKSftBws>A B^Jni@t(tegjS3 H Vehicle Handling is Minor Factor in Accidents A rigorous analysis by Ford Motor Co. researchers postulates that the driver plays "by far" the most important role In vehicle handling. In fact some statistics have led to estimates that 90% of all traffic accidents are due to human errors. And, similar to the famous analysis that many World War n infantrymen failed to fire their rifles in combat, recent studies show that only a fraction of a percent of drivers produce lateral accelerations as high as 0. 35 g or longitudinal decelerations as high as 0.6 g in emergencies. Therefore, even in an extreme emergency, a ty pical driver may be using less than 50% of a vehicle's cornering ability. According to Ford, "The ease of vehicle control and not the level of vehicle performance constitutes the most important vehicle handling qual ity." Reportedly, it is now possible to realistically predict vehicle handl ing qualities by computer. Thus, hopefully, handling qualities may be in corporated in the vehicle while it is still being designed. The new ap proach should enhance handling qualities and ease vehicle control for the average driver. Asbestos Emissions from Brakes Are Not Significant The theory that vehicles are substantial emitters of asbestos seems to have been put to rest by researchers at Ford Motor Co. As noted in an earlier report in Automotive Engineering, EPA-sponsored work at Bendtx showed that most of the asbestos emitted from brakes and clutches is converted to other products with only 3.2% total asbestos emitted en tering the atmosphere. Now the Ford research shows that most brake lining asbestos is converted to a nonfibrous material by high flash tem peratures at the braking surfaces. According to a Ford report, "Less than 0.02% of lining wear was released as asbestos fibers. And the con centration of asbestos fibers in the urban atmosphere, due to brake us age, was conservatively estimated at less than 0.07 x 10"9 grams per cubic meter." Catalytic Converters Will Improve f/ileage, Oriveability Though seemingly paradoxical, the use of catalytic converters should im prove vehicle fuel economy, driv!-ability and starting. Reason, accord ing to GM is that since the converters do a large share of exhaust clean up, the other emission controls can be readjusted to improve engine per formance and efficiency. GM also stresses that using unleaded fuels will help reduce hydrocarbon and particulate emissions, lengthen spark plug life, and lower carburetor and ignition systems maintenance. Automotive Engineering, November 1973 PRODUCED BY Bonn V Scientific Research Staff Ford Motor Company 20000 Rotunda Drive Dearborn, Michigan 48121 Mailing Address: P.O.Box 2053 Dearborn, Michigan 48121 November 5, 1973 Mr. Leonard Brockman Senior Air Pollution Control Engineer Air Compliance Engineering Room 132 State Office Building Hartford, Connecticut 06115 Dear Mr. Brockman: Diane Uecker asked me to transmit our paper on "Asbestc* Emissions from Brake Dynamometer Tests". This is on S.A.E. paper (730549) given this year. I hope it will meet your needs. Yours very truly Enclosure cc v' R. I :r / David F. Moyer, Director Systems Research Laboratory > 80 0 0 006=? PRODUCED BY FORD r~. O H )\ E O CL UJ cr .REPORT No ASBESTOS EMISSIONS FROM BRAKE DYNAMOMETER TESTS by A. E. Anderson Mechanical Research Department and . R. L. Gealer Chemical Engineering Department and R. C. McCune and J. W. Sprys Technical Services & Administration .* V V : SCIENTIFIC ~ ~ STAFF V-. -*..., "TECHNICAL- REPORT` ( v,*. B000 &0&6 PRODUCED BY Bonn TECHNICAL REPORT No. SR 73-64 SCIENTIFIC RESEARCH STAFF FORD MOTOR COMPANY PROJECT NO, June 4, 1973 DATE ASBESTOS EMISSIONS FROM BRAKE DYNAMOMETER TESTS by A. E. Anderson, R. L. Gealer, R. C. McCune, J. W. Sprys SUMMARY dynamometer tests of a production disc brake provided new information on asbestos fiber emissions during breakin, normal use, ana high temperature use conditions. Both ambient air and brake cooling were sampled isokinetically, using 0.I1*5 um filters. Examination of test and background filters required a clarification process to maximize fiber detectability, the use of transmission electron microscopy (at 1*0,000 X) for detection, and electron diffraction for positive identification of asbestos fibers. Most of the lining asbestos was found to be converted to a non-fibrous material by the high flash temperatures of the braking surface. Less than 0.02% of the lining wear was released as asbestos fibers. The concentration of asbestos fibers in the urban atmosphere, due to brake usage, was conservatively estimated at less than 0.07 x 10`9 grams per cubic meter. Based on this upper bound, the use of brakes was Judged to be not significant as a source of atmospheric asbestos. APPROVED: Mechanical Research Department T. P. Hopkins, Manager Technical Services & Administration J. V. fGU'VWU-A, ricuici(^i Chemical Engineering Department 8000 0087 ' PRODUCED BY PORT) INTRODUCTION Asbestos has been a major constituent of automotive friction materials for more than 50 years. It is used to impart strength, flexibility, and heat resistance to a brake lining and to enhance friction and wear properties. Most present brake linings use resin or rubber binders and chrysotile asbestos, together with organic and inorganic friction modifiers and fillers. The asbestos content varies with formulation, from a low of to about 65$ by weight. Minimum asbestos levels are found in some higji performance European disc brake linings which are highly filled with metals and inorganic constituents. Brake linings in the U. S. average about 50# asbestos content.. Of a total U. S. annual asbestos consumption of 800,000 tons (730 Mkg), about 28,000 tons (25 Mkg) of chrysotile asbestos are purchased annually for friction materials of all types (1).* Of this, it has been calculated that brake lining wear consumes about 12,000 tons (11 Mkg) of asbestos per year. Roughly an equal amount remains on brake shoes at the time of replacement or is manu-. facturing wastage. Recent tests have shown that densely populated urban atmospheres often contain significantly higher asbestos concentrations than stirrounding areas (2). Background asbestos levels in the atmosphere result from the natural weathering of asbestos-bearing rock and soil, as well as from mining, farming, and excavating. The generally higher urban concentrations suggest commercial and industrial sources. Brake lining and clutch facing wear was suggested by Thomson (3) as a possible source for higher asbestos levels in the urban atmosphere. Lynch (k), in a study undert t. by the Public Health Service, reported the findings of several brake dynamometer and friction machine tests in which wear debris was trapped on a filter and subsequently examined by means of a transmission electron microscope (TE>i). He concluded "Reference (10) suggests 59,000 tons (53 Mkg) is more correct. BO00 00B8 PRODUCED BY FORD 2- that "free fibers from brake lining wear seem to be an inconsequential health factor in urban air pollution." lynch detected no free fiber from an automobile clutch and a bus drum brake, but some free fibers were found in one test of an experimental disc brake. With mounting concern over air quality in general, and asbestos pollution in particular, this study was initiated in 1970 to provide additional data on the asbestos emissions from disc brakes. OBSERVATIONS OF LINING WEAR Ihe near absence of free asbestos fiber from lining wear has been reported by Luxon (5) using X-ray diffraction and by Lynch (U) using the TEM (transmission electron microscope). Several authors have suggested that interfacial temperatures during braking could be high enough to decompose the chrysotile asbestos into non-fibrous thermal degradation products. Ana lytical- relationships exist which permit calculation of interfacial tempera tures (6). However, several of the significant parameters are difficult to determine accurately for heterogeneous materials such as brake linings. The asbestos crudes (larger fiber bundles) were calculated to reach their rapid decomposition temperature during normal braking at speeds above 56 MPH (25 m/s) as an upper bound value and above 18 MPH (8 m/s J as a lower bound value. An experimental approach was undertaken to provide closer bounds. Added insight into the thermal decomposition of asbestos fibers in brake lining wear was attempted by direct visualization of the frictional process. A small laboratory friction test machine was constructed using a thermal shock res: start (Tyoor) glass rubbing surface (replecinr the conventional cert iron) in which the friction interface was directly viewed with a low power (7-50X) binocular microscope (7). Scaled rubbing velocities were used to compensate for the thermophysical property differences between the glass and cast iron. 8000 0089 PRODUCED RV FORn -3- Moderate scaled velocities, roughly equivalent to 12 MFH (5 m/s ), provided a view of intermittently incandescent asbestos crudes. During the initial burnishing operation resinous material surrounding these asbestos crudes was observed to pyrolize, producing microbeads of condensation products around the crude. Ihese organic products of resin degradation and the apparently powdered asbestos decomposition products were seen to smear into platelets, often of such size as to be discernible to the unaided eye. At higher rubbing velocities (over 30 MPH, or 13 m/s ) the platelets formed a surface char layer tinder the action of more severe thermal and mechanical action. The larger asbestos crudes then could be seen to glow with apparent depth and for greater time durations, often several seconds. The actual brake lining contact area was only a few percent of the total available surface, with contact spots moving in a random manner with tine. From these friction visualization studies it appeared that local flash temperatures and severe mecl^nieal action could be major factors in the breakdown of asbestos fibers for most brake usage. Examination of the lining surfaces revealed the presence of non-fibrous magnesium silicate in both crystalline (Forsterite) and amorphous phases. Magnesium silicate is a thermal degradation product of cbrysotile asbestos. Forsterite transformations have been reported to occur at 6006C over a period of hours. Differential thermal analysis (DTA) studies in our laboratory indicated this transformation occurs within seconds at 820C. Special brake lining formulations were then prepared and tested on the glass visualization apparatus and a Friction Assessment and Screening Test (FAST) machine; (8). Chemical reactions were found to take place at the fricvlc:. i:.'.-; face which would rerrire a flash tercperrrure rise of "UCC to initiate when an equivalent of 35 MPH (16 m/s) rubbing speed was used on the FAST machine. At this same speed melting of inorganic lining additives and metal particles confirmed brake flash temperatures up to 980*C. ' fioao 0090 PRODUCED BY FORD -4- Based on these findings, it would not appear surprising for few asbestos fibers to be emitted from brakes in normal usage. However some mechanical removal of fiber appeared possible during the first several brake applications with new linings. Also, high brake temperatures possibly could weaken the organic binders and cause increased fiber emissions. TEST PROCEDURES Complete sample collection and examination procedures, along with sample data calculations are included as Appendixes I, II, and III. Briefly, the tests were performed as follows: a new Pinto disc brake assembly was installed on J single station brake dynamometer in a room which was cleaned of extraneous asbestos sources.- Air from within the room was blown through a diffuser screen to provide a velocity distribution over the brake which approximated that of vehicle usage. The air stream in front of and behind the brake was sampled isokinetically, using matched 0.45 Um filters, holders, and air pumps. /Note the system schematic in Figure 1 and the actual test setup in Figure 2. The brake exhaust air was discharged out of the building. i ) . The first pair of filters were used during the first 82 burnish stops, to represent "breakin" conditions. After further burnishing, a second pair of filters collected samples during 560 "normal use" brake applications. A third set of filters then were utilized in a "high temperature use" test of 4l brake stops. .............. All brake applications were made from a 40 MPH (l8 m/s) equivalent speed. ireakin and normal use tesus employed brake torques corresponding to one-quarter "g"(2.45 m/s2) deceleration. This torque level was doubled for the high terperaiure tests. During the normal use procedure, the test filter was located for 20 brake applications at each of 28 grid locations in the exhaust duct throat, to insure a representative sampling of the air flow over the brake. This test grid ' R000 009] PRODIJCFD RV cnur, and filter may be seen in Figure J. A central collection site in the test grid vas used for the "breakin test" and the final "high temperature" test. ( Samples of the three pairs of filters (breakin, normal use, and high temperature use) were subjected to a clarification process involving low temperature ashing to oxidize all organic material and mechanical action to separate the particles. This assures maximum detectability of asbestos fiber (2). RESULTS AND DISCUSSION Transmission electron microscopy at 40,000 magnification was used in the search for fibers. At this magnification the ultimate fibrils anpear to be .I * above one millimeter (0.040 inch) in diameter. Quantity, length, and apparent diameter measurements provided data for calculation of asbestos fiber mass per ur.it of filter area. Coupled with dimension, mass, and flow determinations from the dynamometer tests, this data was used to calculate the emitted asbestos fiber concentration in the collected wear dust, in the cooling air stream, and from the brake lining worn. The size distribution of collected fibers was not determined by this method, since the clarification process involved sufficient i mechanical action to reduce most fiber bundles to the ultimate fibril size. Additional samples of the "normal use" test filters were examined on the TEM without recourse to the clarification process, in an effort to determine the asbestos fiber size distribution. Roughly 10$ of the asbestos fiber was visible on the background sample, based on the results from corres ponding samples after clarification. The largest observed fiber bundle was C.cC i-n in diareaer and over 1.1 urn long. A similar direct TEM search of the "normal use" test filter revealed about 2$ of the asbestos fibers observed after -as attributed to the greater concentration of obscuring matter in the test filter. However, the largest observed asbestos fiber in the test filter (0.1J pm in diameter and over 1.2 pm long) was about the same size as was found on the background sample. 6000 0092 PRODUCED BY FORD -6- The similar, low fiber content of both background and test filters precluded a fiber size distribution estimate. However, it appeared that the quantity of the larger asbestos fibers on the test filter was no greater than that' of the background filter. This supports the observation from the lining wear visualization tests that normal brake wear degrades most of the asbestos fibers. A brake lining grade of asbestos appears on the TEM as in Figure 4. The fiber bundles are composed of strong, but weakly adhering fibrils of about 0.0J pm (roughly 1 microinch) diameter. Mechanical action causes the larger fibers to "open" into smaller fibers or even fibrils, as illustrated in Figure 5 Contrast these "raw material" fibers with one of the larger fibers (Figure 6) and one of the more typical fibrils (Figure 7) from the "normal use" test filter. . The similar, low fiber content of both background and test filters required clarification to permit an asbestos fiber count, thus providing more accurate fiber mass determination, but obscuring the actual fiber size distribu tion. Therefor^, the calculations of fiber concentration (Table 1) were expressed as asbestos mass per unit mass of lining wear dust and asbestos mass per unit 'l mass of lining worn. Asbestos fiber concentration in the ambient air (background) and in the brake exhaust air (test) was calculated in units of nanograms (10~9 grams) per cubic meter of air. However, the actual asbestos emissions from brake usage would be diluted substantially through mixing. The asbestos concentration in urban air due to brake usage was estimated, based upon existing automotive exhaust lead dilution data. These calculations appear in Appendix III. All the test results in Table 1 have been reported as ten times the calculated test values, to allow for possible losses in collection, processing, err counting. These values, therefore, should provide upper tour is for asbestos emissions from brake usage. For example, the local (Detroit, Michigan) atmospheric asbestos concentration ranges from 0.5 to 13.4 nanograms per cubic meter. The POCO 0C93 PRODUCED BY FORD -7- observed background asbestos value was 1.9 ng/m3, for the normal use test, but is reported in Table 1 as 19 ng/m3. The low asbestos emissions from t* the test disc brake under "normal use" conditions is underscored by the addition of but 13 ng/m3 (1.3 ng/m3 observed) in the undiluted exhaust air stream. TABLE 1 ASBESTOS EMISSIONS FROM "NORMAL USE" BRAKING Dynamometer Data for a Production Disc Brake* . Background Asbestos in Ambient Air <19 x 10"9 g/m3 . ' Asbestos Fiber from Brake in Exhaust Air <13 x 10"9 g/m3 . Total Asbestos Fiber in Exhaust Air <32 x 10"9 g/m3 . Estimated Brake Asbestos Fiber in Urban Air <0.07 x 10`9 g/m3 . Asbestos Fiber fran Brake in Airborn Wear Dust . Asbestos Fiber Released from Lining Wear <0.05# <0.02$ * Reported values are 10 times the observed test values to provide upper bounds The lining wear rate during the first 82 breakin stops was found to be about five times above the "normal use" rate. Asbestos fiber release during breakin was also higher, an average sevenfold increase. However, since the breekin veer is less than 1^ of the tr.tal hir ing wear, the increase of emitted asbestos fiber resulting from this temporary sevenfold increase would be about 3$, when averaged over the life of the linings. high its:, erasure bra^e v.age also increased lining wear rates, in this case by a factor of eleven. Asbestos fiber emissions increased by less than a factor of three. Frequent vehicle operation under such high temperature . 9000 009a PRODUCED BY FORD -8- conditions would lower lining life to levels far below present averages. However, even if all brake wear provided the same fiber emission rate as found in the high temperature use test, the percentage fiber release to the atmosphere would still be under 0.06$ of the lining wear. Bie remaining brake wear was a mixture of non-fibrous organic and inorganic matter. Forty-seven percent of the estimated 62 to 77$ collectable wear debris were accounted for by the test filter on the normal use test. The remaining 15 to 50$ presumably were retained on the lining edges, the caliper, spindle, rotor, wheel, and tire. Accurate measurement of this material was not possible, due io the added retention of dust from the ambient air. More precise values of brake lining asbestos emissions or the determination of their particle size distributions appear possible, for these low fiber concentrations, only by testing brakes in an asbestos free atmosphere. This approach was used in an EPA sponsored study (9), where pre-filtered air was flowed through sealed brakes at a flow rate greatly reduced from normal. CONCLUSIONS A'l . 1. Automotive brake usage provides a very small emission of asbestos fiber i (less than 0.02$ of the lining worn). 2. Automotive brake usage provides a very small asbestos fiber input to urban atmospheres (estimated to be below 0.07 ng/m3). 5. Intense local heating and severe local mechanical action causes the decom position of most asbestos fiber in brake linings during typical usage. 8t>00 6095 ' PRODUCED RY poon -9 - APPENDIX I SAMPLE COLLECTION DYNAMOMETER ROOM PREPARATION The normal brake cooling air was found to be more variant and higher in dust concentration than was the room air. Consequently, the supply air duct was removed and sealed. To reduce the background asbestos level to a minimum, the dynamometer room was thoroughly cleaned and vacuumed while maximum exhaust air flow was maintained. All potential sources of fiber emissions were removed from the room and asbestos handling was curtailed in adjacent rooms. A production Pinto disc brake assembly was installed on the single station brake dynamometer, as shown on the schematic of Figure 1. The major elements of the test setup may be seen in the photograph of Figure 2. Cooling air was supplied from the room by means of a fan and diffuser screen. Contain ment of all possible airborn wear dust was assured by fitting a rectangular collector nozzle to the exhaust air duct, about two feet downstream of the brake. Metal panels were installed below and beside the brake to further contain the cooling air flow and to help provide a representative air flow over the brake, compared with vehicle service. System parameters were adjusted until the air velocity distribution matched closely with actual usage and the air flowing over the brake assembly was fully captured by the exhaust duct. This was confirmed using a smoke generator. The erhaust d-ct throat was parti' ioned ir.to a 4 by 7 array cf roughly three inch square grids (Figure 3)* The velocity profile within this grid war re-.rurai tc provide rear, values for each R000 0096 ' PRODUCED ry mn -10- SAMPLE FILTER PREPARATION Microporous membrane filters vitb 0.^5 urn pores vere selected to assure higi retention of asbestos fibrils and most of the wear dust powders. A matched pair of Gelman sampling pumps and 55 mm diameter holders were used. Hiin metal cones of 12 included angle were fabricated and sealed to the filter entrance. Uiese cones increased the tip entrance velocity to that of the exhaust air duct so isokinetic sampling could be achieved. The cone tips were carefully matched in size. Flowmeters and differential pressure indicators were installed in the system to monitor the filter airflow during each test and to set the tip entrance velocity before each test. Tests were performed on the unused filters to determine their weight change with variation of humidity. Filter weights were measured on a microbalance to the nearest 10 micrograms. Filters were placed in the center of the designated exhaust duct grid and at a fixed position upstream of the brake, but below the diffuser screen. This latter (background) filter was located where the upstream air velocity equalled the average over the test grid. In this way the sampling was isokinetic with essentially equal volume flows through both filters. TEST PROCEDURE . All brake stops were conducted from the same speed equivalent (U0 MPH, or 18 m/s) to maintain fixed air flow conditions. Burnish and "normal, use" brake applications were at 0.25 "s" (2.^5 m/s&) deceleration and with a two minute time interval, 'inis provided a peak rotor temperature of l80C (550F). Ibe number of brake applications were selected to provide about cr.e gran ;f lir.ir.r wear per test. Breakin wear was monitored for the first 82 stops. No sampling was performed for about 200 more brake applications, while the linings and rotor developed essentially steady-state conditions 8000 0097 PROD! rrpn Pv Prp T', The "normal use" test was then performed on this burnished brake assembly. Twenty brake applications were made under the same conditions, with the test filter located sequentially at each of the twenty-eight grid locations. The filter cone entrance velocity was adjusted to match the grid velocity at each relocation. Four grids were used to monitor exhaust velocity. Slight adjustments were sometimes required to compensate for drift which appeared to be external wind initiated. A third test was performed to provide an estimate of the fiber emissions fronp a hot brake assembly. As in the breakin test, the test filter -I was positioned in a central location for this procedure. Thirty-one stops were made at 0.5 "g" (h.p m/s2)' and minimal time interval until the rotor attained 1*10#C (770F). This temperature was then maintained by adjusting the application time interval. Ten additional stops were made as the brake was allowed to cool. All filter weight determinations were performed at equilibrium conditions and .then corrected for humidity. After use, the filters were i individually stored in covered glass containers. Lining weights were taken after removal of wear debris but before they had cooled completely, to minimize weight changes from water absorption. Between tests the linings were stored in a dry Jar. The relevant test data are included in the following table. A slight pad drag caused the outboard lirirg to wear above expectations on the "normal use" test. Since this added work was not included in the lining wear rate calculations, the specific wear is above the usual range for this lining. T5o adverse effect on the test results would be expected to have resulted iron this drag. Similar pad drag effects may occur on cars, when smooth road conditions prevent "pad knockback." 8000 0098 ' PRODUCED BY FORD Test Brake Speed, RPM Brake Lecel, "g" Wheel Load, kg Brake Applications Total Energy, kW-h Max. Apply Temp, C Total Lining Wear, g i Lining Wear Rate, g/kW-h Breakin 535 0*0 MPH) 0.25 (2.1*5 m/s2) 257 (567 lb) 82 0.938 (1.25 hp-hr) 115 (2l*0F) 1.10 1.17 (0.051 ijto) Normal Use Hi Temperature Use 535 0*0 MPH) 535 (1*0 MPH) 0.25 (2.1*5 m/s2) 0.50 (i*.9 m/s2) 257 (567 lb) 560 257 (567 lb) 1*1 6.1*05 (8.51* hp-hr) 0.1*69 (0.625 hp-hr) 115 (2l*0F) 1*10 (770F) 1.60 In3 o.25 (o.on 1.07 2.26 (0.100 ghr) I AftoO 0099 ' PRODUCED BY FORD -13- SAMPLE EXAMINATION APPENDIX II PREPARATION AND EXAMINATION OF ASBESTOS CARRYING SAMPLES FROM TEST FILTERS* 1. All slides, dishes, scalpels, and other utensils used in the following preparations were cleaned in acetone, followed by rinse in 200 proof ethanol. 2. An area of measured dimension was selected at random from the test filter, cut and placed particle side down on a clean glass slide. i I 3. Several dtfops of acetone were placed on the filter segment to partially II dissolve and secure it to the plate. 4. Die samples were ashed for a period of two hours by using a low temperature asher at a chamber pressure of 0.5 torr (70 Pa) oxygen and power of ( 200 watts. 5. Several dro^s of a 1^ solution of nitro-cellulose in amyl acetate were placed on the residue, and a clean watch glass was used to grind the mixture i for a period of five minutes. 6. A second clean glass slide was then placed over the mixture of nitro-cellulose and residue, and a "smear" obtained by pressing the two slides together and then sliding them apart. . 7. Die films thus formed were permitted to dry and then removed by scoring the edge cf the slide with e scalpel and "floating" the film free from the slide in a distilled water bath. It was found that the film was most easily removed from the slide introduced in Step 6. *Sample preparation'techniques outlined below are similar to those reported by Selikoff, et el. in Reference 2. 8000 0100 PRODUCED BY FORD 8. Appro::irEtely if elec+rr- microscope rrids (; mm. firmer grids) were placed at random on the floating film, anci the film vas rafted by ! putting a clean slide on top of the film and drawing the slide down, through the water so as to trap the grids between the slide and the film (which should now cling to the slide). 9. A carbon layer of approximately 0.06 um was deposited on the film to prevent charging during examination in the transmission electron microscope (TEM). Direct examination specimens were prepared by depositing a carbon layer on the dust side of the test filter and dissolving the filter in acetone. I Electron microscope grids were used, both to support the sample end to provide II grid location reference marks. TEM EXAMINATION AND COUNTING PROCEDURES Approximately ten electron microscope grids were prepared for each of the five filter samples analyzed. Four grids were arbitrarily selected from each sample and two grid squares on each grid were scanned for asbestos. The individual grid squares are approximately 90 pm on each side and were examined at a T&M magnification of about 40,000. For each grid area scanned, photographs were taken where possible of the first, last, end one randomly chosen fibril for the purpose of determining an average fibril diameter accurately. Measurements were then made visually; tnat is each fibril, fiber, or asbestos bundle was compared to known calibration marks on the electron microscope screen to estimate the lengths. 3he length could be estimated to within 2056, as determined by the photographic measurements. The marks on the screen ere 0.5 om apart corresponding to 0.125 hm when a magnification of 40,000 is used. Ibis approach was taken because it was impractical to photograph all the fibrils and, furthermore, length neusurenents were not as critical as diameter measure ments in determining fiber volume. Where both measurement methods were used, the values provii_r.r the greatest indicated brake asbestos levels were chosen. 5be results are shown in the following table: 8000 0161 . ' PRODUCED BY FOR r> -15- Sample A B C I) E F "1 , ASBESTOS CONCENTRATION ON FILTERS Sample Identification Concentration (ng/cm2 of filter) Test-normal stop-new brakes 15.52 Background for A 1.06 Test-normal stop-burnished brakes T.98 Background for C 4.64 Test-high temperature stop-burnished brakes 5.57 Background for E - not used, insufficient sample > Blank - unused filter 0.55 Frosn photographic measurements of 120 chrysotile fibrils, the asbestos fibril average diameter was determined to be 0.0337 with distributions similar to that observed by other workers (10). From 45 fibrils of triple jet- milled chrysotile the average diameter was determined to be 0.0316 Mm with a standard deviation of O.OO63 Mm. ASBESTOS IDENTIFICATION Asbestos can be identified in the transmission electron microscope in one of two ways. The first and absolute method is by electron diffraction. Such a diffraction pattern is presented as Figure 8. Measurement of diameters and correlation of these measurements with a known standard gives the interplanar spacings of the material. Comparison of these spacings with the ASIM file identifies the material as clino-chrysotile (asbestos). The second method of identification is by appearance. Figure 9a represents er image of asbestos obtained in the TEM. Fine lameilae ere observed within the fibril which are parallel to the long axis. This appearance is characteristic of chrysotile asbestos fibrils. Because of the nature of the electron beam, radiation and heat damage can occur in the material markedly . 0066 0102 PRODUCED BY FORD altering the appearance. Such changes in asbestos are represented in Figure 9b. The fine linear appearance of the fibril of Figure 9a has been changed to a mottled structure. ' l ( I ( V;.- BOOO 01C 3 ' PRODUCED RY Rfum ( 8000 01t>4 -17- APPENDIX III DATA REDUCTION ' 3be following table contains the pertinent test data and calculated results from the brake dynamometer tests: Test Sample Breakin Normal Use Hi Temp Use Calculation Units Test Bkgrd Test Bkgrd Test Bkgrd Basis______ 1. Filter Air Flow m3 2.22 2.22 23.00 21.80 0.564 0.564 Measured 2. Filter pickup mg 0.56 0.10 1.56 0.90 0.27 0.00 Measured 3. Filter Asb. Conc.ng/cm2 15.32 1.06 7.98 4.64 5.37 0.12* Measured 4. "Blank" Asb.Cone.ng/cm 0.33 0.33 0.33 0.33 0.33 0.33 Measured 5. Filter Area cm 9.62 9.62 9.62 9.62 9.62 9.62 Measured 6. Filter Asbestos ng 144.2 7.02 73.59 41.46 48.48' 1.07* C(3)-(4)] x (5! 7. Asb.Cone, in Air ng/m* 64.95 3.16 3.19 I.90 85.96 1.90* (6) f (1) 8. Lining Asb. in Bxh. Air ng/m 61.8 1.29 84.1 A(7) 9- Lining Asb. on Filter ng . 137.2 29.7 47.4 (8) X (1) 10. Duct flow/filter flow 11. Lining Asb. released 108 12. Lining worn mg 1235 O.I69 1100 1235 O.0367 1600 1235 0.0586 1070 From Meas. (9) x (10) Measured 13. Asb. released as % of wear 0.015 0.002356 0.005556 (11) v (12) x 3 14. Lining dust on filter ^ 0.26*** 0.61** C.27*** A(2) 15. Lining dust in air mg 16. y, Asb. in wear dust 17. Lining dust as % of wear 321 -J. r*\sO~ s?i^o 2956*** 754 0.0049)6 4756 333 C. 016/c 3156*** (10) x (14) (11) * (1?) x : (15) 4- (12) x 3 * Value calculated based o: ''normal use" background, due to insufficient sample ** Corrected fcr f; ~ ' difference throu.c: cert and backrrcur.d filters *** Filter in one (central; location, and thus possibly non-representative PRODUCED BY FORD -16- ESTIMATION OF BRAKE LINING ASBESTOS DILUTION IN URBAN ATMOSPHERE The concentration of asbestos fiber from the brake lining vear debris is assumed to be the same as was found in the "normal usage" dynamometer test and to be dispersed and have the same residence times as the lead emitted from the engine. Assume an average mileage of 15 MPG from cars which emit 75% of the lead to the atmosphere. When gasoline averaged 2.52 grams of lead per gallon, the typical lead concentrations in urban atmospheres were about 2jHg/m3 (JAPCA, Sep. 1969, 19, p. 684). . Typical U. S. cars wear 202 grams of lining per year and drive 10,000 miles per year. The "normal use" dynamometer tests provided asbestos fiber amounting to 0.002J% (2.5 x 10~5) of the brake lining worn. Allowing a factor of ten to provide an upper bound in this determina tion, the asbestos concentration in urban atmospheres from brake wear should be less than 10 ^2.5 MU, OOO gal Urban atmospheres vary in asbestos fiber concentration from city to city, within a city, and from one tine to another. This variation does not correlate with expected automobile brake usage. The concentration has been reported to reach 100 (2). Thus it appears that the wear of brake lining produces, at most, a small fraction of the asbestos fiber in urban air. This is not surprising when one considers that brake lining vear involves only 1.5' of U. S. asbestos usage and that brake visage converts over 99*95/6 of this to non-fibrous dust. <*000 0105 PRODITCHD RV Prion -19- CAi.rui^7roKS of coliectic:: efficiency LINING COMPOSITION ESTIMATE FROM LABORATORY ANALYSIS SiOj> 16.3$^ MgO 17.8 Fe203 AI3O3 2.5 0.3 h20 5.5 CaC03 15.4 Zn 3.9 Organic Total 38.3 100.0$ Chrysotile Asbestos 42.1*$ WEAR DEBRIS ESTIMATE \ Decomposed Asbestos 36.9$ Decomposed Limestone 8.6$ Zinc Metal Inorganic 3.91 49.4$ ORGANIC Volatile 10.5* . Uncertain Low Volatility 15.7* 12.1$ Organic Collectable 12.1$ to 27.3$ Total Collectable 61.5$ to 77.2$ Collected on Filter 47$ Collectt:li Materiel not trapped by filter 14.5$ to 3^.2$* ( * This material presumably on shoe edges, caliper, rotor, wheel, and tire. ft 0 0 0 0 J 0 ft PRODUCED BY FORD REFERENCES 1. Sullivan, R. J. et al., "Preliminary Air Pollution Survey of Asbestos," N.A.P.C.A. Publication APTD 69-27, (1969). 2. Selikoff, E. J., et al., "Asbestos Air Pollution," Arch. Environ. Health, Vol. 25, (July 1972). 'J. Thomson, J. G., "Asbestos and the Urban Dweller," Ann. N. Y. Acad. Sci., 152:196 (1965). lynch, J. R., "Brake Lining Decomposition Products," J. Air Pollution Control Assoc. 18:12 (1968). 5. Jiuxon, S., "Technical Implementation of the New Asbestos Regulations," Ann. Occup. Hyg. (Brit.) Vol. 1J (1970). 6. Rabinowicz, E., "Friction and Wear of Materials," John Wiley, (1965). 7. Anderson, A. E., "Wear in Brake Materials," ASMS Wear Conf., (I969). 8. Anderson, A. E., et al., "A New Laboratory Friction and Wear Test for the Characterization of Brake Linings," SAE Trans., pp. 561-9, (1968). 9. Jacko, K. G., et al., "Brake and Clutch Emissions Generated During Vehicle Operation," SAE Preprint 7505^8, (1975)* 10. Yada, K., "Study of the Microstructure of Chrysotile Asbestos by High Resolution Electron Microscopy," Acta Crystal, Vol. A, 27, (1971). 8000 0107 PRODUCED BY FOPn m m ( 090 010b PRODUCED BY FORD F ig u re 1 Dvnano^r.eter te s t schem atic Test Grid Test Broke cE a-> A) <c e soon 0J09 PRODUCED RY FORn F ig u re 2 dynamometer te s t se tu p . Figure 3 View of brake assembly and test grid. PRODUCED BY FORn COOO 0111 ' PRODUCED BY FORD F ig u re k TEM image o f c h r y s o t ile a sb e sto s f ib e r s . 9000 Oil? PRODUCED BY FORD F ig u re 5 TEM im age o f p a r t i a l l y opened f i b e r b u n d le s . PRODUCED BY FORD F ig u re 6 TEM image o f f ib e r b u n d le on "n o rm a l u s e " f i l t e r . BOOO 0114 PRODUCED RV Poor. F ig u re J TEM image o f f i b r i l on "n o rm a l u s e " f i l t e r . PRODUCED RY POPn F ig u re 8 TEM e le c tro n d if f r a t io n p a tte rn o f c h r y s o tile f i b r i l . 9 1 1 Q OOQti figure 9a,b TEM iBage of fibril before () and after 0>) electron tea. age ' PRODUCED BY FORD distribution list G. R. Beardsley R. M. Campau T. Cole V. D. Compton W. R. Dance D. F. Pi sous W. J. Foxwell R. W. Gaines R. L. Gealer 8. Gratch E. E. Hagenlocker T. P.Hopkins M. Humenik, Jr. J. T. Huston D. A. Jensen K. L. Johnson D. J. Karalash J. A. Kirschke J. E. Mayer, Jr. R. C. McCune C. D. Melvin J. S. Ninomiya D. W. Paul L. R. Petersen J. V. Petrocelli W. R. Pierson R. C. Ronzi C. E. Scheffler J. W. Sprys B. Weinstock M. H. Weintraub J. H. Zich Records Retention (2) Staff Services (2) Technical Information (2) ROOD 0117 ' PRODUCED BY FORD Inter OfAc* TOs R. 1. Gealer T Sctentlfic Reaaarch Staff June 22, 1973 v. ;y Subject: Report SR 73-64 I think a copy should be sent also to Dr. V. Sussman Serge Gratch ed eooe oii^ Bf- 3$ PRODUCED BY FORD